Low-carbon high-barrier biodegradable mulching film and preparation method thereof
Through the blending of PBAT, PLA, PPCP and homemade modified barrier fillers, the problems of poor water vapor gas barrier properties and poor mechanical properties of PBAT plastic film are solved, and the preparation of low-carbon high-barrier biodegradable plastic film is achieved, with excellent mechanical properties and rapid Degradation ability, suitable for agricultural mulching applications.
Patent Information
- Application Number
- CN202411263876.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The existing biodegradable plastic film PBAT has poor water vapor gas barrier properties, poor mechanical strength and slow degradation, which limits its application in agricultural plastic films.
Using PBAT, PLA, PPCP blend, and by making homemade modified barrier fillers, using chemical reactions such as silane coupling agent, lactic acid, perfluoroacyl chloride, etc., to design an aromatic ring, fat structure, ester group, carbonate and F elements. Two-dimensional sheet-like filler improves the compatibility, barrier properties and mechanical properties of the material.
The preparation of low-carbon high-barrier biodegradable plastic film has been achieved, with excellent mechanical strength, water vapor and gas barrier properties and rapid degradation capabilities, reducing labor costs and suitable for large-scale promotion.
Smart Images

Figure YMB9GCLAJZ8HZNTRMBWRJUITETU3RTLPL0MJVPEN
Abstract
Description
Technical Field
[0001] The invention relates to a low-carbon high-barrier biodegradable ground film and a preparation method thereof. The invention belongs to the field of polymer degradable films. Background Art
[0002] Ground film plays a huge role in reducing soil moisture evaporation, improving soil moisture utilization efficiency and promoting crop growth and development, which has greatly promoted the development of my country's agricultural economy. However, the polyethylene component of ordinary ground film cannot be biodegraded, resulting in "white pollution" and requiring manual cleaning, which increases labor costs. Using biodegradable ground film is a good direction. This type of material is divided into natural biodegradable ground film (such as starch, protein, cellulose, etc.) and synthetic biodegradable ground film (such as polylactic acid, polypropylene carbonate, polybutylene adipate terephthalate, etc.).
[0003] Most of the current biodegradable mulches are produced using biodegradable polyester PBAT (polybutylene adipate terephthalate). PBAT has excellent biodegradability as well as good ductility, elongation at break, heat resistance and impact resistance. However, its water vapor barrier performance is poor and it cannot block excessively strong ultraviolet rays. When used as mulch, its water vapor permeability is high and its water retention is poor, which limits its application as agricultural mulch. Therefore, it is necessary to prepare a high-barrier biodegradable mulch material that not only has good biodegradability but also has excellent water vapor barrier and mechanical properties. In addition, due to the different growth cycles of different crops, after the crop growth cycle ends, the mulch needs to be degraded as soon as possible to achieve a low-carbon effect.
[0004] Among biodegradable materials, polylactic acid (PLA) is an aliphatic polyester that naturally decomposes into CO2 and water under composting conditions. It is a green and environmentally friendly bio-sourced material. It is also the only transparent biodegradable polymer with excellent light transmittance. In addition, it also has excellent tensile strength and stiffness. PPCP (polypropylene carbonate) is a biodegradable plastic copolymerized by carbon dioxide and propylene oxide, which has good biodegradability, high water resistance and high oxygen resistance. Blending and modifying PBAT, PLA and PPCP seems to be a new direction. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a low-carbon high-barrier biodegradable mulch film in view of the defects of the prior art PBAT film, such as poor water vapor and gas barrier properties, poor mechanical strength, and slow degradation. The method is formulated to use PBAT, PPCP, and PLA as the main resins and homemade modified barrier fillers; it is prepared by mixing, granulating, and film blowing processes. The technical solution adopted by the present invention to solve its technical problems is: The present invention provides a method for preparing a modified barrier filler, comprising the following steps: S11, placing the barrier filler and the silane coupling agent containing a carbon-carbon double bond in an alcohol solvent for silylation coupling reaction to obtain an intermediate product I; S12, subjecting lactic acid to a ring-opening reaction with an epoxide to obtain an intermediate product II; S13, subjecting the intermediate product II to a nucleophilic substitution reaction with a perfluoroacyl chloride to obtain an intermediate product III; S14, free radical polymerization of the intermediate product I, the intermediate product III, aromatic acrylate, aliphatic epoxy olefins, ethylene carbonate, and unsaturated quaternary ammonium salt to obtain a target product, i.e., a modified barrier filler.
[0006] Further, The usage ratio of the barrier filler, the silane containing a carbon-carbon double bond and the alcohol solvent is 1 g: 0.8-1.5 g: 80 mL; and The barrier filler is a lamellar structure.
[0007] Furthermore, the lactic acid and epoxy olefins are added in a molar ratio of carboxyl to epoxy of 1:1.
[0008] Further, The intermediate product II and the perfluoroacyl chloride are added at a molar ratio of hydroxyl group to acyl chloride of 1:1; and The carbon atom of the perfluoroacyl chloride is C5-C8.
[0009] Furthermore, the intermediate product I, the intermediate product III, the aromatic acrylate, the aliphatic epoxy olefin, the ethylene carbonate and the unsaturated quaternary ammonium salt are added in a molar ratio of carbon-carbon double bonds of 0.15-0.25: 0.05-0.15: 0.15-0.25: 0.2-0.3: 0.1-0.2: 0.05-0.15.
[0010] The present invention also provides a modified barrier filler, which is prepared by the preparation method of the modified barrier filler.
[0011] Another object of the present invention is to provide a low-carbon high-barrier biodegradable mulch film, comprising the following raw materials in parts by weight: PPCP 15-25 parts; PLA 5-25 parts; PBAT 50-80 parts; 3.0-5.0 parts of modified barrier filler; UV absorber 0.5-1.0 part; Light stabilizer 0.2-0.5 parts; Antioxidant 0.2-0.5 parts; Anti-hydrolysis agent 0.3-0.8 parts; Plasticizer 2.0-4.0 parts; 2.0-3.0 parts of heat stabilizer; Lubricant 0.2-0.5 parts; Degradation accelerator 0.1-0.2 parts; Among them, the total mass of PPCP, PLA and PBAT is 100 parts.
[0012] Furthermore, the degradation accelerator is iron stearate.
