Anti-frosting low-temperature TGIC (triglycidyl isocyanurate) curing weather-resistant polyester resin as well as preparation method and application thereof
By optimizing the raw material composition and preparation method, the storage stability and frost resistance of low-temperature TGIC cured polyester resin in practical applications are solved, and efficient curing and good performance under low-temperature conditions are achieved.
Patent Information
- Application Number
- CN202411009537.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-19
AI Technical Summary
At this stage, low-temperature TGIC cured polyester resin is difficult to effectively control the low-temperature curing rate, resulting in poor storage stability and frost resistance, which cannot meet the actual application needs.
Using optimized raw material composition structure and preparation method, including the combination of polyols, polyacids, acidification blocking agents, organotin catalysts, antioxidants and curing accelerators, prepared by steps such as esterification reaction, vacuum polycondensation and blocking reaction. Anti-frost low temperature TGIC curing weather-resistant polyester resin, controlling curing rate and improving mechanical properties and durability.
Effectively improves the anti-frost performance, avoids the "white frost" phenomenon, improves storage stability and mechanical properties, reduces energy consumption, meets practical application needs, and maintains good coating performance and appearance quality under low temperature conditions. .
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder coatings, and in particular relates to a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin and a preparation method and application thereof. Background Art
[0002] Powder coating is a solid powdered synthetic resin coating composed of solid resin, pigment, filler and additives. It has the advantages of no pollution and low energy consumption, and is widely used in the fields of automobile decoration, shipbuilding industry, etc. Among them, most solid resins are polyester resins, which are unsaturated thermosetting resins generated by the reaction of several organic acids and polyols. Traditional polyester resins need to be cured at high temperatures, and high-temperature curing requires a lot of energy, has high requirements for equipment and operating environment, and has high production costs. In addition, high-temperature curing may also cause degradation or deformation of heat-sensitive materials, limiting the application range of polyester resins. In order to overcome the problems of high-temperature curing, low-temperature curing polyester resins have been used. Although it can improve the problems caused by high-temperature curing, low-temperature curing is very likely to affect the mechanical properties and durability of polyester resins due to incomplete or uneven curing, showing lower hardness, wear resistance and chemical stability. What is more serious is that the leveling performance of the powder coating produced will decrease, and it is very easy to produce a "white frost" phenomenon, which not only affects the appearance quality of the product, but also causes the adhesion of the surface coating to decrease, thereby affecting the overall performance of the product.
[0003] There are studies in the prior art on the problems of decreased leveling and "white frost" caused by low-temperature curing, such as patent application CN116041676A-A polyester resin for low-temperature TGIC curing powder coating and preparation method thereof, CN111533892A-A polyester resin for high weather resistance low-temperature TGIC curing powder coating and preparation method thereof, which improve the mechanical properties and durability of polyester resin by adjusting the chemical composition or curing temperature, and solve the problems of decreased leveling and "white frost" phenomenon in the current low-temperature curing polyester resin. However, the existing low-temperature TGIC curing polyester resin can only guarantee its leveling and anti-blooming performance to a certain extent, but it is difficult to effectively control the rate of low-temperature curing, so that the storage stability and anti-blooming performance of the existing low-temperature TGIC curing polyester resin in actual application are poor, and it is difficult to meet the actual application requirements. For this reason, a new technical solution is needed to solve the above technical problems. Summary of the invention
[0004] The object of the present invention is to provide a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin and a preparation method and application thereof, so as to solve the problems raised in the above background technology that it is difficult to effectively control the low-temperature curing rate of the low-temperature TGIC-cured polyester resin at the current stage, resulting in poor storage stability and anti-blooming performance of the existing low-temperature TGIC-cured polyester resin in practical applications, and it is difficult to meet the actual application needs.
