Preparation and application of perfluorosulfonic acid ion exchange membrane

By forming and peeling the ion exchange membrane on the support layer of the perfluorosulfonic acid ion exchange membrane, using chemical bonds to accompany the support layer components, the ion selectivity and cost problems of the perfluorosulfonic acid ion exchange membrane are solved, and the ion selectivity and cost problems of the perfluorosulfonic acid ion exchange membrane are achieved. Excellent electrical performance and industrial application prospects in flow batteries.

CN118978730AActive Publication Date: 2024-11-19ANHUI CONCH CLEAN ENERGY TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411275735.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The existing perfluorosulfonic acid ion exchange membrane has poor ion selectivity and high cost in all vanadium flow batteries, which limits its industrial application.

Method used

The supporting layer is prepared by aromatic organic substances containing amino functional groups, and the surface is coated with perfluorosulfonic acid ion exchange membrane resin. After curing, peeling off to form a high ion-selective perfluorosulfonic acid ion exchange membrane, and the supporting layer components are attached with chemical bonds. Improve membrane performance.

Benefits of technology

The ion selectivity and mechanical properties of the perfluorosulfonic acid ion exchange membrane are improved, so that it exhibits excellent electrical properties in all vanadium flow batteries, and has a simple and practical preparation method and high production efficiency, which is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978730A_ABST
    Figure CN118978730A_ABST
Patent Text Reader

Abstract

The invention discloses preparation and application of a perfluorosulfonic acid ion exchange membrane. The preparation method comprises the following steps: preparing a supporting layer by adopting an aromatic organic matter containing an amino functional group; coating perfluorosulfonic acid ion exchange membrane resin on the supporting layer, and forming an ion exchange membrane on the surface of the supporting layer after curing; and stripping the ion exchange membrane from the surface of the support layer. The perfluorosulfonic acid ion exchange membrane prepared by the preparation method is applied to an all-vanadium redox flow battery. The perfluorosulfonic acid ion exchange membrane prepared by the invention has relatively good ion selectivity and mechanical property, and when the perfluorosulfonic acid ion exchange membrane is applied to preparation of an all-vanadium redox flow battery, the battery has excellent electrical property. The preparation method has the characteristics of simplicity, practicability and high production efficiency, and has an industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an ion exchange membrane, and in particular to the preparation and application of a perfluorosulfonic acid ion exchange membrane for an all-vanadium liquid flow battery. Background Art

[0002] Liquid flow battery is a large-scale electrochemical energy storage technology with advantages such as long cycle life, high safety, and independent power and capacity. It can be widely used in wind power, solar power and other renewable energy power generation and storage, and realize large-scale application of renewable energy. Among them, all-vanadium liquid flow battery energy storage technology has become one of the preferred technologies for large-scale and efficient energy storage due to its high safety, long life, large output power and energy storage capacity, good charge and discharge cycle performance, and environmental friendliness.

[0003] Ion exchange membrane is one of the key materials of all-vanadium liquid flow battery. It plays the role of blocking the cross-mixing of vanadium ions in the positive and negative electrolytes, and at the same time transferring hydrogen ions to form a battery circuit. Its performance directly affects the performance of the battery system. An ideal ion exchange membrane should have the characteristics of high ion selectivity, high ion conductivity, high chemical stability and low cost. At present, the most widely used commercial membrane is the perfluorosulfonic acid ion exchange membrane (Nafion) produced by DuPont in the United States. However, its ion selectivity is relatively poor compared with non-fluorinated ion exchange membranes and its high price limits its industrial application. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a perfluorosulfonic acid ion exchange membrane, so as to solve the problem of how to prepare a perfluorosulfonic acid ion exchange membrane with high ion selectivity. Another purpose of the present invention is to propose an application of a perfluorosulfonic acid ion exchange membrane in an all-vanadium redox flow battery, so as to solve the problem of how to prepare an all-vanadium redox flow battery.

[0005] Technical solution: The method for preparing a perfluorosulfonic acid ion exchange membrane of the present invention comprises the following steps:

[0006] (1) Using aromatic organic matter containing amino functional groups to prepare the support layer;

[0007] (2) coating a perfluorosulfonic acid ion exchange membrane resin on the support layer, and forming an ion exchange membrane on the surface of the support layer after curing;

[0008] (3) Peeling off the ion exchange membrane from the surface of the support layer.