[0013] Another object of the present invention is to provide a method for preparing a low-carbon high-barrier biodegradable mulch film, comprising the following steps: S21, mixing, i.e. Place all raw materials in a mixer according to the formula and mix them evenly; S22, granulation, i.e. Put into the granulation unit, extrude and pelletize at 160-200℃; and S23, blown film, i.e. The pellets are put into a film blowing machine for film blowing and winding to obtain a low-carbon and high-barrier biodegradable mulch film.
[0014] Beneficial effects of the present invention: (1) The present invention provides a low-carbon high-barrier biodegradable mulch film, which is mainly composed of PBAT and supplemented with PPCP and PLA as functional resins, and the resins are all degradable materials. PBAT, as the main resin, has excellent ductility, heat resistance and impact resistance; PPCP has excellent transparency and water vapor and gas barrier properties; PLA has excellent mechanical strength and stiffness. The three degradable materials complement each other and have excellent mechanical strength and ductility, stiffness, water vapor and gas barrier properties, etc.
[0015] (2) The present invention provides a low-carbon high-barrier biodegradable mulch film, the formula of which contains a self-made modified barrier filler, which is a linear macromolecular chain modified two-dimensional lamellar filler structure containing aromatic ring side groups, fatty structure side groups, ester groups, carbonates, F elements, epoxy side groups and quaternary ammonium salt structures. First, through molecular design, the chemical structure (aromatic ring, aliphatic structure, ester group, carbonate and lactate structure) in the modified barrier filler has excellent compatibility and dispersibility with the main resin, and can be used as a compatibilizer; especially the dispersibility in the PBAT phase is better; second, the two-dimensional sheet or layered structure has a good barrier effect on water vapor and oxygen; third, the F element can lead the additive to enrich on the surface, further improving the barrier property; and the hydrophobicity of the fluorine element has a positive effect on the barrier property of water vapor; fourth, the epoxy structure can react with the hydroxyl or carboxyl group in PLA and PBAT and with the plasticizer structure, and has an excellent chain extension effect; and it reduces the mobility of small molecules, which can effectively improve the mechanical properties of the material; fifth, the organic chain structure has a certain molecular chain length, which is beneficial to it being subjected to orientation force during the film blowing process, so that the filler is oriented and arranged, further improving the barrier property; sixth, the quaternary ammonium salt structure has high-efficiency broad-spectrum antibacterial properties, which is beneficial to plant growth.
[0016] (3) The present invention provides a method for preparing a low-carbon and high-barrier biodegradable mulch film. Through a reasonable formula design, a degradation accelerator is used while using additives such as UV absorbers, light stabilizers, and antioxidants to ensure that the performance of the mulch film slowly decreases during its normal service life and quickly degrades after its service life, thereby reducing labor costs and having low-carbon characteristics.
[0017] (4) The present invention provides a method for preparing a low-carbon and high-barrier biodegradable mulch film, which is prepared using a conventional film blowing process and is simple to operate and suitable for large-scale promotion and use. DETAILED DESCRIPTION
[0018] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0019] The purpose of the present invention is to develop a low-carbon high-barrier biodegradable mulch film to solve the problems of poor water vapor barrier, poor mechanical properties and slow degradation after use of the existing PBAT. The design ideas are: First, due to the dominant role of PBAT, by blending with PLA and PPCP, the problems of poor barrier and mechanical properties can be partially solved, but there is also the problem of poor compatibility of dispersants; second, through formula design, balance antioxidants, light stabilizers and other additives and add degradation promoters to achieve good performance during the service life and rapid degradation after the service life. The solution to poor dispersibility is: first, a modified two-dimensional lamellar filler is made by yourself, which has the effect of further improving the barrier properties while also having the effect of volume expansion and chain extension; at the same time, after the two-dimensional lamellar filler is modified, there will be a certain movement during the film blowing stretch orientation to form a better shielding layer, further improving the barrier properties. The theoretical basis for the realization is: first, for the modified barrier filler, a silane coupling agent is used to modify it to obtain a barrier filler containing a carbon-carbon double bond; then, lactic acid and epoxy olefins are subjected to carboxyl epoxy, and the generated hydroxyl group is subjected to substitution reaction with fluorine-containing acyl chloride to obtain olefins containing fluorine and lactic acid structure; then, acrylates or olefins with different side group structures are designed to undergo free radical polymerization to obtain macromolecular modified barrier fillers. The above-mentioned self-made ingredients are added to the formula system for mixing, granulation, and film blowing processes, and the components work synergistically with each other to effectively improve the barrier properties, mechanical properties, etc. The embodiments of the present invention are as follows: The embodiment of the present invention provides a method for preparing a modified barrier filler, comprising the following steps: S11, adding a barrier filler and a silane coupling agent containing a carbon-carbon double bond to an alcohol solvent, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 50-70° C. for 4-10 h, filtering, taking out the insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product I; The usage ratio of the barrier filler, the silane coupling agent containing a carbon-carbon double bond and the alcohol solvent is 1g: 0.8-1.5g: 80mL; and The barrier filler is a lamellar structure; it may be graphene oxide, montmorillonite, mica flakes, talcum powder, etc.; and graphene oxide is preferred; The graphene oxide is graphene oxide prepared by an improved Hummer's method; and the hydroxyl content of the graphene oxide is 3.0-8.0 mmol / g.
[0020] The silane coupling agent containing a carbon-carbon double bond may be a vinyl silane coupling agent or an acryloxy silane coupling agent; The vinyl silane coupling agent may be KH151, KH171 or KH172, etc., and preferably KH151.
[0021] The acryloxysilane coupling agent may be KH570, KH571, KH670 or GX572, etc., and KH570 is preferred.
[0022] The alcohol solvent may be anhydrous methanol, anhydrous ethanol, anhydrous isopropanol, etc., and anhydrous ethanol is preferred.
[0023] S12, add lactic acid, epoxy olefins, tetrabutylammonium bromide and hydroquinone to tetrahydrofuran, heat under reflux for 24 hours, cool to room temperature, add deionized water A, shake, add ethyl acetate for extraction, take the organic phase, dry it with anhydrous sodium sulfate A, filter, take the filtrate, distill it under reduced pressure, and dry it in vacuo at 40°C for 12 hours to obtain intermediate product II.
[0024] The lactic acid and epoxy olefins are added in a molar ratio of carboxyl group to epoxy group of 1:1; The lactic acid, tetrabutylammonium bromide, tetrahydrofuran, deionized water A, ethyl acetate, and anhydrous sodium sulfate A are added in a ratio of 1 mmol: 0.1 mmol: 5 mL: 10 mL: 20 mL: 1 g; The epoxy olefins may be glycidyl methacrylate, (glycidyloxy)ethyl methacrylate, allyl glycidyl ether, 1,2-epoxy-7-octene or 1,2-epoxy-9-decene.