[0005] To achieve the above object, the present invention provides the following technical solution: a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin, wherein the raw material components of the polyester resin include, by mass, 20 to 40 parts of polyols, 40 to 60 parts of polyacids, 10 to 30 parts of acidifying end-capping agents, 0.01 to 0.1 parts of organic tin catalysts, 0.05 to 0.15 parts of antioxidants, and 0.5 to 1.5 parts of curing accelerators, wherein the polyols are neopentyl glycol, 1,2,4-butanetriol, 3,3-dimethylpentane-1,5-diol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 2,2-diethyl-1,3-propanediol, and the like. The polyacid is a mixture of terephthalic acid, isophthalic acid, methylsuccinic acid, and trans-1,4-cyclohexanedicarboxylic acid; the acidifying end-capping agent is a mixture of maleic anhydride, phthalic anhydride, 1,2-cyclohexanedicarboxylic anhydride, and 2-hydroxypropane-1,2,3-tricarboxylic acid; the organic tin catalyst is a mixture of one or two of monobutyltin oxide, triphenyltin oxide, and butyltin hydroxide; the antioxidant is a mixture of one or two of phosphorous acid and N-phenyl-2-naphthylamine; and the curing accelerator is a mixture of one or two of triphenylethylphosphonium bromide and butyltriphenylphosphonium chloride.
[0006] Furthermore, the polyester resin has an acid value of 40 to 50 mgKOH / g, a viscosity of 1750 to 1950 mPas@200°C, and a glass transition temperature of 50 to 54°C.
[0007] According to the above-set raw material components, the anti-blooming low-temperature TGIC curing weather-resistant polyester resin is prepared, and the specific steps are as follows: S1. Esterification reaction of polyol and polyacid under the action of organic tin catalyst at 200-240° C. for 8-10 hours to obtain a prepolymer, wherein the acid value of the prepolymer is 30-33 mgKOH / g and the viscosity is 300-500 cps@200° C.; S2, lowering the temperature to 200-220°C, adding an antioxidant to the prepolymer, stirring for 4-6 minutes, raising the temperature to 200-240°C, and conducting a vacuum polycondensation reaction under negative pressure for 3-5 hours, wherein the vacuum degree of the vacuum polycondensation reaction is -0.09-0.1Mpa, and the acid value is 15-18 mgKOH / g and the viscosity is 2800-3200 cps@200°C at the end of the vacuum polycondensation reaction; S3. After the vacuum polycondensation reaction is completed, an inert gas is introduced to break the vacuum, the temperature is lowered to 210-220°C, and an acidified end-capping agent is added to carry out an end-capping reaction. At the end of the end-capping reaction, the acid value is 40-50 mgKOH / g and the viscosity is 2000-3000 cps@200°C; S4, after the end-capping reaction is completed, a curing accelerator is added at 165-178° C. for 5-10 minutes of curing treatment; S5, after the curing treatment, the final product, the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin, is obtained through discharging, cooling, crushing and packaging.
[0008] The anti-blooming low-temperature TGIC-cured weather-resistant polyester resin prepared by using the above-set raw material components and preparation method can be applied to the production of powder coatings.
[0009] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention optimizes the composition structure of raw materials and the ratio between the raw materials, so that the anti-blooming performance of the polyester resin is effectively improved, and the problem of "white frost" on the coating surface affecting the aesthetics of the product is avoided. Triphenylethylphosphonium bromide and butyltriphenylphosphonium chloride are used as curing accelerators, so that the curing rate of the polyester resin can be effectively controlled at a relatively low temperature, and the low-temperature curing time is effectively shortened, and the production efficiency is improved. At the same time, energy consumption is effectively reduced, and a better energy-saving effect is ensured, so that the storage stability and anti-blooming performance of the polyester resin in practical applications are better, and the actual application requirements are met. By changing the composition structure of polyols and polyacids, the polyester resin has excellent mechanical properties (mechanical properties include hardness, wear resistance and adhesion) and chemical resistance after low-temperature curing, so that the polyester resin can resist the erosion of chemical substances and extend the service life of the coating; 2. The present invention uses an acidified end-capping agent, an organic tin catalyst and an antioxidant to catalyze the reaction of polyols and