[0009] The present invention prepares a perfluorosulfonic acid ion exchange membrane by forming an ion exchange membrane layer on a support layer and then peeling off the ion exchange membrane layer. During the peeling process, a small amount of support layer components will remain on the surface of the ion exchange membrane, thereby effectively improving the ion selectivity coefficient of the perfluorosulfonic acid ion exchange membrane without affecting the mechanical properties of the membrane.

[0010] Preferably, in step (1), the method for preparing the support layer comprises the following steps:

[0011] (11) dissolving an aromatic organic compound containing an amino functional group in an organic solvent and stirring the mixture to prepare a uniform blend solution;

[0012] (12) The blended solution is poured onto a flat plate, scraped flat and the solvent is evaporated to obtain a support layer.

[0013] Preferably, the aromatic organic matter containing amino functional groups includes at least one of 1,2-benzenedicarboxylic acid amide, 1,3-benzenedicarboxylic acid amide, 1,4-benzenedicarboxylic acid amide, and 1,3,5-benzenetricarboxamide, and the organic solvent is at least one of dimethyl sulfoxide, dimethylacetamide, N-methylpyrrolidone, and N,N-dimethylformamide.

[0014] Preferably, in step (11), the molar ratio of the organic solvent to the aromatic organic compound containing an amino functional group is 100:1-100; and the stirring condition is sufficient stirring at a temperature of 50-60° C. for 12-36 hours.

[0015] Preferably, in step (12), the time for volatilizing the solvent is at least 10 seconds.

[0016] Preferably, in step (2), the method of coating the perfluorosulfonic acid ion exchange membrane resin on the support layer is: immersing the support layer in a perfluorosulfonic acid ion exchange membrane resin solution at 30-50°C for at least 5 seconds and then taking it out; the curing method is: transferring the support layer coated with the perfluorosulfonic acid ion exchange membrane resin solution into a poor solvent for curing for at least 30 minutes. The curing to form a double-layer composite membrane in this step is based on the formation of the following chemical bonds:

[0017]

[0018] Through this chemical bond, a portion of 1,2-benzenedicarbamide will be attached to the surface of the membrane when the perfluorosulfonic acid ion exchange membrane is peeled off.

[0019] Preferably, the solvent of the perfluorosulfonic acid ion exchange membrane resin solution is at least one of dimethyl sulfoxide, dimethylacetamide, N-methylpyrrolidone, and N,N-dimethylformamide, and the concentration of the solution is 5-60wt%; the poor solvent is at least one of water, ethanol, isopropanol or acetone.

[0020] Preferably, the concentration of the perfluorosulfonic acid ion exchange membrane resin solution is 10-20 wt %.

[0021] Preferably, the support layer has a thickness of at least 10 μm.

[0022] Another aspect of the present invention discloses the application of the perfluorosulfonic acid ion exchange membrane prepared by the above preparation method in an all-vanadium redox flow battery.

[0023] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0024] The perfluorosulfonic acid ion exchange membrane prepared by the invention has good ion selectivity and mechanical properties. When the perfluorosulfonic acid ion exchange membrane is used to prepare an all-vanadium liquid flow battery, the battery has excellent electrical properties.

[0025] The invention has the characteristics of simple and practical preparation method, high production efficiency and prospect of industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a microscopic morphology diagram of the perfluorosulfonic acid ion exchange membrane prepared in the present invention. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0028] Example 1: A method for preparing a perfluorosulfonic acid ion exchange membrane is as follows:

[0029] (1) 1,2-benzenedicarboxylic acid amide was dissolved in dimethyl sulfoxide and stirred at 55° C. for 24 hours to prepare a uniform mixed solution, wherein the molar ratio of dimethyl sulfoxide to 1,2-benzenedicarboxylic acid amide was 100:50.

[0030] (2) The blended solution was poured onto a flat plate, and was scraped onto a stainless steel plate using a 10 μm scraper, and the solvent was evaporated for 10 seconds, and a support layer was formed after solidification. The support layer was then immersed in a DMSO solution containing 20% ​​wt perfluorosulfonic acid ion exchange membrane resin (Suzhou Kerun NEPEM-1000) at 40°C for 10 seconds, and then taken out and transferred to water for solidification for 60 minutes to form an ion exchange membrane on the surface of the support layer.

[0031] (3) After solidification, the support layer is peeled off by conventional physical methods such as pulling or tearing to obtain a perfluorosulfonic acid ion conductive membrane containing only a dense separation layer with a membrane thickness of 0.5 μm. Figure 1 shown.

[0032] Example 2: A method for preparing a perfluorosulfonic acid ion exchange membrane is as follows:

[0033] (1) 1,3-benzenedicarboxylic acid amide was dissolved in dimethylacetamide, and the mixture was stirred at 50° C. for 36 hours to prepare a uniform mixed solution, wherein the molar ratio of dimethylacetamide to 1,3-benzenedicarboxylic acid amide was 100:10.

