Crown ether ring-containing ladder type polymer as well as synthesis method and application thereof
By designing a trapezoidal polymer containing crown ether rings, using its high hydrophilicity and adaptability, the problems of low adsorption capacity and poor stability of existing lithium ion adsorption materials are solved, and efficient lithium ion separation and enrichment are achieved. Suitable for lithium-ion extraction process in salt lake brine.
Patent Information
- Application Number
- CN202411042021.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The existing lithium-ion adsorption materials have low adsorption capacity and poor stability during the lithium extraction process in salt lake brine, making it difficult to meet the needs of efficient separation and enrichment of lithium ions.
Using a trapezoidal polymer containing crown ether ring, the structure design of two main chains and crosslinked chain bridges is formed to form a repeating structural unit containing 15 crown 4, combining methoxy linking groups to improve the hydrophilicity and adsorption of the material. Capability, used for the separation and enrichment of lithium ions in salt lake brine.
The adsorption capacity of lithium ions is significantly improved to 61.37 mg/g, the selective capture capacity of lithium ions is enhanced, and the high stability is maintained in the acid-base brine environment, adapting to the salt lake brine conditions at pH 5-10.
Smart Images

Figure CN118978683A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a ladder polymer containing a crown ether ring and a synthesis method and application thereof, belonging to the technical field of polymer materials. Background Art
[0002] As the lightest metal element in nature with the lowest standard electrode potential and the largest electrochemical equivalent, lithium is an ideal "battery metal". Therefore, it will have long-term demand rigidity in power and energy storage application scenarios that require high specific energy, and is known as the "white oil of the future."
[0003] The global lithium resource supply system is divided into two major systems: lithium extraction from ore and lithium extraction from salt lakes. Among them, lithium resources from salt lake brines account for nearly 60% of the world's proven lithium resources and are expected to become the ideal main source of global lithium resource supply in the future.
[0004] In the process of lithium extraction from salt lakes, the lithium recovery rate in the salt field section (mining and transporting brine, and drying salt fields step by step) is actually only about 40%, which is the link with the largest entrainment losses. Therefore, trying to move the lithium extraction link forward has become the focus of the current industry. The most extreme process design, which is also the technology that is currently being focused on, is to shift from "extracting lithium from old brine" to "extracting lithium from raw brine" to achieve direct lithium extraction in the true sense.
[0005] The adsorption method will play a core role in raw brine lithium extraction because it conforms to the industry trend of "low-grade, low-cost, green lithium extraction technology". Obviously, the key to raw brine lithium extraction undoubtedly lies in efficient adsorbents. Generally speaking, lithium extraction adsorbents can also achieve the versatility of old brine adsorption and raw brine adsorption, and switch as needed.
[0006] The lithium extraction adsorbent that has been commercialized and is most suitable for the widest range of brine types (chloride type, magnesium sulfate subtype, etc.) is mainly aluminum molecular sieve adsorbent, with a theoretical powder adsorption capacity of about 20 mg / g, a saturated adsorption capacity of about 5 mg / g to 10 mg / g after granulation, and a dynamic adsorption capacity of about 2 mg / g to 5 mg / g in practice, which is suitable for chloride or magnesium sulfate subtype salt lakes with a pH value of 5 to 7. The next generation of manganese ion sieve adsorbents and titanium ion sieve adsorbents have problems that need to be improved, such as easy dissolution and poor stability of manganese materials, and the high bond energy of Ti-O in titanium materials improves the stability of the molecular structure, but there are problems such as difficult desorption, slow solid-phase mass transfer, and low adsorption capacity.
[0007] Crown ether is a macrocyclic ether compound first synthesized by Charles J. Pedersen et al. in 1967. Since its synthesis, crown ether has achieved important development in a wide range of fields due to its unique ring structure and its complexing effect on metal ions.
[0008] Crown ethers can complex with metal ions, that is, the negatively charged oxygen atoms in crown ethers complex with positively charged metal cations to form stable complexes under the action of dipole-charge, thereby achieving the selective capture of metal ions by crown ethers. Crown ethers such as 15-crown-4, 14-crown-4, and 12-crown-4 have strong binding ability for lithium ions and can be used for the selective separation of lithium ions in salt lake brine.