polyacids, so that the polyester resin does not produce harmful byproducts when cured at low temperature, effectively improving the safety of the polyester resin preparation, being more friendly to operators and the environment, and meeting the environmental protection requirements of green production; 3. The present invention adopts five preparation steps of prepolymer-vacuum polycondensation reaction-capping reaction-curing treatment-discharging, cooling, crushing and packaging, so that the preparation process of the polyester resin is simpler, the preparation cost of the polyester resin is effectively reduced, and the preparation effect and efficiency of the polyester resin are guaranteed. By performing the curing treatment at 165-178° C., the polyester resin can be quickly cured at a relatively low temperature, and the low-temperature curing time is shortened, thereby ensuring the storage stability and anti-blooming performance of the polyester resin in practical applications, and meeting the actual application requirements; 4. The present invention optimizes the formula of the polyester resin composition so that the polyester resin can not only exhibit stronger weather resistance when used outdoors, but also resist the influence of ultraviolet rays, rain and other adverse environmental factors for a long time, maintain the performance and appearance quality of the coating. The polyester resin is applied to powder coatings and can be widely used in special occasions with anti-blooming properties, such as outdoor facilities and low-temperature environment operating equipment, and has strong market competitiveness and application prospects. DETAILED DESCRIPTION
[0010] The following examples are used to further illustrate the content of the present invention, but do not limit the application of the present invention. Embodiment 1:
[0011] This embodiment provides a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin, and a preparation method thereof comprises the following steps: First, the raw materials are taken according to the following mass parts: neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol, 2,2-diethyl-1,3-propylene glycol, terephthalic acid, isophthalic acid, methylsuccinic acid, trans-1,4-cyclohexanedicarboxylic acid, maleic anhydride, 1,2-cyclohexanedicarboxylic anhydride, monobutyltin oxide, phosphorous acid, and triphenylethylphosphine bromide, the mass parts of which are 17:3.5:10.5:3.5:5:49:2:2:3:3:0.5:1: 0.7:0.3, wherein a mixture of neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol and 2,2-diethyl-1,3-propanediol is used as a polyol, a mixture of terephthalic acid, isophthalic acid, methylsuccinic acid and trans-1,4-cyclohexanedicarboxylic acid is used as a polyacid, maleic anhydride and 1,2-cyclohexanedicarboxylic anhydride are used as acidifying end-capping agents, monobutyl tin oxide is used as an organic tin catalyst, phosphorous acid is used as an antioxidant, and triphenylethylphosphine bromide is used as a curing accelerator; Secondly, neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol, 2,2-diethyl-1,3-propylene glycol are placed in a reactor protected by nitrogen, and terephthalic acid, isophthalic acid, methylsuccinic acid, trans-1,4-cyclohexanedicarboxylic acid and monobutyltin oxide are added. Under the protection of nitrogen, the temperature is raised to 210°C, the esterification reaction is started and the water is discharged. At the same time, the cooling water of the fractionation column is turned on to ensure that the column top temperature does not exceed 102°C, and then the temperature is further raised to 240°C and maintained for 6 hours to obtain a prepolymer. During the reaction, samples are taken to measure the acid value. When the acid value reaches 30-33 mgKOH / g and the viscosity reaches 300-500 cps@200°C, the esterification reaction is terminated and the vacuum polycondensation reaction is entered; Next, the temperature is lowered to 200-220°C, phosphorous acid is added to the prepolymer, stirred for 4-6 minutes, and after being fully mixed, the temperature is raised to 200-240°C again, and the vacuum is turned on. A vacuum polycondensation reaction is carried out for 3-5 hours at a negative pressure of -0.09-0.1Mpa. During the reaction, samples are taken to measure the acid value. When the acid value reaches 15-18 mgKOH / g and the viscosity reaches 2800-3200 cps@200°C, the vacuum polycondensation is terminated and the end-capping reaction is started; Then, nitrogen was introduced to break the vacuum, and the temperature was lowered to 210-220°C. Maleic anhydride and 1,2-cyclohexanedicarboxylic anhydride were added under nitrogen protection