Fluorine-containing inorganic polymer as well as preparation method and application thereof

By using fluorine-containing inorganic polymers as binders in solid-state batteries, the problems of insufficient bonding power and small electrochemical window of solid-state batteries are solved, and strong mechanical adhesion and high electrochemical performance are achieved at low addition amounts. And improves battery safety.

CN118978704APending Publication Date: 2024-11-19LIONGO (CHANGZHOU) NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411252827.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The solid electrolyte adhesives of existing solid-state batteries have problems such as insufficient bonding force, large amount of use, small electrochemical window and incompatible with inorganic oxides, which affect the mechanical and electrochemical properties of the battery.

Method used

Using fluorine-containing inorganic polymer as the binder for solid electrolytes, prepared by heating polycondensation reaction of aluminum hydroxide and monofluorinated phosphoric acid, providing repeating units with structure of formula (I), combining polar P-O and Al-O segments The synergistic effect of the product achieves strong mechanical adhesion and excellent inorganic compatibility, and achieves perfect bonding and electrochemical properties of the material at low addition amounts.

Benefits of technology

It provides strong mechanical adhesion and high electrochemical windows, supports stable long cycles at higher voltages, and has excellent flame retardancy to ensure battery safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978704A_ABST
    Figure CN118978704A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of chemical materials, and particularly relates to a fluorine-containing inorganic polymer as well as a preparation method and application thereof. The fluorine-containing inorganic polymer provided by the invention comprises a repeating unit with a structure as shown in a formula (I). Benefited from the synergistic effect of the polar P-O and Al-O chain segments, when the inorganic polymer provided by the invention is used as a binder of a solid electrolyte, the inorganic polymer can provide strong mechanical adhesive force to wrap the solid electrolyte under the condition of extremely small addition amount, and because the inorganic polymer is an inorganic component, the inorganic polymer has better compatibility with the inorganic solid electrolyte; due to the introduction of F, the electrochemical window of the electrolyte can be further improved, and the stable long circulation of a system with higher voltage is supported. Besides, compared with a traditional polymer binder, when the inorganic polymer provided by the invention is used as a binder of a solid electrolyte, excellent flame retardance can be provided for a battery, and the safety of the battery is ensured. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical materials, and in particular relates to a fluorine-containing inorganic polymer and a preparation method and application thereof. Background Art

[0002] Solid-state batteries are batteries that use solid electrodes and solid electrolytes. Compared with traditional liquid batteries, they have higher energy density, faster charging speed, higher safety and longer life.

[0003] For solid-state batteries, the binder of solid electrolyte plays a crucial role in both the mechanical and electrochemical properties of solid-state batteries. However, the more common solid electrolyte binders currently have problems such as insufficient bonding strength, large binder dosage, small electrochemical window, and poor compatibility with inorganic oxides. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a fluorine-containing inorganic polymer and a preparation method and application thereof. The fluorine-containing inorganic polymer provided by the present invention, when used as a binder for a solid electrolyte, can provide strong mechanical adhesion and a high electrochemical window, excellent inorganic compatibility, and can still achieve perfect bonding of the material and excellent electrochemical properties at a low addition amount.

[0005] The present invention provides a fluorine-containing inorganic polymer, comprising repeating units of formula (I):

[0006]

[0007] The present invention also provides a method for preparing a fluorine-containing inorganic polymer, comprising the following steps:

[0008] Mixing aluminum hydroxide and monofluorinated phosphoric acid, heating and polycondensing, to obtain a fluorine-containing inorganic polymer having a repeating unit of the structure of formula (I);

[0009]

[0010] Preferably, the monofluorinated phosphoric acid is mixed in the form of a monofluorinated phosphoric acid aqueous solution, and the concentration of the monofluorinated phosphoric acid aqueous solution is 45-65 vol%.

[0011] Preferably, the mass ratio of the aluminum hydroxide to the monofluorinated phosphoric acid aqueous solution is (10-50):100.