[0009] However, crown ethers are expensive and difficult to recycle. They are often grafted or polymerized onto substrates such as fibers, organic resins, and porous macromolecular materials to form organic ligand composite materials. This organic ligand composite material not only retains the ligand's specific recognition ability for lithium ions, but also has the properties of the substrate such as high stability, acid resistance, and easy solid-liquid separation, thereby significantly improving the crown ether's accessibility and recyclability. However, in the synthesis of these organic ligand composite materials, the amount of crown ether added generally does not exceed 20%, the crown ether functional group density is low, the metal ion binding sites are few, and the adsorption capacity for lithium ions is low, making it difficult to compete with low-priced inorganic adsorption materials.
[0010] Crown ether polymers (abbreviated as polycrown ethers) also have the properties of selectively coordinating cations, and have the advantages of low toxicity and easy recycling, so they have broad application prospects in phase transfer catalysis, metal separation and concentration, etc.
[0011] Chinese patent CN100363397 C discloses a hyperbranched polymer containing a crown ether ring. Under mild reaction conditions, a series of novel hyperbranched polymers containing crown ether rings are obtained by condensing a monobenzocrown ether or a dibenzocrown ether containing two active groups with 1,3,5 trisubstituted benzene. The polymer has good coordination properties and has important application prospects in ion selective electrodes, chromatographic separation, functional membrane materials, etc.
[0012] Chinese patent CN17624518 A discloses a crown ether covalent organic polymer material, which uses triaminobenzo-18-crown-6, diaminobenzo-24-crown-8 and 1,3,5-triformylphloroglucinol as organic units, and is prepared by Schiff base condensation reaction. The crown ether covalent organic polymer material includes T-18C6-C0P and T-24C8-C0P, which are stable in a highly acidic environment, have a good adsorption effect on palladium, and also have excellent selectivity and high adsorption capacity for palladium, providing a new idea and structure for separating and recovering palladium in a highly acidic environment.
[0013] Chinese patent CN11253571 B discloses a dibenzocrown ether polyimide polymer, which is obtained by polycondensation of diamino dibenzocrown ether and aromatic dibasic acid anhydride in a solvent. The polymer has an adsorption capacity of 33.6 mg / g to 37.8 mg / g for lithium ions.
[0014] Obviously, the above crown ether polymers are all formed by condensation of crown ether monomers and cross-linking agents, and it is not noticed that the atomic binding force of crown ethers binding to various cationic ligands depends not only on the relative size of the cavity and the size of the target ion, but also on the chemical environment in which it is located. Summary of the invention
[0015] In view of the shortcomings of the prior art, the object of the present invention is to provide a lithium ion adsorption material with high adsorption capacity, strong selectivity and good stability.
[0016] Another object of the present invention is to provide a method for synthesizing the lithium ion adsorption material of the present invention.
[0017] Another object of the present invention is to use the lithium ion adsorption material of the present invention to separate and enrich lithium ions in salt lake brine.
[0018] To achieve the above object, the present invention provides a ladder polymer containing a crown ether ring, which consists of two main chains and a cross-linked bridge. The first main chain is a polyoxyethylene chain, and the second main chain is a polyoxypropylene chain. The two chains are connected by repeated cross-linked bridges of dimethyl ether groups. The number average molecular weight is 5600 to 13000, and the chemical structure is as follows:
[0019]
[0020] Wherein, n is the number of ethoxy repeating units in the first main chain, m is the number of propoxy repeating units in the second main chain, and M is the connecting group on the second main chain.
[0021] The two main chains of the ladder polymer containing the crown ether ring are cross-linked with the repeating chain bridge to form a repeating structural unit containing the following 15 crowns 4, and the cavity radius is Similar to the radius of lithium ions, it has strong adaptability.
[0022]
[0023] The connecting group M on the second main chain of the ladder polymer containing a crown ether ring includes methyl, ethyl and methoxy, preferably methoxy, which enhances the hydrophilicity of the polymer and improves the ability to capture lithium ions.