[0034] (2) The blended solution was poured onto a flat plate, and was scraped onto a Teflon flat plate using a 50 μm scraper, and the solvent was evaporated for 10 min, and a support layer was formed after solidification. The support layer was then immersed in a DMAC solution containing 10% wt perfluorosulfonic acid ion exchange membrane resin at 50° C. for 30 s, and then taken out and transferred to water for solidification for 30 min to form an ion exchange membrane on the surface of the support layer.

[0035] (3) After solidification, the support layer is peeled off and removed by conventional physical methods such as pulling or tearing to obtain a perfluorosulfonic acid ion conductive membrane containing only a dense separation layer.

[0036] Example 3: A method for preparing a perfluorosulfonic acid ion exchange membrane is as follows:

[0037] (1) 1,4-benzenedicarboxylic acid amide was dissolved in N-methylpyrrolidone, and the mixture was stirred at 60° C. for 12 h to prepare a uniform mixed solution, wherein the molar ratio of N-methylpyrrolidone to 1,4-benzenedicarboxylic acid amide was 100:100.

[0038] (2) The blended solution was poured onto a flat plate, and was scraped onto a stainless steel plate using a 20 μm scraper, and the solvent was evaporated for 100 seconds, and a support layer was formed after solidification. The support layer was then immersed in an NMP solution containing 60% wt perfluorosulfonic acid ion exchange membrane resin at 30° C. for 5 seconds, and then taken out and transferred to water for solidification for 45 minutes to form an ion exchange membrane on the surface of the support layer.

[0039] (3) After solidification, the support layer is peeled off and removed by conventional physical methods such as pulling or tearing to obtain a perfluorosulfonic acid ion conductive membrane containing only a dense separation layer.

[0040] Example 4: A method for preparing a perfluorosulfonic acid ion exchange membrane is as follows:

[0041] (1) 1,3,5-benzenetricarboxamide was dissolved in N,N-dimethylformamide and stirred at 40° C. for 24 h to prepare a uniform mixed solution, wherein the molar ratio of N,N-dimethylformamide to 1,3,5-benzenetricarboxamide was 100:30.

[0042] (2) The blended solution was poured onto a flat plate, and was scraped onto a Teflon flat plate using a 15 μm scraper, and the solvent was evaporated for 1 min, and a support layer was formed after solidification. The support layer was then immersed in a DMSO solution containing 5% wt perfluorosulfonic acid ion exchange membrane resin at 50° C. for 30 s, and then taken out and transferred to water for solidification for 30 min to form an ion exchange membrane on the surface of the support layer.

[0043] (3) After solidification, the support layer is peeled off and removed by conventional physical methods such as pulling or tearing to obtain a perfluorosulfonic acid ion conductive membrane containing only a dense separation layer.

[0044] Comparative Example 1: The rest is the same as Example 1, except that:

[0045] Without preparing a supporting layer, a DMSO solution of perfluorosulfonic acid ion exchange membrane resin was directly coated on a stainless steel plate to prepare a perfluorosulfonic acid ion exchange membrane with a thickness of 0.5 μm.

[0046] Comparative Example 2: Commercially available Nafion 117 with a thickness of 0.5 μm was used as the ion exchange membrane sample.

[0047] Comparative Example 3: An ion exchange membrane was prepared as follows:

[0048] 1,2-benzenedicarboxamide was added to a 20%wt DMSO solution of perfluorosulfonic acid ion exchange membrane resin, and the molar ratio of dimethyl sulfoxide to 1,2-benzenedicarboxamide was 100:1. After being fully mixed, the mixture was scraped on a stainless steel plate, and finally transferred to water for curing for 60 minutes, and the membrane layer was removed from the plate to obtain an ion exchange membrane with a thickness of 0.5 μm.

[0049] The mechanical properties, electrical properties and ion selectivity of the ion exchange membranes in Examples 1-4 and Comparative Examples 1-2 were tested as follows:

[0050] Use a final concentration of 1.5 mol / L VOSO 4 , 3 mol / L sulfuric acid aqueous solution simulates the electrolyte of all-vanadium redox flow battery, and measures H + and VO 2+ The ion diffusion coefficient of the ion when it diffuses through the ion conductive membrane to the blank side of the deionized water is calculated using H + and VO 2+ The ratio of the diffusion coefficients of the blank side H + The change of concentration over time is determined by + The composite electrode measured VO 2+ The changes in concentration over time were measured by UV-Vis spectrophotometer.