[0012] Preferably, the specific process of the heating polycondensation includes:

[0013] The mixture is first mixed and reacted at a first heating temperature for a period of time, and then mixed and reacted at a second heating temperature for a period of time; the first heating temperature is 80-90°C, and the second heating temperature is 100-120°C.

[0014] Preferably, the mixing reaction time at the first heating temperature is 20 to 40 minutes, and the mixing reaction time at the second heating temperature is 20 to 40 minutes.

[0015] The present invention provides a solid electrolyte membrane, the components of which include: an oxide electrolyte, a lithium salt and a binder, the components of the binder include the fluorine-containing inorganic polymer described in the above technical solution or the fluorine-containing inorganic polymer prepared by the preparation method described in the above technical solution.

[0016] Preferably, the oxide electrolyte is one or more of LATP, LLZO and LLTO; the lithium salt is one or more of LiPF6, LiTFSI and LiFSI.

[0017] Preferably, the mass ratio of the oxide electrolyte, the lithium salt and the binder is 100:(10-30):(2-6).

[0018] The present invention provides a battery, comprising: a positive electrode, a negative electrode and a solid electrolyte membrane arranged between the positive electrode and the negative electrode, and the solid electrolyte membrane is the solid electrolyte membrane described in the above technical solution.

[0019] Compared with the prior art, the present invention provides a fluorine-containing inorganic polymer and its preparation method and application. The fluorine-containing inorganic polymer provided by the present invention includes repeating units of the structure of formula (I). Thanks to the synergistic effect of polar PO and Al-O segments, the inorganic polymer provided by the present invention can provide strong mechanical adhesion to wrap the solid electrolyte in a very small amount when used as a binder for solid electrolytes. Since they are both inorganic components, they have better compatibility with inorganic solid electrolytes and lower interface impedance. The introduction of F can further improve the electrochemical window of the electrolyte and support the stable long cycle of higher voltage systems. In addition, compared with traditional polymer binders, the inorganic polymer provided by the present invention can also provide excellent flame retardancy for the battery when used as a binder for solid electrolytes to ensure the safety of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0021] Figure 1 It is a chemical reaction pathway diagram provided by the present invention. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The present invention provides a fluorine-containing inorganic polymer, comprising repeating units of formula (I):

[0024]

[0025] The present invention also provides a method for preparing the fluorine-containing inorganic polymer described in the above technical solution, wherein the chemical reaction path is as follows: Figure 1 As shown, the preparation steps include:

[0026] Aluminum hydroxide and monofluorinated phosphoric acid are mixed and heated for polycondensation to obtain a fluorine-containing inorganic polymer having a repeating unit of the structure of formula (I).

[0027] In the preparation method provided by the present invention, the monofluorinated phosphoric acid is preferably mixed in the form of a monofluorinated phosphoric acid aqueous solution, and the concentration of the monofluorinated phosphoric acid aqueous solution is preferably 45-65 vol%, specifically 45 vol%, 46 vol%, 47 vol%, 48 vol%, 49 vol%, 50 vol%, 51 vol%, 52 vol%, 53 vol%, 54 vol%, 55 vol%, 56 vol%, 57 vol%, 58 vol%, 59 vol%, 60 vol%, 61 vol%, 62 vol%, 63 vol%, 64 vol% or 65 vol%.

[0028] In the preparation method provided by the present invention, the mass ratio of the aluminum hydroxide and the monofluorinated phosphoric acid aqueous solution is preferably (10-50):100, specifically 10:100, 12:100, 15:100, 17:100, 20:100, 23:100, 25:100, 27:100, 30:100, 32:100, 35:100, 37:100, 40:100, 42:100, 45:100, 47:100 or 50:100.

[0029] In the preparation method provided by the present invention, the specific process of the heating polycondensation preferably includes: first mixing and reacting at a first heating temperature for a period of time, and then mixing and reacting at a second heating temperature for a period of time. Wherein, the first heating temperature is preferably 80-90°C, specifically 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C or 90°C; the time for the mixed reaction at the first heating temperature is preferably 20-40min, specifically 20min, 23min, 25min, 27min, 30min, 32min, 35min, 37min or 40min; the second heating temperature is preferably 100-120°C, specifically 100°C, 102°C, 105°C, 107°C, 110°C, 112°C, 115°C, 117°C or 120°C; the time for the mixed reaction at the second heating temperature is preferably 20-40min, specifically 20min, 23min, 25min, 27min, 30min, 32min, 35min, 37min or 40min.