[0025] The amount of hydroquinone used is 0.1wt% of the mass of the epoxy olefins.
[0026] S13, dissolve the intermediate product II and triethylamine in N,N-dimethylformamide A and place them in a reaction container, dissolve the perfluoroacyl chloride in N,N-dimethylformamide B and place it in a constant pressure dropping funnel, ice bath, stir, and after the addition is completed, control the temperature at 0-5°C and continue stirring for 8-14 hours. After the reaction is completed, filter and distill under reduced pressure, dissolve the concentrate in dichloromethane, add saturated sodium bicarbonate solution and wash 3 times, then wash 3 times with deionized water B, separate the liquids, take the organic phase, dry it with anhydrous sodium sulfate B, filter, distill the filtrate under reduced pressure, and dry it in vacuo at 80°C for 4 hours to obtain the intermediate product III.
[0027] The intermediate product II and the perfluoroacyl chloride are added at a molar ratio of hydroxyl group to acyl chloride of 1:1; The dosage ratio of the intermediate product II, triethylamine, N,N-dimethylformamide A, N,N-dimethylformamide B, dichloromethane, saturated sodium bicarbonate solution, deionized water B, and anhydrous sodium sulfate B is: 0.1 mol: 0.1 mol: 100 mL: 50 mL: 200 mL: 200 mL: 200 mL: 10 g.
[0028] The number of carbon atoms in the perfluoroacyl chloride is C5-C8; when the number of carbon atoms is less than 5, the surface migration enrichment effect of the modified barrier filler is poor, which affects the barrier effect; when the number of carbon atoms is greater than 8, the modified barrier filler is enriched on the surface, the barrier effect is excellent, but the volume expansion effect is lacking. In addition, the migration enrichment of the modified barrier filler is also related to the proportion of the intermediate product III monomer to a certain extent.
[0029] S14, add intermediate product I, intermediate product III, aromatic acrylate, aliphatic epoxy olefins, ethylene carbonate, unsaturated quaternary ammonium salt, initiator AIBN to N,N-dimethylformamide C, raise the temperature to 75-85°C, and stir for 6-10 hours; after the reaction is completed, cool to room temperature, filter, take the filtrate, distill under reduced pressure, and vacuum dry at 60°C for 6 hours to obtain the target product, i.e., the modified barrier filler.
[0030] The intermediate product I, intermediate product III, aromatic acrylate, aliphatic epoxy olefins, ethylene carbonate and unsaturated quaternary ammonium salt are added in a molar ratio of carbon-carbon double bonds of 0.15-0.25: 0.05-0.15: 0.15-0.25: 0.2-0.3: 0.1-0.2: 0.05-0.15.
[0031] The aromatic acrylate may be phenyl methacrylate, 2-phenoxyethyl acrylate, benzyl methacrylate, 4-(6-(acryloyloxy)hexyloxy)benzoic acid, etc.; and preferably 2-phenoxyethyl acrylate; The aliphatic epoxy olefins may be glycidyl methacrylate, (glycidyloxy)ethyl methacrylate, allyl glycidyl ether, 1,2-epoxy-7-octene or 1,2-epoxy-9-decene, etc.; and preferably (glycidyloxy)ethyl methacrylate; The ethylene carbonate may be ethylene carbonate or allyl methyl carbonate, etc., and preferably allyl methyl carbonate; The unsaturated quaternary ammonium salt may be acryloyloxyethyl trimethyl ammonium chloride or the like.
[0032] The usage ratio of the intermediate product I to N,N-dimethylformamide C is 1 mol:500 mL.
[0033] The amount of the initiator AIBN used is 1.0-1.5% of the total weight of the monomers.
[0034] A low-carbon high-barrier biodegradable mulch film according to an embodiment of the present invention comprises the following raw materials in parts by weight: PPCP 15-25 parts; PLA 5-25 parts; PBAT 50-80 parts; 3.0-5.0 parts of modified barrier filler; UV absorber 0.5-1.0 part; Light stabilizer 0.2-0.5 parts; Antioxidant 0.2-0.5 parts; Anti-hydrolysis agent 0.3-0.8 parts; Plasticizer 2.0-4.0 parts; 2.0-3.0 parts of heat stabilizer; Lubricant 0.2-0.5 parts; Degradation accelerator 0.1-0.2 parts; Among them, the total mass of PPCP, PLA and PBAT is 100 parts.
[0035] The PPCP, with a glass transition temperature (Tg) of 46° C., was purchased from Shandong Lianchuang Co., Ltd.
[0036] The PLA, model PT102, was purchased from Pulisi Biotechnology Co., Ltd. The PBAT, brand name TH801T, was purchased from Xinjiang Blue Mountain Tunhe Polyester Co., Ltd.
[0037] The UV absorber is a benzotriazole, specifically UV-326, UV-327, UV-328 or UV-329, etc. Moreover, in the following embodiments of the present invention, the UV absorber is UV-329.
[0038] The light stabilizer hindered amine can be UV-292, UV-770 or GW540, etc., and UV-292 is preferred. In the following embodiments of the present invention, the light stabilizer is UV-292.
[0039] The antioxidant is a hindered phenol; it can be antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant 2246, etc.; and the antioxidant described in the following embodiments of the present invention is antioxidant 1010.
[0040] The anti-hydrolysis agent is a monomeric anti-hydrolysis agent bis(2,6-diisopropylbenzene) carbodiimide, model number HyMax1010, purchased from Shanghai Langyi Functional Materials Co., Ltd.
[0041] The plasticizer can be glycerol, trimethylolpropane, pentaerythritol, triethyl citrate, low molecular weight polyester diol, polyether diol, etc.; small molecules and plasticizers with a certain molecular weight are selected for compounding and use, while achieving a certain plasticizing effect and having low migration; and the plasticizer described in the following embodiments of the present invention is glycerol, triethyl citrate, and PCL400 mixed in a mass ratio of 3:2:1.
[0042] The heat stabilizer is a calcium zinc stabilizer, specifically calcium stearate, zinc stearate, and hydrotalcite mixed in a mass ratio of 2:2:1.
[0043] The lubricant is EBS, oleamide or erucamide, and the lubricant in the following embodiments of the present invention is EBS.