[0051] Table 1 Performance test results of different ion exchange membrane samples

[0052]

[0053] As can be seen from the results in Table 1, the lack of a small amount of residual 1,2-benzenedicarboxamide provided by the support layer will cause the ion selectivity coefficient of the ion exchange membrane to be greatly reduced. The mechanical and electrical properties of the ion exchange membrane prepared in the present invention are slightly better than those of the existing ion exchange membrane, while the ion selectivity coefficient is greatly higher than that of the existing ion exchange membrane. Comparative Example 3 shows that directly adding 1,2-benzenedicarboxamide to the ion exchange membrane not only does not improve the performance of the membrane, but instead causes a significant reduction in the ion selectivity performance.

Claims

1. A method for preparing a perfluorosulfonic acid ion exchange membrane, It is characterized in that The steps include: (1) Using aromatic organic matter containing amino functional groups to prepare the support layer; (2) coating a perfluorosulfonic acid ion exchange membrane resin on the support layer, and forming an ion exchange membrane on the surface of the support layer after curing; (3) Peeling off the ion exchange membrane from the surface of the support layer.

2. The method for preparing the perfluorosulfonic acid ion exchange membrane according to claim 1, It is characterized in that In step (1), the method for preparing the support layer comprises the following steps: (11) dissolving an aromatic organic compound containing an amino functional group in an organic solvent and stirring the mixture to prepare a uniform blend solution; (12) The blended solution is poured onto a flat plate, scraped flat and the solvent is evaporated to obtain a support layer.

3. The method for preparing the perfluorosulfonic acid ion exchange membrane according to claim 2, It is characterized in that The aromatic organic matter containing amino functional groups includes at least one of 1,2-benzenedicarboxamide, 1,3-benzenedicarboxamide, 1,4-benzenedicarboxamide, and 1,3,5-benzenetricarboxamide, and the organic solvent is at least one of dimethyl sulfoxide, dimethylacetamide, N-methylpyrrolidone, and N,N-dimethylformamide.

4. The method for preparing the perfluorosulfonic acid ion exchange membrane according to claim 2, It is characterized in that In step (11), the molar ratio of the organic solvent to the aromatic organic compound containing an amino functional group is 100:1-100; the stirring condition is to fully stir at a temperature of 50-60° C. for 12-36 hours.

5. The method for preparing the perfluorosulfonic acid ion exchange membrane according to claim 2, It is characterized in that In step (12), the time for volatilizing the solvent is at least 10 seconds.

6. The method for preparing the perfluorosulfonic acid ion exchange membrane according to claim 1, It is characterized in that In step (2), the method for coating the perfluorosulfonic acid ion exchange membrane resin on the support layer is: immersing the support layer in a perfluorosulfonic acid ion exchange membrane resin solution at 30-50° C. for at least 5 seconds and then taking it out; the method for curing is: transferring the support layer coated with the perfluorosulfonic acid ion exchange membrane resin solution into a poor solvent for curing for at least 30 minutes.

7. The method for preparing the perfluorosulfonic acid ion exchange membrane according to claim 6, It is characterized in that The solvent of the perfluorosulfonic acid ion exchange membrane resin solution is at least one of dimethyl sulfoxide, dimethylacetamide, N-methylpyrrolidone, and N,N-dimethylformamide, and the concentration of the solution is 5-60wt%; the poor solvent is at least one of water, ethanol, isopropanol, or acetone.

8. The method for preparing the perfluorosulfonic acid ion exchange membrane according to claim 7, It is characterized in that The concentration of the perfluorosulfonic acid ion exchange membrane resin solution is 10-20 wt %.

9. The method for preparing the perfluorosulfonic acid ion exchange membrane according to claim 1, It is characterized in that The support layer has a thickness of at least 10 μm.

10. Use of the perfluorosulfonic acid ion exchange membrane prepared according to the preparation method according to any one of claims 1 to 9 in an all-vanadium redox flow battery.

Citation Information

Patent Citations

  • Tertiary amine amphoteric ion exchange membrane and preparation method thereof

    CN108899566A

  • Perfluorosulfonic acid composite membrane for vanadium flow battery, preparation method thereof and use thereof

    CN110197918A

  • Multi-layer composite membrane for flow batteries or water treatment and preparation method and application of multi-layer composite membrane

    CN111495218A

  • Ion exchange membrane, preparation method thereof and flow battery

    CN117820719A

  • Ion exchange membrane and method for producing the same

    JP2016145271A