[0030] In the preparation method provided by the present invention, after the fluorine-containing inorganic polymer is obtained, it is preferably dispersed in a solvent for subsequent use; the solvent is preferably ethanol.

[0031] The present invention also provides a solid electrolyte membrane, the components of which include: oxide electrolyte, lithium salt and binder.

[0032] In the solid electrolyte membrane provided by the present invention, the oxide electrolyte is preferably LATP (Li 1.3 Al 0.3 Ti 1.7 (PO4)3), LLZO(Li7La3Zr2O 12 ) and LLTO(Li 0.33 La 0.56 TiO3) or more; the lithium salt is one or more of LiPF6, LiTFSI and LiFSI; the components of the binder include the fluorine-containing inorganic polymer described in the above technical solution or the fluorine-containing inorganic polymer obtained by the preparation method described in the above technical solution.

[0033] In the solid electrolyte membrane provided by the present invention, the mass ratio of the oxide electrolyte, the lithium salt and the binder is preferably 100:(10-30):(2-6); wherein the mass ratio of the oxide electrolyte and the lithium salt can be specifically 100:10, 100:11, 100:12, 100:13, 100:14, 100:15, 100:16, 100:17, 100:18, 100:19, 100:20, 100:21, 100:22, 100:23, 100:24, 100:25 :25, 100:26, 100:27, 100:28, 100:29 or 100:30; the mass ratio of the oxide electrolyte to the binder may be 100:2, 100:2.3, 100:2.5, 100:2.7, 100:3, 100:3.2, 100:3.5, 100:3.7, 100:4, 100:4.2, 100:4.5, 100:4.7, 100:5, 100:5.2, 100:5.5, 100:5.7 or 100:6.

[0034] In the present invention, the solid electrolyte membrane is preferably formed by mixing an oxide electrolyte, a lithium salt and a binder and then pressing them, and more preferably formed by mixing an oxide electrolyte, a lithium salt and a binder dispersion and then pressing and drying them. The concentration of the binder dispersion is preferably 30 to 50 wt%, and more preferably 40 wt%.

[0035] The present invention also provides a battery, comprising: a positive electrode, a negative electrode and a solid electrolyte membrane arranged between the positive electrode and the negative electrode, wherein the solid electrolyte membrane is the solid electrolyte membrane described in the above technical solution.

[0036] The technical solution provided by the present invention uses low-cost inorganic materials to polymerize and prepare fluorine-containing inorganic polymers. Thanks to the synergistic effect of polar PO and Al-O segments, the fluorine-containing inorganic polymer, when used as a binder for solid electrolytes, can provide strong mechanical adhesion to wrap the solid electrolyte with a very small amount of addition. Since they are both inorganic components, they have better compatibility with inorganic solid electrolytes and lower interface impedance. The introduction of F can further improve the electrochemical window of the electrolyte and support the stable long cycle of higher voltage systems. In addition, compared with traditional polymer binders, the inorganic polymer provided by the present invention can also provide excellent flame retardancy for the battery when used as a binder for solid electrolytes, ensuring the safety of the battery.

[0037] For the purpose of greater clarity, the present invention is described in detail with reference to the following examples and comparative examples.

[0038] Example 1

[0039] 1. Binder synthesis

[0040] 50 g of dilute fluorinated phosphoric acid with a volume concentration of 55% was added to a round-bottom flask, and then 5 g of Al(OH)3 powder was slowly added to the above solution, stirred at 85°C for 30 min, and then heated to 110°C and stirred for 30 min to obtain a fluorine-containing inorganic polymer having a repeating unit of the structure of formula (I) (1H NMR: 3.96 (1H), 3.52 (1H)). The fluorine-containing inorganic polymer was dispersed in an ethanol solution to obtain a binder dispersion with a concentration of 40 wt%.