[0024] The synthesis method of the crown ether ring-containing ladder polymer comprises the following steps:
[0025] First, an intermediate polymer is prepared, comprising:
[0026] A1) weighing a 3-(2-oxiranemethoxy)methyl-oxetane derivative monomer and mixing it with an anhydrous organic solvent to prepare a solution with a molar ratio of 1:0.3 to 1;
[0027] A2) injecting 2.0% to 6.0% of anionic polymerization initiator in nitrogen atmosphere to initiate anionic polymerization of the monomer solution at a temperature of 40° C. to 65° C. for 60 h to 120 h;
[0028] A3) After the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then washed with an anhydrous organic solvent corresponding to step A1, and finally dried to obtain an intermediate polymer, which is composed of the following repeating structural units:
[0029]
[0030] Wherein, n is the number of repetitions of the structural unit.
[0031] Then, preparing the target polymer comprises:
[0032] B1) weighing the intermediate polymer and mixing with an anhydrous organic solvent to prepare a solution with a molar ratio of 1:0.1 to 0.5;
[0033] B2) injecting a co-initiator and 2.0% to 4.0% of a cationic polymerization initiator in the amount of the intermediate polymer substance under a nitrogen atmosphere to initiate a cationic polymerization reaction of the intermediate polymer solution at a temperature of 0° C. to 30° C. for 100 h to 144 h;
[0034] B3) After the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then washed with the corresponding anhydrous organic solvent in step B1, and finally dried to obtain the target polymer, i.e., a ladder polymer containing a crown ether ring.
[0035] The 3-(2-oxiranemethoxy)methyl-oxetane derivative in step A1 has the general chemical structure formula:
[0036]
[0037] Wherein, M is a connecting group on oxetane, including methyl, ethyl and methoxy.
[0038] Generally, anhydrous organic solvents can be prepared from ethanol, dichloromethane, chloroform, tetrahydrofuran and N,N-dimethylformamide by methods such as redistillation or molecular sieve dehydration.
[0039] Generally, the nitrogen atmosphere is a saturated nitrogen atmosphere, and its water oxygen concentration is less than 50 ppM.
[0040] The anionic polymerization initiator in step A2 includes sodium hydride, n-butyl lithium, tert-butyl potassium and lithium diisopropylamide.
[0041] In step B2, the co-initiator includes water, acetic acid and diethanolamine, and the cationic polymerization initiator includes aluminum trichloride, zinc dichloride, boron trifluoride and trifluoromethanesulfonic acid.
[0042] The ladder polymer containing the crown ether ring can be used to separate and enrich lithium ions in salt lake brine.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] 1. The adsorption capacity of the crown ether ring-containing ladder polymer of the present invention for lithium ions can reach 61.37 mg / g, which has obvious advantages over existing lithium ion adsorption materials such as inorganic aluminum-based adsorbents (LDH structure, lithium adsorption capacity 4-8 mg / g). The two main chains and repeating chain bridges of the ladder polymer containing crown ether rings of the present invention are cross-linked to form a repeating structural unit containing 15 crowns and 4 crowns, which is formed by bulk polymerization, has a large density of crown ether functional groups and many adsorption sites, thereby significantly improving the adsorption capacity. On the other hand, the introduction of methoxy groups in the main chain enhances the hydrophilicity of the cross-linked polymer, further improving the ability to capture lithium ions.
[0045] 2. The two main chains of the ladder polymer containing crown ether rings of the present invention are cross-linked with the repeating chain bridge to form a repeating structural unit containing 15 crowns and 4, and the cavity radius is It has a radius similar to that of lithium ions and has extremely strong adaptability, thus achieving selective capture of lithium ions.
[0046] 3. The ladder polymer containing crown ether rings of the present invention has high compressive strength and shear resistance due to its molecular chain cross-linked structure, strong adaptability to acidic and alkaline brine environment, and can adapt to various salt lake brines within pH 5-10. Compared with most current lithium adsorption materials, it has incomparable advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 is the chemical structural formula of the ladder polymer containing crown ether ring of the present invention.
[0048] Figure 2 This is an electron microscope scanning image of the ladder polymer containing crown ether rings of the present invention.