to carry out acid hydrolysis and termination (i.e., end-capping reaction). The reaction lasted for 1 hour. During the reaction, samples were taken to measure the acid value. When the acid value reached 40-50 mgKOH / g and the viscosity reached 2000-3000 cps@200°C, the end-capping reaction was completed and the curing process was started. Then, when the temperature is lowered to 165-178°C, triphenylethylphosphonium bromide is added to perform a curing treatment for 5-10 minutes; Finally, after curing treatment, the final product, the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin, is obtained after discharging, cooling, crushing and packaging. The glass transition temperature of the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin is 50.1°C. Embodiment 2:
[0012] This embodiment provides a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin, and a preparation method thereof comprises the following steps: First, the raw materials are taken according to the following mass parts: neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol, 2,2-diethyl-1,3-propylene glycol, terephthalic acid, isophthalic acid, methylsuccinic acid, trans-1,4-cyclohexanedicarboxylic acid, maleic anhydride, 1,2-cyclohexanedicarboxylic anhydride, butyltin hydroxide, phosphorous acid, and butyltriphenylphosphonium chloride, the mass parts of which are 19:3:10:3:4:45:4:4:3.5:3.5:2.5:0.5 respectively. 0.7:0.3, wherein a mixture of neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol and 2,2-diethyl-1,3-propanediol is used as a polyol, a mixture of terephthalic acid, isophthalic acid, methylsuccinic acid and trans-1,4-cyclohexanedicarboxylic acid is used as a polyacid, maleic anhydride and 1,2-cyclohexanedicarboxylic anhydride are used as acidifying end-capping agents, butyltin hydroxide is used as an organic tin catalyst, phosphorous acid is used as an antioxidant, and butyltriphenylphosphonium chloride is used as a curing accelerator; Secondly, neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol, 2,2-diethyl-1,3-propylene glycol are placed in a reactor protected by nitrogen, and terephthalic acid, isophthalic acid, methylsuccinic acid, trans-1,4-cyclohexanedicarboxylic acid and butyltin hydroxide are added. Under the protection of nitrogen, the temperature is raised to 210°C, the esterification reaction is started and the water is discharged. At the same time, the cooling water of the fractionation column is turned on to ensure that the column top temperature does not exceed 102°C, and then the temperature is further raised to 240°C and maintained for 6 hours to obtain a prepolymer. During the reaction, samples are taken to measure the acid value. When the acid value reaches 30-33 mgKOH / g and the viscosity reaches 300-500 cps@200°C, the esterification reaction is terminated and the vacuum polycondensation reaction is entered; Next, the temperature is lowered to 200-220°C, phosphorous acid is added to the prepolymer, stirred for 4-6 minutes, and after being fully mixed, the temperature is raised to 200-240°C again, and the vacuum is turned on. A vacuum polycondensation reaction is carried out for 3-5 hours at a negative pressure of -0.09-0.1Mpa. During the reaction, samples are taken to measure the acid value. When the acid value reaches 15-18 mgKOH / g and the viscosity reaches 2800-3200 cps@200°C, the vacuum polycondensation is terminated and the end-capping reaction is started; Then, nitrogen was introduced to break the vacuum, and the temperature was lowered to 210-220°C. Maleic anhydride and 1,2-cyclohexanedicarboxylic anhydride were added under nitrogen protection to carry out acid hydrolysis and termination (i.e., end-capping reaction). The reaction lasted for 1 hour. During the reaction, samples were taken to measure the acid value. When the acid value reached 40-50 mgKOH / g and the viscosity reached 2000-3000 cps@200°C, the end-capping reaction was completed and the curing process was started. Then, when the temperature is lowered to 165-178°C, butyl triphenyl phosphonium chloride is added to perform a curing treatment for 5-10 minutes; Finally, after curing treatment, the final product, the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin, is obtained after discharging, cooling, crushing and packaging. The glass transition temperature of the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin is 51.3°C. Embodiment 3:
[0013] This embodiment provides a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin, and a preparation method thereof comprises the following steps: First, the raw materials are taken according to the following mass parts: neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol, 2,2-diethyl-1,3-propanediol, terephthalic acid, isophthalic acid, methylsuccinic acid, trans-1,4-cyclohexanedicarboxylic acid, maleic anhydride, 1,2-cyclohexanedicarboxylic anhydride, triphenyltin oxide, N-phenyl-2-naphthylamine, and triphenylethylphosphine bromide, the mass parts of which are 19:3:5:3:7.5:46:4:4:3:3:2.5:0.5:0 respectively. 7:0.3, wherein a mixture of neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol and 2,2-diethyl-1,3-propanediol is used as a polyol, a mixture of terephthalic acid, isophthalic acid, methylsuccinic acid and trans-1,4-cyclohexanedicarboxylic acid is used as a polyacid, maleic anhydride and 1,2-cyclohexanedicarboxylic anhydride are used as acidifying end-capping agents, triphenyltin oxide is used as an organic tin catalyst, N-phenyl-2-naphthylamine is used as an antioxidant, and triphenylethylphosphine bromide is used as a curing accelerator; Secondly, neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol, 2,2-diethyl-1,3-propylene glycol are placed in a reactor protected by nitrogen, and terephthalic acid, isophthalic acid, methylsuccinic acid, trans-1,4-cyclohexanedicarboxylic acid and triphenyltin oxide are added. Under the protection of nitrogen, the temperature is raised to 210°C, the esterification reaction is started and the water is discharged. At the same time, the cooling water of the fractionation column is turned on to ensure that the column top temperature does not exceed 102°C, and then the temperature is further raised to 240°C and maintained for 6 hours to obtain a prepolymer. During the reaction, samples are taken to measure the acid value. When the acid value reaches 30-33 mgKOH / g and the viscosity reaches 300-500 cps@200°C, the esterification reaction is terminated and a vacuum polycondensation reaction is entered; Next, the temperature is lowered to 200-220°C, N-phenyl-2-naphthylamine is added to the prepolymer, and stirred for 4-6 minutes. After being fully mixed, the temperature is raised to 200-240°C again, and the vacuum is turned on. A vacuum polycondensation reaction is carried out for 3-5 hours at a negative pressure of -0.09-0.1Mpa. During the reaction, samples are taken to measure the acid value. When the acid value reaches 15-18 mgKOH / g and the viscosity reaches 2800-3200 cps@200°C, the vacuum polycondensation is terminated and the end-capping reaction is started. Then, nitrogen was introduced to break the vacuum, and the temperature was lowered to 210-220°C. Maleic anhydride and 1,2-cyclohexanedicarboxylic anhydride were added under nitrogen protection to carry out acid hydrolysis and termination (i.e., end-capping reaction). The reaction lasted for 1 hour. During the reaction, samples were taken to measure the acid value. When the acid value reached 40-50 mgKOH / g and the viscosity reached 2000-3000 cps@200°C, the end-capping reaction was completed and the curing process was started. Then, when the temperature is lowered to 165-178°C, triphenylethylphosphonium bromide is added to perform a curing treatment for 5-10 minutes; Finally, after curing treatment, the final product, the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin, is obtained after discharging, cooling, crushing and packaging. The glass transition temperature of the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin is 51.2°C. Embodiment 4:
[0014] This embodiment provides a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin, and a preparation method thereof comprises the following steps: First, the raw materials were taken according to the following mass parts: neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol, 2,2-diethyl-1,3-propanediol, terephthalic acid, isophthalic acid, methylsuccinic acid, trans-1,4-cyclohexanedicarboxylic acid, maleic anhydride, 1,2-cyclohexanedicarboxylic anhydride, monobutyltin oxide, phosphorous acid, and triphenylethylphosphine bromide, the mass parts of which were 19:3:16:3:1:45:4:4:3:3:0.5:2.5:0 respectively. 7:0.3, wherein a mixture of neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol and 2,2-diethyl-1,3-propanediol is used as a polyol, a mixture of terephthalic acid, isophthalic acid, methylsuccinic acid and trans-1,4-cyclohexanedicarboxylic acid is used as a polyacid, maleic anhydride and 1,2-cyclohexanedicarboxylic anhydride are used as acidifying end-capping agents, monobutyltin oxide is used as an organotin catalyst, phosphorous acid is used as an antioxidant, and triphenylethylphosphine bromide is used as a curing accelerator; Secondly, neopentyl glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,3-dimethylpentane-1,5-diol, 1,2,4-butanetriol, 2,2-diethyl-1,3-propylene glycol are placed