[0041] 2. Preparation of all-solid-state electrolyte membrane

[0042] Take 0.5 g of the above-mentioned binder dispersion, 10 g of oxide electrolyte LATP powder and 1 g of lithium salt LiTFSI, mix them in a mortar, and after mixing evenly, use a double-roll mill to press them into a film with a thickness of 30 to 50 μm, then cut them into discs with a diameter of 16 mm, and vacuum dry them at 100°C.

[0043] 3. Battery assembly

[0044] Assemble the battery in the order of negative electrode, all-solid electrolyte membrane, positive electrode or according to the requirements of different test systems, with a packaging pressure of 6kg / cm 2 After packaging, the battery was placed at 60°C for 12 hours and then at room temperature for 24 hours for further testing.

[0045] Example 2

[0046] 1. Binder synthesis

[0047] 50 g of dilute fluorinated phosphoric acid with a volume concentration of 55% was added to a round-bottom flask, and then 10 g of Al(OH)3 powder was slowly added to the above solution, stirred at 85°C for 30 min, and then heated to 110°C and stirred for 30 min to obtain a fluorine-containing inorganic polymer having a repeating unit of the structure of formula (I). The fluorine-containing inorganic polymer was dispersed in an ethanol solution to obtain a binder dispersion with a concentration of 40 wt%.

[0048] 2. Preparation of all-solid-state electrolyte membrane

[0049] Take 0.75 g of the above-mentioned binder dispersion, 10 g of oxide electrolyte LLZO powder and 1.5 g of lithium salt LiTFSI, mix them in a mortar, and after mixing evenly, use a double-roll mill to press them into a film with a thickness of 30 to 50 μm, then cut them into discs with a diameter of 16 mm, and vacuum dry them at 100°C.

[0050] 3. Battery assembly

[0051] Assemble the battery in the order of negative electrode, all-solid electrolyte membrane, positive electrode or according to the requirements of different test systems, with a packaging pressure of 6kg / cm2 After packaging, the battery was placed at 60°C for 12 hours and then at room temperature for 24 hours for further testing.

[0052] Example 3

[0053] 1. Binder synthesis

[0054] 50 g of dilute fluorinated phosphoric acid with a volume concentration of 55% was added to a round-bottom flask, and then 15 g of Al(OH)3 powder was slowly added to the above solution, stirred at 85°C for 30 min, and then heated to 110°C and stirred for 30 min to obtain a fluorine-containing inorganic polymer having a repeating unit of the structure of formula (I). The fluorine-containing inorganic polymer was dispersed in an ethanol solution to obtain a binder dispersion with a concentration of 40 wt%.

[0055] 2. Preparation of all-solid-state electrolyte membrane

[0056] Take 1 g of the above-mentioned binder dispersion, 10 g of oxide electrolyte LLTO powder and 2 g of lithium salt LiPF6, mix them in a mortar, and after mixing evenly, use a double-roll mill to press them into a film with a thickness of 30 to 50 μm, then cut them into discs with a diameter of 16 mm, and vacuum dry them at 100°C.

[0057] 3. Battery assembly

[0058] Assemble the battery in the order of negative electrode, all-solid electrolyte membrane, positive electrode or according to the requirements of different test systems, with a packaging pressure of 6kg / cm 2 After packaging, the battery was placed at 60°C for 12 hours and then at room temperature for 24 hours for further testing.

[0059] Example 4

[0060] 1. Binder synthesis

[0061] 50 g of dilute fluorinated phosphoric acid with a volume concentration of 55% was added to a round-bottom flask, and then 20 g of Al(OH)3 powder was slowly added to the above solution, stirred at 85°C for 30 min, and then heated to 110°C and stirred for 30 min to obtain a fluorine-containing inorganic polymer having a repeating unit of the structure of formula (I). The fluorine-containing inorganic polymer was dispersed in an ethanol solution to obtain a binder dispersion with a concentration of 40 wt%.