[0049] Figure 3 It is the hydrogen nuclear magnetic resonance spectrum of the intermediate polymer of the present invention.
[0050] Figure 4 It is the hydrogen nuclear magnetic resonance spectrum of the ladder polymer containing crown ether ring of the present invention. DETAILED DESCRIPTION
[0051] The present invention is described in detail below, and is intended to enable those skilled in the art to implement the present invention. It should be understood that these descriptions are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0052] The present invention provides a ladder-shaped polymer containing a crown ether ring, which is a white polymer and consists of two main chains and a cross-linked bridge, and has a chemical structural formula as follows: Figure 1 In the figure, the first main chain is a polyoxyethylene chain, the second main chain is a polyoxypropylene chain, the two chains are connected by a repeated cross-linking bridge dimethyl ether group, n is the number of ethoxy repeating units in the first main chain, m is the number of propoxy repeating units in the second main chain, and M is a connecting group on the second main chain.
[0053] The two main chains of the ladder polymer containing the crown ether ring are cross-linked with the repeating chain bridge to form a repeating structural unit containing the following 15 crowns 4, and the cavity radius is Similar to the radius of lithium ions, it has strong adaptability.
[0054]
[0055] The connecting group M on the second main chain of the ladder polymer containing a crown ether ring includes methyl, ethyl and methoxy, preferably methoxy, which enhances the hydrophilicity of the polymer and improves the ability to capture lithium ions.
[0056] Figure 2 This is a typical electron microscope scanning image of the ladder-shaped polymer containing crown ether rings of the present invention, and its surface three-dimensional network structure can be seen.
[0057] The synthesis method of the above-mentioned ladder polymer containing a crown ether ring comprises the following steps:
[0058] First, an intermediate polymer is prepared, comprising:
[0059] A1) weighing a 3-(2-oxiranemethoxy)methyl-oxetane derivative monomer and mixing it with an anhydrous organic solvent to prepare a solution with a molar ratio of 1:0.3 to 1;
[0060] A2) injecting 2.0% to 6.0% of anionic polymerization initiator in nitrogen atmosphere to initiate anionic polymerization of the monomer solution at a temperature of 40° C. to 65° C. for 60 h to 120 h;
[0061] A3) After the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then washed with an anhydrous organic solvent corresponding to step A1, and finally dried to obtain an intermediate polymer, which is composed of the following repeating structural units: Figure 3 This is a typical H NMR spectrum of the intermediate polymer.
[0062]
[0063] Wherein, n is the number of repetitions of the structural unit.
[0064] Then, preparing the target polymer comprises:
[0065] B1) weighing the intermediate polymer and mixing with an anhydrous organic solvent to prepare a solution with a molar ratio of 1:0.1 to 0.5;
[0066] B2) injecting a co-initiator and 2.0% to 4.0% of a cationic polymerization initiator in the amount of the intermediate polymer substance under a nitrogen atmosphere to initiate a cationic polymerization reaction of the intermediate polymer solution at a temperature of 0° C. to 30° C. for 100 h to 144 h;
[0067] B3) After the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then washed with an anhydrous organic solvent corresponding to step B1, and finally dried to obtain the target polymer, i.e., a ladder polymer containing a crown ether ring. Figure 4 This is its classic hydrogen nuclear magnetic resonance spectrum.
[0068] The 3-(2-oxiranemethoxy)methyl-oxetane derivative in step A1 has the general chemical structure formula:
[0069]
[0070] Wherein, M is a connecting group on oxetane, including methyl, ethyl and methoxy.
[0071] Generally, anhydrous organic solvents can be prepared from ethanol, dichloromethane, chloroform, tetrahydrofuran and N,N-dimethylformamide by methods such as redistillation or molecular sieve dehydration.
[0072] Generally, the nitrogen atmosphere is a saturated nitrogen atmosphere, and its water oxygen concentration is less than 50 ppM.
[0073] The anionic polymerization initiator in step A2 includes sodium hydride, n-butyl lithium, tert-butyl potassium and lithium diisopropylamide.