[0044] The degradation accelerator is ferric stearate; ferric stearate has high photosensitivity and also has auxiliary effects on thermal stability and lubricity. By controlling the dosage and compounding with UV absorber and light stabilizer, the material can have light stabilization effect during the service life and rapid degradation effect in the later period.
[0045] The embodiment of the present invention provides a method for preparing a low-carbon high-barrier biodegradable mulch film, comprising the following steps: S21, mixing, i.e. Place all raw materials in a high-speed mixer according to the formula, stir at 200 rpm for 20-30 minutes, and mix evenly; S22, granulation, i.e. Put it into the granulation unit, extrude it at 160-190℃, water cool it, cut it into pellets, and dry it at 50℃; The twin-screw extruder in the granulator unit is a general-purpose screw with an aspect ratio of 36:1, a screw speed of 150-250rpm, and a pelletizer speed of 230-270rpm; S23, blown film, i.e. The pellets are put into a film blowing machine for film blowing and rolled up to obtain a low-carbon and high-barrier biodegradable mulch film with a thickness of 5-20 μm.
[0046] The single screw extruder in the film blowing machine is set at a temperature of 180-190° C., a rotation speed of 200-300 rpm, a traction speed of 6 m / min, and a blowing ratio of 3-4.
[0047] In order to further understand the present invention, a low-carbon high-barrier biodegradable mulch provided by the present invention is described in detail below in conjunction with specific embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0048] A method for preparing a modified barrier filler comprises the following steps: S11, adding graphene oxide and silane coupling agent KH570 to anhydrous ethanol solvent, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 8 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I; The usage ratio of the graphene oxide, the silane coupling agent KH570 and the anhydrous ethanol solvent is 1 g: 1.0 g: 80 mL; The graphene oxide is graphene oxide prepared by an improved Hummer's method; and the hydroxyl content of the graphene oxide is 5.0 mmol / g.
[0049] Its infrared data are as follows: 3315 cm -1 、1710cm -1 :-COOH exists (weak peak); 2953 cm -1 :-CH exists; 1248 cm -1 : Epoxy groups exist (weak peak); 1109 cm -1 、801cm -1 :-Si-O- exists; 1735cm -1 :-C=O exists; 1609cm -1 、811cm -1 :-C=C-exists.
[0050] S12, add lactic acid, glycidyl methacrylate, tetrabutylammonium bromide and hydroquinone to tetrahydrofuran, heat under reflux for 24 hours, cool to room temperature, add deionized water A, shake, add ethyl acetate for extraction, take the organic phase, dry it with anhydrous sodium sulfate A, filter, take the filtrate, distill it under reduced pressure, and dry it in vacuo at 40°C for 12 hours to obtain intermediate product II.
[0051] The lactic acid and glycidyl methacrylate are added in a molar ratio of carboxyl group to epoxy group of 1:1; The lactic acid, tetrabutylammonium bromide, tetrahydrofuran, deionized water A, ethyl acetate, and anhydrous sodium sulfate A are added in a ratio of 1 mmol: 0.1 mmol: 5 mL: 10 mL: 20 mL: 1 g; The amount of hydroquinone used is 0.1wt% of the mass of the epoxy olefins.
[0052] Its infrared data are as follows: 3394cm -1 :-OH exists; 1710cm -1 :-C=O (carboxyl) does not exist; 1735cm -1 :-C=O (ester group) exists; 1606cm -1 、811cm -1 :-C=C- exists; 1265cm -1 、938cm -1 、825cm -1 : Epoxy group does not exist.
[0053] S13, dissolve the intermediate product II and triethylamine in N,N-dimethylformamide A and place them in a reaction container, dissolve perfluoroheptanoyl chloride in N,N-dimethylformamide B and place them in a constant pressure dropping funnel, ice bath, stir, and after the addition is completed, control the stirring at 0°C for 14 hours. After the reaction is completed, filter and distill under reduced pressure, dissolve the concentrate in dichloromethane, add saturated sodium bicarbonate solution and wash 3 times, then wash 3 times with deionized water B, separate the liquids, take the organic phase, dry it with anhydrous sodium sulfate B, filter, distill the filtrate under reduced pressure, and dry it in vacuo at 80°C for 4 hours to obtain the intermediate product III.
[0054] The intermediate product II and perfluoroheptanoyl chloride are added at a molar ratio of hydroxyl group to acyl chloride of 1:1; The dosage ratio of the intermediate product II, triethylamine, N,N-dimethylformamide A, N,N-dimethylformamide B, dichloromethane, saturated sodium bicarbonate solution, deionized water B, and anhydrous sodium sulfate B is: 0.1 mol: 0.1 mol: 100 mL: 50 mL: 200 mL: 200 mL: 200 mL: 10 g.
[0055] Its infrared data are as follows: 3394cm -1 :-OH does not exist; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1606cm -1 、811cm -1 :-C=C- exists; 1311cm -1 :-CF exists.
[0056] S14, add intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, acryloyloxyethyl trimethylammonium chloride and initiator AIBN to N,N-dimethylformamide C, heat to 80°C, and stir for 8.5h; after the reaction is completed, cool to room temperature, filter, take the filtrate, distill under reduced pressure, and vacuum dry at 60°C for 6h to obtain the target product, i.e., the modified barrier filler.
[0057] The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0.2:0.1:0.2:0.25:0.15:0.1.
[0058] The usage ratio of the intermediate product I to N,N-dimethylformamide C is 1 mol:500 mL; The amount of the initiator AIBN used is 1.2% of the total weight of the monomers.
[0059] Its infrared data are as follows: 3315 cm -1 、1710cm -1 :-COOH exists (weak peak); 2953 cm -1 :-CH exists; 1109 cm -1 、801cm -1 :-Si-O- exists; 1735cm -1 :-C=O exists; 1623cm -1 、1609 cm -1 、811cm -1 :-C=C- does not exist; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1311cm -1 :-CF exists; 1260cm -1 、938cm -1 、825cm -1 : Epoxy group exists.
[0060] A low-carbon high-barrier biodegradable mulch film comprises the following raw materials in parts by weight: PPCP 20 parts; PLA 15 copies; PBAT 65 copies; 4.0 parts of modified barrier filler; 0.8 parts of UV absorber; Light stabilizer 0.4 parts; 0.3 parts of antioxidant; 0.5 part of anti-hydrolysis agent; 3.0 parts of plasticizer; 2.5 parts of heat stabilizer; 0.4 parts of lubricant; 0.15 parts of degradation accelerator; Among them, the total mass of PPCP, PLA and PBAT is 100 parts.