[0062] 2. Preparation of all-solid-state electrolyte membrane

[0063] Take 1.25 g of the above-mentioned binder dispersion, 10 g of oxide electrolyte LATP powder and 2.5 g of lithium salt LiTFSI, mix them in a mortar, and after mixing evenly, use a double-roll mill to press them into a film with a thickness of 30 to 50 μm, then cut them into discs with a diameter of 16 mm, and vacuum dry them at 100°C.

[0064] 3. Battery assembly

[0065] Assemble the battery in the order of negative electrode, all-solid electrolyte membrane, positive electrode or according to the requirements of different test systems, with a packaging pressure of 6kg / cm 2 After packaging, the battery was placed at 60°C for 12 hours and then at room temperature for 24 hours for further testing.

[0066] Example 5

[0067] 1. Binder synthesis

[0068] 50 g of dilute fluorinated phosphoric acid with a volume concentration of 55% was added to a round-bottom flask, and then 25 g of Al(OH)3 powder was slowly added to the above solution, stirred at 85°C for 30 min, and then heated to 110°C and stirred for 30 min to obtain a fluorine-containing inorganic polymer having a repeating unit of the structure of formula (I). The fluorine-containing inorganic polymer was dispersed in an ethanol solution to obtain a binder dispersion with a concentration of 40 wt%.

[0069] 2. Preparation of all-solid-state electrolyte membrane

[0070] Take 1.5 g of the above-mentioned binder dispersion, 10 g of oxide electrolyte LLZO powder and 3 g of lithium salt LiFSI, mix them in a mortar, and after mixing evenly, use a double-roll mill to press them into a film with a thickness of 30 to 50 μm, then cut them into discs with a diameter of 16 mm, and vacuum dry them at 100°C.

[0071] 3. Battery assembly

[0072] Assemble the battery in the order of negative electrode, all-solid electrolyte membrane, positive electrode or according to the requirements of different test systems, with a packaging pressure of 6kg / cm 2 After packaging, the battery was placed at 60°C for 12 hours and then at room temperature for 24 hours for further testing.

[0073] Comparative Example 1

[0074] 1. Preparation of all-solid-state electrolyte membrane

[0075] Take 2.5 g of NMP dispersion of PVDF binder (concentration 40 wt%), 10 g of oxide electrolyte LATP powder and 1 g of lithium salt LiTFSI, mix them in a mortar, and after mixing evenly, use a double-roll mill to press them into a film with a thickness of 30 to 50 μm, and then cut them into discs with a diameter of 16 mm.

[0076] 2. Battery assembly

[0077] Assemble the battery in the order of negative electrode, all-solid electrolyte membrane, positive electrode or according to the requirements of different test systems, with a packaging pressure of 6kg / cm 2 After packaging, the battery was placed at 60°C for 12 hours and then at room temperature for 24 hours for further testing.

[0078] Comparative Example 2

[0079] 1. Preparation of all-solid-state electrolyte membrane

[0080] Take 2g of NMP dispersion of PTFE binder (concentration 60wt%), 10g of oxide electrolyte LLZO powder and 1g of lithium salt LiTFSI, mix them in a mortar, and after mixing evenly, use a double-roll mill to press them into a film with a thickness of 30-50μm, and then cut them into discs with a diameter of 16mm.

[0081] 2. Battery assembly

[0082] Assemble the battery in the order of negative electrode, all-solid electrolyte membrane, positive electrode or according to the requirements of different test systems, with a packaging pressure of 6kg / cm 2 After packaging, the battery was placed at 60°C for 12 hours and then at room temperature for 24 hours for further testing.

[0083] Performance Testing

[0084] The mechanical and electrical properties of the batteries assembled in Examples 1 to 5 and Comparative Examples 1 to 2 were tested. The test methods are as follows:

[0085] (1) Ionic conductivity test:

[0086] The button cell was assembled according to the SS|electrolyte|SS system (SS is stainless steel), and an AC impedance test was performed using an electrochemical workstation to obtain the impedance value.