[0074] In step B2, the co-initiator includes water, acetic acid and diethanolamine, and the cationic polymerization initiator includes aluminum trichloride, zinc dichloride, boron trifluoride and trifluoromethanesulfonic acid.
[0075] Some examples of synthesizing the above-mentioned ladder polymers containing crown ether rings are further listed below.
[0076]
Example 1
[0077] First, 0.5 mol of 3-methyl-3-[(2-oxiranemethoxy)methyl]-oxetane monomer is weighed and mixed with anhydrous N,N-dimethylformamide to prepare a solution with a molar ratio of 1:0.5; in a saturated nitrogen atmosphere (water oxygen concentration is less than 50 ppM), 2.0% sodium hydride (mixed and dissolved with a trace amount of anhydrous methanol and 0.01 mol of sodium hydride) of the above monomer substance is injected to initiate an anionic polymerization reaction of the above monomer solution, and the reaction is fully reacted at a temperature of 40°C for 96 hours; after the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then repeatedly washed with anhydrous N,N-dimethylformamide and finally freeze-dried to obtain an intermediate polymer.
[0078] Then, 0.5 mol of the intermediate polymer is weighed and mixed with anhydrous chloroform to prepare a solution with a molar ratio of 1:0.1; under a saturated nitrogen atmosphere (water oxygen concentration is less than 50 ppM), a trace amount of water and 2.0% aluminum chloride (a trace amount of water and 0.01 mol of aluminum chloride are mixed and dissolved) of the intermediate polymer substance are injected to initiate the cationic polymerization reaction of the intermediate polymer solution, and the reaction is fully carried out at a temperature of 0°C for 120 hours; after the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then washed with anhydrous chloroform and finally freeze-dried to obtain the target polymer, i.e., a ladder polymer containing a crown ether ring. The number average molecular weight (Mn) of the ladder polymer containing a crown ether ring obtained by gel permeation chromatography (GPC) is 7800.
[0079]
Example 2
[0080] First, 0.5 mol of 3-methyl-3-[(2-oxiranemethoxy)methyl]-oxetane monomer is weighed and mixed with anhydrous ethanol to prepare a solution with a molar ratio of 1:1; under a saturated nitrogen atmosphere (water oxygen concentration is less than 50 ppM), 6.0% n-butyl lithium of the above monomer substance is injected to initiate an anionic polymerization reaction of the above monomer solution, and the reaction is fully carried out at a temperature of 50°C for 72 hours; after the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then repeatedly washed with anhydrous ethanol and finally freeze-dried to obtain an intermediate polymer.
[0081] Then, 0.5 mol of the intermediate polymer was weighed and mixed with anhydrous ethanol to prepare a solution with a molar ratio of 1:0.1; under a saturated nitrogen atmosphere (water oxygen concentration is less than 50 ppM), a trace amount of water and 4.0% zinc dichloride (a trace amount of water and 0.02 mol of zinc dichloride were mixed and dissolved) of the intermediate polymer substance were injected to initiate the cationic polymerization reaction of the intermediate polymer solution, and the reaction was fully carried out at a temperature of 20°C for 144 hours; after the reaction, the solution was firstly distilled under reduced pressure to obtain a solid precipitate, which was then washed with anhydrous ethanol and finally freeze-dried to obtain the target polymer, i.e., a ladder polymer containing a crown ether ring. The number average molecular weight (Mn) of the ladder polymer containing a crown ether ring was 9100 after analysis by gel permeation chromatography (GPC).
[0082]
Example 3
[0083] First, 0.5 mol of 3-ethyl-3-[(2-oxiranemethoxy)methyl]-oxetane monomer is weighed and mixed with anhydrous ethanol to prepare a solution with a molar ratio of 1:0.3; under a saturated nitrogen atmosphere (water oxygen concentration is less than 50 ppM), 6.0% sodium hydride (0.03 mol sodium hydride) of the above monomer substance is directly added to initiate an anionic polymerization reaction of the above monomer solution, and the reaction is fully carried out at a temperature of 50° C. for 60 hours; after the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then repeatedly washed with anhydrous ethanol and finally freeze-dried to obtain an intermediate polymer.