in a reactor protected by nitrogen, and terephthalic acid, isophthalic acid, methylsuccinic acid, trans-1,4-cyclohexanedicarboxylic acid and monobutyltin oxide are added. Under the protection of nitrogen, the temperature is raised to 210°C, the esterification reaction is started and the water is discharged. At the same time, the cooling water of the fractionation column is turned on to ensure that the column top temperature does not exceed 102°C, and then the temperature is further raised to 240°C and maintained for 6 hours to obtain a prepolymer. During the reaction, samples are taken to measure the acid value. When the acid value reaches 30-33 mgKOH / g and the viscosity reaches 300-500 cps@200°C, the esterification reaction is terminated and the vacuum polycondensation reaction is entered; Next, the temperature is lowered to 200-220°C, phosphorous acid is added to the prepolymer, stirred for 4-6 minutes, and after being fully mixed, the temperature is raised to 200-240°C again, and the vacuum is turned on. A vacuum polycondensation reaction is carried out for 3-5 hours at a negative pressure of -0.09-0.1Mpa. During the reaction, samples are taken to measure the acid value. When the acid value reaches 15-18 mgKOH / g and the viscosity reaches 2800-3200 cps@200°C, the vacuum polycondensation is terminated and the end-capping reaction is started; Then, nitrogen was introduced to break the vacuum, and the temperature was lowered to 210-220°C. Maleic anhydride and 1,2-cyclohexanedicarboxylic anhydride were added under nitrogen protection to carry out acid hydrolysis and termination (i.e., end-capping reaction). The reaction lasted for 1 hour. During the reaction, samples were taken to measure the acid value. When the acid value reached 40-50 mgKOH / g and the viscosity reached 2000-3000 cps@200°C, the end-capping reaction was completed and the curing process was started. Then, when the temperature is lowered to 165-178°C, triphenylethylphosphonium bromide is added to perform a curing treatment for 5-10 minutes; Finally, after curing treatment, the final product, the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin, is obtained after discharging, cooling, crushing and packaging. The glass transition temperature of the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin is 53.4°C.
[0015] A powder coating was prepared using a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin prepared in Examples 1-4, and powder spraying and curing were performed and application performance tests were performed. The test results were compared with the application performance of a powder coating prepared using an existing low-temperature curing powder coating resin as a comparative example. The results are as follows: ; Remarks The test methods for the above test items are as follows: Adhesion performance test method: According to the national standard GB / T 9286, powder coating resin is used to make powder coating, which is sprayed on a 1mm thick steel plate by electrostatic spraying. After curing, the adhesion performance is tested by the 100-grid method; Flexibility test method: According to the national standard GB / T 6742, powder coating resin is used to make powder coating, which is sprayed on a 1mm thick steel plate by electrostatic spraying. After curing, the flexibility is tested by cylindrical bending method; Impact performance test method: According to the national standard GB / T 1732, powder coating resin is used to make powder coating, which is sprayed on a 1mm thick steel plate by electrostatic spraying. After curing, the impact resistance of the paint film is tested by a gravity impact instrument; Weather resistance was measured in a UVA test box according to GB / T 23987-2009, with a light intensity of 0.52W / m2, irradiation for 8h, blackboard temperature of (60±3)℃, condensation for 4h, (50±3)℃; Leveling performance rating is based on the leveling effect rating standard of PCI in the United States, and horizontal fluidity is measured in accordance with GB / T21782; Anti-blooming test: bake at 120℃ for 4 hours, then cool and measure the gloss. The lower the gloss retention rate, the better the gloss retention rate. It can be seen from the above table that the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin of the embodiment of the present invention is prepared into a powder coating with good impact resistance and flexibility. The introduction of asymmetric small molecules in the formula improves the anti-blooming performance of the powder resin. At the same time, the weather-resistant polyester resin has excellent weather resistance and can always maintain good performance during outdoor use.