[0087] The electrolyte ion conductivity is obtained according to the formula σ = L / RS; in the formula, L is the thickness of the solid electrolyte (unit: cm), R represents the impedance value obtained by fitting calculation (unit: Ω), and S represents the contact area between the solid electrolyte membrane and the electrode (unit: cm 2 ). The AC impedance test frequency used in this patent is 0.1Hz-5MHz, and the voltage amplitude is 10mV.

[0088] (2) Cation migration number test:

[0089] Measuring Li + The migration number needs to be calculated using chronoamperometry, which is to apply a polarization voltage (10mV) to the assembled Li|SSE|Li symmetric battery (SSE is a solid electrolyte), and record the current value at the beginning of polarization and the stable current value after polarization time, as well as the impedance before and after the plan. The calculation formula is as follows:

[0090] t Li +=IssRss(ΔV-IoRo)IoRo(ΔV-IssRss);

[0091] In the formula, t Li + is the lithium ion migration number, Iss is the current value after polarization stabilization (A), Rss is the impedance after polarization stabilization (Ω), Io is the current value at the beginning of polarization (A), Ro is the impedance at the beginning of polarization (Ω), and ΔV is the polarization voltage value (V).

[0092] (3) Lithium metal battery cycle test:

[0093] Using NCM811 as the positive electrode, lithium metal button batteries were assembled according to the positive electrode|electrolyte|Li system. The charge and discharge test was carried out at a charge and discharge rate of 1C to test the battery's cycle performance.

[0094] (4) Mechanical strength test:

[0095] The prepared solid electrolyte was cut into dumbbell-shaped specimens according to the national standard, and the thickness was determined using a screw micrometer. The upper and lower ends of the dumbbell-shaped specimens were fixed on a tensile machine, and a tensile test was performed at a speed of 10 mm / min to determine the breaking strength and breaking elongation.

[0096] The performance test results are shown in the following table:

[0097]

[0098] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A fluorine-containing inorganic polymer, characterized in that Comprising a repeating unit of formula (I):

2. A method for preparing a fluorine-containing inorganic polymer, characterized in that: The following steps are involved: Mixing aluminum hydroxide and monofluorinated phosphoric acid, heating and polycondensing, to obtain a fluorine-containing inorganic polymer having a repeating unit of the structure of formula (I); 3. The preparation method according to claim 2, characterized in that: The monofluorinated phosphoric acid is mixed in the form of a monofluorinated phosphoric acid aqueous solution, and the concentration of the monofluorinated phosphoric acid aqueous solution is 45-65 vol%.

4. The preparation method according to claim 3, characterized in that: The mass ratio of the aluminum hydroxide to the monofluorinated phosphoric acid aqueous solution is (10-50):

100.

5. The preparation method according to claim 2, characterized in that: The specific process of the heating polycondensation includes: The mixture is first mixed and reacted at a first heating temperature for a period of time, and then mixed and reacted at a second heating temperature for a period of time; the first heating temperature is 80-90°C, and the second heating temperature is 100-120°C.

6. The preparation method according to claim 5, characterized in that: The mixing reaction time at the first heating temperature is 20 to 40 minutes, and the mixing reaction time at the second heating temperature is 20 to 40 minutes.

7. A solid electrolyte membrane, characterized in that: The components of the solid electrolyte membrane include: an oxide electrolyte, a lithium salt and a binder, and the components of the binder include the fluorine-containing inorganic polymer according to claim 1 or the fluorine-containing inorganic polymer prepared by the preparation method according to any one of claims 2 to 6.

8. The solid electrolyte membrane according to claim 7, characterized in that: The oxide electrolyte is one or more of LATP, LLZO and LLTO; the lithium salt is one or more of LiPF6, LiTFSI and LiFSI.

9. The solid electrolyte membrane according to claim 7, characterized in that: The mass ratio of the oxide electrolyte, the lithium salt and the binder is 100:(10-30):(2-6).

10. A battery, characterized in that: The battery comprises: a positive electrode, a negative electrode and a solid electrolyte membrane arranged between the positive electrode and the negative electrode, and the solid electrolyte membrane is the solid electrolyte membrane according to any one of claims 7 to 9.