[0084] Then, 0.5 mol of the intermediate polymer was weighed and mixed with anhydrous dichloromethane to prepare a solution with a molar ratio of 1:0.1; under a saturated nitrogen atmosphere (water oxygen concentration is less than 50 ppM), a trace amount of diethanolamine and 4.0% boron trifluoride (a trace amount of diethanolamine and 0.02 mol of boron trifluoride were mixed and dissolved) of the intermediate polymer substance were injected to initiate the cationic polymerization reaction of the intermediate polymer solution, and the reaction was fully carried out at a temperature of 30°C for 100 hours; after the reaction, the solution was firstly distilled under reduced pressure to obtain a solid precipitate, which was then washed with anhydrous dichloromethane and finally freeze-dried to obtain the target polymer, a ladder polymer containing a crown ether ring. The number average molecular weight (Mn) of the ladder polymer containing a crown ether ring obtained by gel permeation chromatography (GPC) was 5600 for analysis.
[0085]
Example 4
[0086] First, 0.5 mol of 3-ethyl-3-[(2-oxiranemethoxy)methyl]-oxetane monomer is weighed and mixed with anhydrous tetrahydrofuran to prepare a solution with a molar ratio of 1:0.8; under a saturated nitrogen atmosphere (water oxygen concentration is less than 50 ppM), 6.0% potassium tert-butoxide (0.03 mol potassium tert-butoxide) of the above monomer substance is directly added to initiate the above monomer solution to undergo anionic polymerization, and the reaction is fully carried out at a temperature of 60° C. for 120 hours; after the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then repeatedly washed with anhydrous tetrahydrofuran and finally vacuum dried to obtain an intermediate polymer.
[0087] Then, 0.5 mol of the intermediate polymer is weighed and mixed with anhydrous tetrahydrofuran to prepare a solution with a molar ratio of 1:0.3; under a saturated nitrogen atmosphere (water oxygen concentration is less than 50 ppM), a trace amount of diethanolamine and 2.0% trifluoromethanesulfonic acid (a trace amount of diethanolamine and 0.01 mol of trifluoromethanesulfonic acid are mixed and dissolved) of the intermediate polymer substance are injected to initiate the cationic polymerization reaction of the intermediate polymer solution, and the reaction is fully carried out at a temperature of 20°C for 100 hours; after the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then washed with anhydrous tetrahydrofuran and finally vacuum dried to obtain the target polymer, i.e., a ladder polymer containing a crown ether ring. The number average molecular weight (Mn) of the ladder polymer containing a crown ether ring obtained by gel permeation chromatography (GPC) is 13,000 for analysis.
[0088]
Example 5
[0089] First, 0.5 mol of 3-methoxy-3-[(2-oxiranemethoxy)methyl]-oxetane monomer is weighed and mixed with anhydrous ethanol to prepare a solution with a molar ratio of 1:0.3; under a saturated nitrogen atmosphere (water oxygen concentration is less than 50 ppM), 4.0% lithium diisopropylamide (0.01 mol lithium diisopropylamide) of the above monomer substance is directly added to initiate an anionic polymerization reaction of the above monomer solution, and the reaction is fully carried out at a temperature of 65° C. for 120 hours; after the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then repeatedly washed with anhydrous ethanol and finally vacuum dried to obtain an intermediate polymer.
[0090] Then, 0.5 mol of the intermediate polymer is weighed and mixed with anhydrous dichloromethane to prepare a solution with a molar ratio of 1:0.1; under a saturated nitrogen atmosphere (water oxygen concentration is less than 50 ppM), a trace amount of acetic acid and 2.0% trifluoromethanesulfonic acid (a trace amount of acetic acid and 0.01 mol of trifluoromethanesulfonic acid are mixed and dissolved) of the intermediate polymer substance are injected to initiate the cationic polymerization reaction of the intermediate polymer solution, and the reaction is fully carried out at a temperature of 10°C for 120 hours; after the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then washed with anhydrous dichloromethane and finally vacuum dried to obtain the target polymer, i.e., a ladder polymer containing a crown ether ring. The number average molecular weight (Mn) of the ladder polymer containing a crown ether ring obtained by gel permeation chromatography (GPC) is 12,000 for analysis.