[0061] A method for preparing a low-carbon high-barrier biodegradable mulch film comprises the following steps: S21, mixing, i.e. Place all raw materials in a high-speed mixer according to the formula, stir at 200 rpm for 25 min, and mix evenly; S22, granulation, i.e. Put it into the granulation unit, set the first zone at 160℃, the second zone at 170℃, the third zone at 180℃, the die head at 180℃, extrude, water cool, granulate, and dry at 50℃; The twin-screw extruder in the granulator unit is a general-purpose screw with a length-to-diameter ratio of 36:1, a screw speed of 200 rpm, and a pelletizer speed of 250 rpm; S23, blown film, i.e. The pellets are put into a film blowing machine for film blowing and rolled up to obtain a low-carbon and high-barrier biodegradable mulch film with a thickness of 10 μm.
[0062] The single screw extruder in the film blowing machine is set to have a temperature of 180° C. in zone 1, 185° C. in zone 1, 188° C. in zone 1, a die head of 190° C., a rotation speed of 250 rpm, a traction speed of 6 m / min, and a blow-up ratio of 3.5.
[0063] The rest is the same as in Example 1, except that: S11, adding graphene oxide and silane coupling agent KH570 to anhydrous ethanol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 50° C. for 10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I; The usage ratio of the graphene oxide, the silane coupling agent KH570 and the anhydrous ethanol solvent is 1 g: 0.8 g: 80 mL; The graphene oxide is graphene oxide prepared by an improved Hummer's method; and the hydroxyl content of the graphene oxide is 3.0 mmol / g.
[0064] Its infrared data are as follows: 3315 cm -1 、1710cm -1 :-COOH exists (weak peak); 2953 cm -1 :-CH exists; 1248 cm -1 : Epoxy groups exist (weak peak); 1109 cm -1 、801cm -1 :-Si-O- exists; 1735cm -1 :-C=O exists; 1609cm -1 、811cm -1 :-C=C-exists.
[0065] S12, add lactic acid, glycidyl methacrylate, tetrabutylammonium bromide and hydroquinone to tetrahydrofuran, heat under reflux for 24 hours, cool to room temperature, add deionized water A, shake, add ethyl acetate for extraction, take the organic phase, dry it with anhydrous sodium sulfate A, filter, take the filtrate, distill it under reduced pressure, and dry it in vacuo at 40°C for 12 hours to obtain intermediate product II.
[0066] The lactic acid and glycidyl methacrylate are added in a molar ratio of carboxyl group to epoxy group of 1:1; The lactic acid, tetrabutylammonium bromide, tetrahydrofuran, deionized water A, ethyl acetate, and anhydrous sodium sulfate A are added in a ratio of 1 mmol: 0.1 mmol: 5 mL: 10 mL: 20 mL: 1 g; The amount of hydroquinone used is 0.1wt% of the mass of the epoxy olefins.
[0067] Its infrared data are as follows: 3394cm -1 :-OH exists; 1710cm -1 :-C=O (carboxyl) does not exist; 1735cm -1 :-C=O (ester group) exists; 1606cm -1 、811cm -1 :-C=C- exists; 1265cm -1 、938cm -1 、825cm -1 : Epoxy group does not exist.
[0068] S13, dissolve the intermediate product II and triethylamine in N,N-dimethylformamide A and place them in a reaction container, dissolve perfluoroheptanoyl chloride in N,N-dimethylformamide B and place it in a constant pressure dropping funnel, ice bath, stir, and after the addition is completed, control the stirring at 5°C for 8 hours. After the reaction is completed, filter and distill under reduced pressure, dissolve the concentrate in dichloromethane, add saturated sodium bicarbonate solution and wash 3 times, then wash 3 times with deionized water B, separate the liquids, take the organic phase, dry it with anhydrous sodium sulfate B, filter, distill the filtrate under reduced pressure, and dry it in vacuo at 80°C for 4 hours to obtain the intermediate product III.
[0069] The intermediate product II and perfluoroheptanoyl chloride are added at a molar ratio of hydroxyl group to acyl chloride of 1:1; The dosage ratio of the intermediate product II, triethylamine, N,N-dimethylformamide A, N,N-dimethylformamide B, dichloromethane, saturated sodium bicarbonate solution, deionized water B, and anhydrous sodium sulfate B is: 0.1 mol: 0.1 mol: 100 mL: 50 mL: 200 mL: 200 mL: 200 mL: 10 g.
[0070] Its infrared data are as follows: 3394cm -1 :-OH does not exist; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1606cm -1 、811cm -1 :-C=C- exists; 1311cm -1 :-CF exists.
[0071] S14, add intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, acryloyloxyethyl trimethylammonium chloride and initiator AIBN to N,N-dimethylformamide C, heat to 75°C, and stir for 10 hours; after the reaction is completed, cool to room temperature, filter, take the filtrate, distill under reduced pressure, and vacuum dry at 60°C for 6 hours to obtain the target product, i.e., the modified barrier filler.
[0072] The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0.2:0.1:0.2:0.25:0.15:0.1.
[0073] The usage ratio of the intermediate product I to N,N-dimethylformamide C is 1 mol:500 mL; The amount of the initiator AIBN used is 1.5% of the total weight of the monomers.
[0074] Its infrared data are as follows: 3315 cm -1 、1710cm -1 :-COOH exists (weak peak); 2953 cm -1 :-CH exists; 1109 cm -1 、801cm -1 :-Si-O- exists; 1735cm -1 :-C=O exists; 1623cm -1 、1609 cm -1 、811cm -1 :-C=C- does not exist; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1311cm -1 :-CF exists; 1260cm -1 、938cm -1 、825cm -1 : Epoxy group exists.
[0075] The rest is the same as in Example 1, except that: S11, adding graphene oxide and silane coupling agent KH570 to anhydrous ethanol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 70° C. for 4 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain intermediate product I; The usage ratio of the graphene oxide, the silane coupling agent KH570 and the anhydrous ethanol solvent is 1 g: 1.5 g: 80 mL; The graphene oxide is graphene oxide prepared by an improved Hummer's method; and the hydroxyl content of the graphene oxide is 8.0 mmol / g.
[0076] Its infrared data are as follows: 3315 cm -1 、1710cm -1 :-COOH exists (weak peak); 2953 cm -1 :-CH exists; 1248 cm -1 : Epoxy groups exist (weak peak); 1109 cm -1 、801cm -1 :-Si-O- exists; 1735cm -1 :-C=O exists; 1609cm -1 、811cm -1 :-C=C-exists.