Claims
1. A frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin, characterized in that: The raw material components of the polyester resin include, by mass, 20 to 40 parts of polyols, 40 to 60 parts of polyacids, 10 to 30 parts of acidified end-capping agents, 0.01 to 0.1 parts of organic tin catalysts, 0.05 to 0.15 parts of antioxidants, and 0.5 to 1.5 parts of curing accelerators, wherein the polyol is a mixture of neopentyl glycol, 1,2,4-butanetriol, 3,3-dimethylpentane-1,5-diol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, and 2,2-diethyl-1,3-propylene glycol; the polyacid is a mixture of terephthalic acid, isophthalic acid, methylsuccinic acid, and trans-1,4-cyclohexanedicarboxylic acid; and the curing accelerator is a mixture of one or two of triphenylethylphosphonium bromide and butyltriphenylphosphonium chloride.
2. The anti-blooming low-temperature TGIC-cured weather-resistant polyester resin according to claim 1, characterized in that: The polyester resin has an acid value of 40-50 mgKOH / g, a viscosity of 1750-1950 mPas@200°C, and a glass transition temperature of 50-54°C.
3. The anti-blooming low-temperature TGIC-cured weather-resistant polyester resin according to claim 1, characterized in that: The acidification end-capping agent is a mixture of maleic anhydride, phthalic anhydride, 1,2-cyclohexanedicarboxylic anhydride and 2-hydroxypropane-1,2,3-tricarboxylic acid.
4. The anti-blooming low-temperature TGIC-cured weather-resistant polyester resin according to claim 1, characterized in that: The organic tin catalyst is one or a mixture of two of monobutyl tin oxide, triphenyl tin oxide and butyl tin hydroxide.
5. The anti-blooming low-temperature TGIC-cured weather-resistant polyester resin according to claim 1, characterized in that: The antioxidant is phosphorous acid, N-phenyl-2-naphthylamine or a mixture of the two.
6. The method for preparing a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin according to any one of claims 1 to 5, characterized in that: The specific steps include: S1, subjecting a polyol and a polyacid to an esterification reaction under the action of an organic tin catalyst at 200 to 240° C. for 8 to 10 hours to obtain a prepolymer; S2, lowering the temperature to 200-220°C, adding an antioxidant to the prepolymer, stirring for 4-6 minutes, raising the temperature to 200-240°C, and conducting a vacuum polycondensation reaction under negative pressure for 3-5 hours; S3, after the vacuum polycondensation reaction is completed, an inert gas is introduced to break the vacuum, the temperature is lowered to 210-220°C, and an acidified end-capping agent is added to carry out an end-capping reaction; S4, after the end-capping reaction is completed, a curing accelerator is added at 165-178° C. for 5-10 minutes of curing treatment; S5, after the curing treatment, the final product, the anti-blooming low-temperature TGIC-cured weather-resistant polyester resin, is obtained through discharging, cooling, crushing and packaging.
7. The method for preparing a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin according to claim 6, characterized in that: In S1, the acid value of the prepolymer is 30 to 33 mgKOH / g, and the viscosity is 300 to 500 cps@200°C.
8. The method for preparing a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin according to claim 6, characterized in that: In S2, the vacuum degree of the vacuum polycondensation reaction is -0.09 to 0.1 MPa. When the vacuum polycondensation reaction is completed, the acid value is 15 to 18 mgKOH / g and the viscosity is 2800 to 3200 cps@200°C.
9. The method for preparing a frosting-resistant low-temperature TGIC-cured weather-resistant polyester resin according to claim 6, characterized in that: In S3, when the end-capping reaction is completed, the acid value is 40-50 mgKOH / g and the viscosity is 2000-3000 cps@200°C.
10. A powder coating, characterized in that: The invention is made of the anti-frosting low-temperature TGIC-cured weather-resistant polyester resin as described in any one of claims 1 to 5.
Citation Information
Cited By
High-weather-resistance polyester aqueous dispersion suitable for coiled material and preparation and application thereof
CN121045758A
High weatherable polyester aqueous dispersion for use in a web and its preparation and use
CN121045758B