[0091] [Comparative Example]
[0092] Conventional unmodified aluminum-based adsorbents were prepared using a co-precipitation method.
[0093] First, 0.5 mol LiCl and 1.0 mol AlCl3 were weighed and placed in 100 ml water, and mixed and dissolved completely to obtain a lithium aluminum aqueous solution; then, 20 ml of a 6 mol / L NaOH solution was prepared and heated to 80°C; the lithium aluminum aqueous solution was then added dropwise to the high-speed stirred NaOH solution at a stirring speed of 350 rpm, and the temperature was maintained at 80°C for a full reaction of 1 hour, and a solid precipitate was obtained by vacuum distillation, which was then washed with distilled water for several times and freeze-dried to obtain [LiAl2(OH)6]X n- 1-n mH2O aluminum-based adsorbent.
[0094] [Simulation test of lithium extraction from salt lake]
[0095] Simulated salt lake brine: Na + 102.4g / L, Mg 2+ 15.9g / L, Li + 0.81g / L, Cl - 201.9g / L, Ca 2+ 2.78, K + 16.3g / L, SO4 2- 20.8g / L, pH 7.4.
[0096] Test method:
[0097] The adsorbent materials were placed in a group of simulated salt lake brine (pre-adsorption solution) and stirred for adsorption at a temperature of 15°C, a stirring speed of 300 r / min, and an adsorption time of 2 h. After the adsorption was completed, vacuum filtration was performed to obtain the post-adsorption solution and the loaded adsorbent material.
[0098] Take the above-mentioned loaded adsorbent material, and desorb it with a hydrochloric acid solution with a concentration of 0.5 mol / L at a rotation speed of 300 r / min and a desorption time of 2 h. After the desorption is completed, vacuum filtration is performed to obtain a desorption solution and an unloaded adsorbent material.
[0099] The element concentrations in the solution before adsorption, the solution after adsorption and the desorption solution were determined by ICP-MS.
[0100] The adsorption capacity of the adsorbent material for lithium ions is calculated according to the following formula:
[0101] Q t =(C0-C t )×V / m
[0102] Among them, Q t ——Adsorption capacity, C0——Lithium ion concentration of solution before adsorption, C t ——Lithium ion concentration of the solution after adsorption, V——volume of the solution, m——mass of the adsorption material.
[0103] The ladder polymers containing crown ether rings obtained in Examples 1 to 5 and the conventional unmodified aluminum-based adsorbent prepared by coprecipitation method in the comparative example were used to carry out a simulation test on lithium extraction from salt lakes. The test results are shown in Tables 1 and 2.
[0104] Table 1 Adsorption capacity of adsorbent materials for lithium ions, mg / g
[0105]
[0106] Table 2 Element concentrations in analytical solutions, g / L
[0107]
[0108] Test conclusion:
[0109] 1. The adsorption capacity of the ladder polymer containing crown ether rings of the present invention for lithium ions can reach 61.37 mg / g, which has obvious advantages over existing lithium ion adsorption materials such as inorganic aluminum-based adsorbents (LDH structure 4-8 mg / g). The two main chains and repeating chain bridges of the ladder polymer containing crown ether rings of the present invention are cross-linked to form a repeating structural unit containing the following 15 crowns 4, which is formed by bulk polymerization, has a large density of crown ether functional groups and many adsorption sites, thereby significantly improving the adsorption capacity. On the other hand, the introduction of methoxy groups in the main chain enhances the hydrophilicity of the cross-linked polymer, thereby improving the ability to capture lithium ions.
[0110] 2. The two main chains of the ladder polymer containing crown ether rings of the present invention are cross-linked with the repeating chain bridge to form a repeating structural unit containing the following 15 crowns 4, and the cavity radius is It has a radius similar to that of lithium ions and has strong adaptability, thus achieving selective capture of lithium ions.
[0111] 3. The ladder polymer containing crown ether rings of the present invention has high compressive strength and shear resistance due to its molecular chain cross-linked structure, strong adaptability to acidic and alkaline brine environment, and can adapt to various salt lake brines within pH 5 to 10. Compared with most current lithium adsorption materials, it has incomparable advantages.