[0077] S12, add lactic acid, glycidyl methacrylate, tetrabutylammonium bromide and hydroquinone to tetrahydrofuran, heat under reflux for 24 hours, cool to room temperature, add deionized water A, shake, add ethyl acetate for extraction, take the organic phase, dry it with anhydrous sodium sulfate A, filter, take the filtrate, distill it under reduced pressure, and dry it in vacuo at 40°C for 12 hours to obtain intermediate product II.
[0078] The lactic acid and glycidyl methacrylate are added in a molar ratio of carboxyl group to epoxy group of 1:1; The lactic acid, tetrabutylammonium bromide, tetrahydrofuran, deionized water A, ethyl acetate, and anhydrous sodium sulfate A are added in a ratio of 1 mmol: 0.1 mmol: 5 mL: 10 mL: 20 mL: 1 g; The amount of hydroquinone used is 0.1wt% of the mass of the epoxy olefins.
[0079] Its infrared data are as follows: 3394cm -1 :-OH exists; 1710cm -1 :-C=O (carboxyl) does not exist; 1735cm -1 :-C=O (ester group) exists; 1606cm -1 、811cm -1 :-C=C- exists; 1265cm -1 、938cm -1 、825cm -1 : Epoxy group does not exist.
[0080] S13, dissolve the intermediate product II and triethylamine in N,N-dimethylformamide A and place them in a reaction container, dissolve perfluoroheptanoyl chloride in N,N-dimethylformamide B and place them in a constant pressure dropping funnel, ice bath, stir, and after the addition is completed, control the stirring at 0°C for 10 hours. After the reaction is completed, filter and distill under reduced pressure, dissolve the concentrate in dichloromethane, add saturated sodium bicarbonate solution and wash 3 times, then wash 3 times with deionized water B, separate the liquids, take the organic phase, dry it with anhydrous sodium sulfate B, filter, distill the filtrate under reduced pressure, and dry it in vacuo at 80°C for 4 hours to obtain the intermediate product III.
[0081] The intermediate product II and perfluoroheptanoyl chloride are added at a molar ratio of hydroxyl group to acyl chloride of 1:1; The dosage ratio of the intermediate product II, triethylamine, N,N-dimethylformamide A, N,N-dimethylformamide B, dichloromethane, saturated sodium bicarbonate solution, deionized water B, and anhydrous sodium sulfate B is: 0.1 mol: 0.1 mol: 100 mL: 50 mL: 200 mL: 200 mL: 200 mL: 10 g.
[0082] Its infrared data are as follows: 3394cm -1 :-OH does not exist; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1606cm -1 、811cm -1 :-C=C- exists; 1311cm -1 :-CF exists.
[0083] S14, add intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, acryloyloxyethyl trimethylammonium chloride and initiator AIBN to N,N-dimethylformamide C, heat to 85°C, and stir for 6 hours; after the reaction is completed, cool to room temperature, filter, take the filtrate, distill under reduced pressure, and vacuum dry at 60°C for 6 hours to obtain the target product, i.e., the modified barrier filler.
[0084] The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0.2:0.1:0.2:0.25:0.15:0.1.
[0085] The usage ratio of the intermediate product I to N,N-dimethylformamide C is 1 mol:500 mL; The amount of the initiator AIBN used is 1.0% of the total weight of the monomers.
[0086] Its infrared data are as follows: 3315 cm -1 、1710cm -1 :-COOH exists (weak peak); 2953 cm -1 :-CH exists; 1109 cm -1 、801cm -1 :-Si-O- exists; 1735cm -1 :-C=O exists; 1623cm -1 、1609 cm -1 、811cm -1 :-C=C- does not exist; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1311cm -1 :-CF exists; 1260cm -1 、938cm -1 、825cm -1 : Epoxy group exists.
[0087] The rest is the same as in Example 1, except that: A method for preparing a modified barrier filler, wherein in S11, The silane coupling agent KH570 was replaced with KH151.
[0088] The rest is the same as in Example 1, except that: A method for preparing a modified barrier filler, wherein in S12, The glycidyl methacrylate was replaced with allyl glycidyl ether.
[0089] The rest is the same as in Example 1, except that: A method for preparing a modified barrier filler, wherein in S13, The perfluoroheptanoyl chloride was replaced by perfluoropentanoyl chloride.
[0090] The rest is the same as in Example 1, except that: A method for preparing a modified barrier filler, wherein in S13, The perfluoroheptanoyl chloride was replaced by perfluorooctanoyl chloride.
[0091] The rest is the same as in Example 1, except that: A method for preparing a modified barrier filler, wherein in S14, The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0.15:0.15:0.15:0.3:0.1:0.15.
[0092] The rest is the same as in Example 1, except that: A method for preparing a modified barrier filler, wherein in S14, The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0.25:0.05:0.25:0.2:0.2:0.05.
[0093] The rest is the same as in Example 1, except that: A low-carbon high-barrier biodegradable mulch film comprises the following raw materials in parts by weight: PPCP 15 copies; PLA 5 parts; PBAT 80 copies; 5.0 parts of modified barrier filler; 1.0 part of UV absorber; 0.5 parts of light stabilizer; 0.2 parts of antioxidant; 0.8 part of anti-hydrolysis agent; 2.0 parts of plasticizer; 3.0 parts of heat stabilizer; 0.5 parts of lubricant; 0.2 parts of degradation accelerator; Among them, the total mass of PPCP, PLA and PBAT is 100 parts.
[0094] A method for preparing a low-carbon high-barrier biodegradable mulch film comprises the following steps: S21, mixing, i.e. Place all raw materials according to the formula in a high-speed mixer and stir at 200 rpm for 20 min to mix evenly; S22, granulation, i.e. Put it into the granulation unit, set the first zone at 160℃, the second zone at 170℃, the third zone at 175℃, the die head at 178℃, extrude, water cool, pelletize, and dry at 50℃; The twin-screw extruder in the granulator unit is a universal screw with a length-to-diameter ratio of 36:1, a screw speed of 150 rpm, and a pelletizer speed of 230 rpm; S23, blown film, i.e. The pellets are put into a film blowing machine for film blowing and rolled up to obtain a low-carbon and high-barrier biodegradable mulch film with a thickness of 5 μm.
[0095] The single screw extruder in the film blowing machine is set to have a temperature of 180° C. in zone 1, 183° C. in zone 1, 185° C. in zone 1, 185° C. in die head, a rotation speed of 200 rpm, a traction speed of 6 m / min, and a blow-up ratio of 3.0.
[0096] The rest is the same as in Example 1, except that: A low-carbon high-barrier biodegradable mulch film comprises the following raw materials in parts by weight: PPCP 25 copies; PLA 25 copies; PBAT 50 copies; 3.0 parts of modified barrier filler; 0.5 parts of UV absorber; Light stabilizer 0.2 parts; 0.5 parts of antioxidant; 0.3 parts of anti-hydrolysis agent; 4.0 parts of plasticizer; 2.0 parts of heat stabilizer; 0.2 parts of lubricant; Degradation accelerator 0.1 part; Among them, the total mass of PPCP, PLA and PBAT is 100 parts.
[0097] A method for preparing a low-carbon high-barrier biodegradable mulch film comprises the following steps: S21, mixing, i.e. Place all raw materials in a high-speed mixer according to the formula, stir at 200 rpm for 30 min, and mix evenly; S22, granulation, i.e. Put it into the granulation unit, set the first zone at 160℃, the second zone at 170℃, the third zone at 180℃, the die head at 190℃, extrude, water cool, granulate, and dry at 50℃; The twin-screw extruder in the granulator unit is a general-purpose screw with a length-to-diameter ratio of 36:1, a screw speed of 250 rpm, and a pelletizer speed of 270 rpm; S23, blown film, i.e. The pellets are put into a film blowing machine for film blowing and rolled up to obtain a low-carbon and high-barrier biodegradable mulch film with a thickness of 20 μm.
[0098] The single screw extruder in the film blowing machine is set to have a temperature of 180° C. in zone 1, 185° C. in zone 2, 192° C. in zone 3, a die of 190° C., a rotation speed of 300 rpm, a traction speed of 6 m / min, and a blow-up ratio of 4.0.
[0099] The following comparative examples are compared with specific embodiment 1: Comparative Example 1 The rest is the same as in Example 1, except that: No PPCP is added to the raw material formula of the low-carbon and high-barrier biodegradable mulch film.
[0100] Comparative Example 2 The rest is the same as in Example 1, except that: No PLA is added to the raw material formula of the low-carbon and high-barrier biodegradable mulch film.
[0101] Comparative Example 3 The rest is the same as in Example 1, except that: No UV absorber is added to the raw material formula of the low-carbon and high-barrier biodegradable mulch film.
[0102] Comparative Example 4 The rest is the same as in Example 1, except that: No light stabilizer is added to the raw material formula of the low-carbon and high-barrier biodegradable mulch film.
[0103] Comparative Example 5 The rest is the same as in Example 1, except that: No antioxidant is added to the raw material formula of the low-carbon and high-barrier biodegradable mulch film.
[0104] Comparative Example 6 The rest is the same as in Example 1, except that: No anti-hydrolysis agent is added to the raw material formula of the low-carbon and high-barrier biodegradable mulch film.
[0105] Comparative Example 7 The rest is the same as in Example 1, except that: No degradation accelerator is added to the raw material formula of the low-carbon and high-barrier biodegradable mulch film.
[0106] Comparative Example 8 The rest is the same as in Example 1, except that: No modified barrier filler is added to the raw material formula of the low-carbon and high-barrier biodegradable mulch film.
[0107] Comparative Example 9 The rest is the same as in Example 1, except that: In a method for preparing a modified barrier filler, The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0:0.1:0.2:0.25:0.15:0.1; that is, intermediate product I is not added.
[0108] Comparative Example 10 The rest is the same as in Example 1, except that: In a method for preparing a modified barrier filler, The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0.2:0:0.2:0.25:0.15:0.1; that is, intermediate product III is not added.
[0109] Comparative Example 11 The rest is the same as in Example 1, except that: In a method for preparing a modified barrier filler, The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0.2:0.1:0:0.25:0.15:0.1; that is, 2-phenoxyethyl acrylate is not added.
[0110] Comparative Example 12 The rest is the same as in Example 1, except that: In a method for preparing a modified barrier filler, The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0.2:0.1:0.2:0:0.15:0.1; that is, no (glycidyloxy)ethyl methacrylate is added.
[0111] Comparative Example 13 The rest is the same as in Example 1, except that: In a method for preparing a modified barrier filler, The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0.2:0.1:0.2:0.25:0:0.1; that is, allyl methyl carbonate is not added.
[0112] Comparative Example 14 The rest is the same as in Example 1, except that: In a method for preparing a modified barrier filler, The intermediate product I, intermediate product III, 2-phenoxyethyl acrylate, (glycidyloxy)ethyl methacrylate, allyl methyl carbonate, and acryloyloxyethyl trimethylammonium chloride are added in a molar ratio of carbon-carbon double bonds of 0.2:0.1:0.2:0.25:0.15:0; that is, acryloyloxyethyl trimethylammonium chloride is not added.
[0113] The physical properties of the low-carbon high-barrier biodegradable mulch films in the embodiments of the present invention and the comparative examples are shown in Tables 1 and 2.
[0114] Table 1 Physical properties test of each embodiment Table 2 Observation records of degradation performance of various examples Number of days 40d 80d 110d 130d 145d 160d Example 1 Induction period Induction period Induction period Induction period Big Rift No membrane period Example 2 Induction period Induction period Induction period Induction period Big Rift No membrane period Example 3 Induction period Induction period Induction period Induction period Big Rift No membrane period Example 4 Induction period Induction period Induction period Induction period Big Rift No membrane period Example 5 Induction period Induction period Induction period Induction period Big Rift No membrane period Example 6 Induction period Induction period Induction period Induction period Big Rift No membrane period Example 7 Induction period Induction period Induction period Induction period Big Rift No membrane period Example 8 Induction period Induction period Induction period Induction period Big Rift No membrane period Example 9 Induction period Induction period Induction period Induction period Big Rift No membrane period Example 10 Induction period Induction period Induction period Induction period Cracking period No membrane period Embodiment 11 Induction period Induction period Cracking period Fragmentation No membrane period No membrane period Comparative Example 1 Induction period Induction period Induction period Induction period Big Rift No membrane period Comparative Example 2 Induction period Induction period Induction period Induction period Big Rift Fragmentation Comparative Example 3 Induction period Cracking period Fragmentation Big Rift No membrane period No membrane period Comparative Example 4 Induction period Cracking period Fragmentation Big Rift No membrane period No membrane period Comparative Example 5 Induction period Induction period Cracking period Fragmentation No membrane period No membrane period Comparative Example 6 Induction period Induction period Cracking period Fragmentation No membrane period No membrane period Comparative Example 7 Induction period Induction period Induction period Induction period Cracking period Big Rift Comparative Example 8 Induction period Cracking period Fragmentation No membrane period No membrane period No membrane period Comparative Example 9 Induction period Cracking period Fragmentation No membrane period No membrane period No membrane period Comparative Example 10 Induction period Induction period Induction period Induction period Big Rift No membrane period Comparative Example 11 Induction period Induction period Induction period Induction period Cracking period Fragmentation Comparative Example 12 Induction period Induction period Induction period Induction period Big Rift No membrane period Comparative Example 13 Induction period Induction period Induction period Induction period Big Rift No membrane period Comparative Example 14 Induction period Induction period Induction period Induction period Big Rift No membrane period Firstly, it can be concluded from Tables 1 and 2 Examples 1-11 that the low-carbon high-barrier biodegradable mulch film of the present invention has excellent mechanical properties, water vapor and oxygen barrier properties, and rapid degradation ability.