[0112] In summary, the ladder polymer containing crown ether rings of the present invention is applied to separate and enrich lithium ions in salt lake brine, and has broad application prospects.
[0113] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A ladder polymer containing a crown ether ring, characterized in that The ladder polymer containing a crown ether ring is composed of two main chains and a cross-linked bridge. The first main chain is a polyoxyethylene chain, and the second main chain is a polyoxypropylene chain. The two chains are connected by repeated cross-linked bridges of dimethyl ether groups. The number average molecular weight is 5600 to 13000, and the chemical structure is as follows: Wherein, n is the number of ethoxy repeating units in the first main chain, m is the number of propoxy repeating units in the second main chain, and M is the connecting group on the second main chain.
2. A ladder polymer containing a crown ether ring according to claim 1, characterized in that: The two main chains of the ladder polymer containing the crown ether ring are cross-linked with the repeating chain bridge to form a repeating structural unit containing the following 15 crowns 4, and the cavity radius is 3. A ladder polymer containing a crown ether ring according to claim 2, characterized in that The connecting group M on the second main chain includes methyl, ethyl and methoxy, preferably methoxy.
4. A method for synthesizing a crown ether ring-containing ladder polymer as claimed in claims 1 to 3, characterized in that: The following steps are included: A. Preparation of an intermediate polymer, comprising: A1) weighing a 3-(2-oxiranemethoxy)methyl-oxetane derivative monomer and mixing it with an anhydrous organic solvent to prepare a solution with a molar ratio of 1:0.3 to 1; A2) injecting 2.0% to 6.0% of anionic polymerization initiator in nitrogen atmosphere to initiate anionic polymerization of the monomer solution at a temperature of 40° C. to 65° C. for 60 h to 120 h; A3) After the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then washed with an anhydrous organic solvent corresponding to step A1, and finally dried to obtain an intermediate polymer, which is composed of the following repeating structural units: Wherein, n is the number of repetitions of the structural unit. B. preparing a target polymer, comprising: B1) weighing the intermediate polymer and mixing with an anhydrous organic solvent to prepare a solution with a molar ratio of 1:0.1 to 0.5; B2) injecting a co-initiator and 2.0% to 4.0% of a cationic polymerization initiator in the amount of the intermediate polymer substance under a nitrogen atmosphere to initiate a cationic polymerization reaction of the intermediate polymer solution at a temperature of 0° C. to 30° C. for 100 h to 144 h; B3) After the reaction is completed, the solution is firstly distilled under reduced pressure to obtain a solid precipitate, which is then washed with the corresponding anhydrous organic solvent in step B1, and finally dried to obtain the target polymer ladder-shaped polycrown ether.
5. The synthesis method according to claim 4, characterized in that The 3-methyl-3-(2-oxiranemethoxy)-oxetane derivative described in step A1 has a general chemical structure formula: Wherein, M is a connecting group on oxetane, including methyl, ethyl and methoxy.
6. The synthesis method according to claim 4, characterized in that The anhydrous organic solvent includes ethanol, dichloromethane, chloroform, tetrahydrofuran and N,N-dimethylformamide.
7. The synthesis method according to claim 4, characterized in that: The nitrogen atmosphere is a saturated nitrogen atmosphere, and the water oxygen concentration is less than 50 ppM.
8. The synthesis method according to claim 4, characterized in that: The anionic polymerization initiator in step A2 includes sodium hydride, n-butyl lithium, tert-butyl potassium and lithium diisopropylamide.
9. The synthesis method according to claim 4, characterized in that: The co-initiator in step B2 includes water, acetic acid and diethanolamine, and the cationic polymerization initiator includes aluminum trichloride, zinc dichloride, boron trifluoride and trifluoromethanesulfonic acid.
10. An application of a crown ether ring-containing ladder polymer, characterized in that: The ladder polymer containing a crown ether ring as described in the preceding claims 1 to 3 and the ladder polymer containing a crown ether ring prepared by the synthesis method of claims 4 to 9 are used for separating and enriching lithium ions in salt lake brine.