[0115] Second, it can be observed from Example 1 and Comparative Examples 1-8 that the low-carbon and high-barrier biodegradable mulch film of the present invention is blended and modified with PBAT, PLA, and PPCP, which has the effect of complementary advantages and has excellent mechanical properties, water vapor and oxygen barrier properties and degradable properties; UV absorbers, light stabilizers, antioxidants, anti-hydrolysis agents, modified barrier fillers, etc. have a synergistic inhibitory effect on the degradation of the mulch film, which can ensure that the mulch film has excellent performance during its service life; the degradation accelerator can make the material degrade quickly after the expiration of its service life, reduce labor costs, and have low-carbon properties; It can be observed from Example 1 and comparative examples 8-14 that in the low-carbon high-barrier biodegradable mulch film of the present invention, the homemade modified barrier filler has excellent barrier effects on both water vapor and oxygen; at the same time, it can be found that the modified filler has better compatibility, excellent chain extension effect and antibacterial properties.
[0116] In summary, the low-carbon and high-barrier biodegradable mulch provided by the present invention, on the one hand, has a self-made modified barrier filler through molecular design; on the other hand, through the formulation, it has excellent comprehensive properties such as mechanical properties and barrier properties.
[0117] The test method is as follows: (1) Mechanical properties: Tested according to the method described in GB / T 1040.3-2006.
[0118] (2) Water vapor permeability: tested in accordance with the method described in GB / T 1037-2021; the average thickness of the film to be tested is 50 μm.
[0119] (3) Oxygen permeability: The test was conducted in accordance with the method described in GB / T 1038.1-2022. The test conditions were 1 atm and the average thickness of the film to be tested was 50 μm.
[0120] (4) Antibacterial rate: The test was conducted according to the method described in ASTM E2180-07 (2012). Test bacteria: Staphylococcus aureus.
[0121] (5) Degradation: According to the experimental design, the degradation of the ground film was observed and recorded at 40d, 80d, 110d, 130d, 145d, and 160d after laying. The degradation of the ground film was monitored and recorded according to the levels of induction period, cracking period, large crack period, fragmentation period, and film-free period to observe the degradation of the covering film.
[0122] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing a modified barrier filler, characterized in that: The following steps are involved: S11, placing the barrier filler and the silane coupling agent containing a carbon-carbon double bond in an alcohol solvent for silylation coupling reaction to obtain an intermediate product I; S12, subjecting lactic acid to a ring-opening reaction with an epoxide to obtain an intermediate product II; S13, subjecting the intermediate product II to a nucleophilic substitution reaction with a perfluoroacyl chloride to obtain an intermediate product III; S14, free radical polymerization of the intermediate product I, the intermediate product III, aromatic acrylate, aliphatic epoxy olefins, ethylene carbonate, and unsaturated quaternary ammonium salt to obtain a target product, i.e., a modified barrier filler.
2. The preparation method according to claim 1, characterized in that: The usage ratio of the barrier filler, the silane containing a carbon-carbon double bond and the alcohol solvent is 1 g: 0.8-1.5 g: 80 mL; and The barrier filler is a lamellar structure.
3. The preparation method according to claim 1, characterized in that: The lactic acid and epoxy olefins are added in a molar ratio of carboxyl to epoxy of 1:
1.
4. The preparation method according to claim 1, characterized in that: The intermediate product II and the perfluoroacyl chloride are added at a molar ratio of hydroxyl group to acyl chloride of 1:1; and The carbon atom of the perfluoroacyl chloride is C5-C8.
5. The preparation method according to claim 1, characterized in that: The intermediate product I, intermediate product III, aromatic acrylate, aliphatic epoxy olefins, ethylene carbonate and unsaturated quaternary ammonium salt are added in a molar ratio of carbon-carbon double bonds of 0.15-0.25: 0.05-0.15: 0.15-0.25: 0.2-0.3: 0.1-0.2: 0.05-0.
15.
6. A modified barrier filler, characterized in that: The modified barrier filler is prepared by the preparation method according to any one of claims 1 to 5.
7. A low-carbon high-barrier biodegradable mulch film, characterized in that: The invention comprises the following raw materials in parts by weight: PPCP 15-25 parts; PLA 5-25 parts; PBAT 50-80 parts; 3.0-5.0 parts of modified barrier filler; UV absorber 0.5-1.0 part; Light stabilizer 0.2-0.5 parts; Antioxidant 0.2-0.5 parts; Anti-hydrolysis agent 0.3-0.8 parts; Plasticizer 2.0-4.0 parts; 2.0-3.0 parts of heat stabilizer; Lubricant 0.2-0.5 parts; Degradation accelerator 0.1-0.2 parts; Among them, the total mass of PPCP, PLA and PBAT is 100 parts.
8. The low-carbon high-barrier biodegradable mulch film according to claim 7, characterized in that: The degradation accelerator is iron stearate.
9. A method for preparing a low-carbon high-barrier biodegradable mulch film, characterized in that: The steps include: S21, mixing, i.e. Place all raw materials in a mixer according to the formula and mix them evenly; S22, granulation, i.e. Put into the granulation unit, extrude and pelletize at 160-200℃; and S23, blown film, i.e. The pellets are put into a film blowing machine for film blowing and winding to obtain a low-carbon and high-barrier biodegradable mulch film.
Citation Information
Patent Citations
High-barrier full-biodegrade mulching film and preparation method thereof
CN106221165A
Biodegradable polylactic acid film and preparation method thereof
CN112210197A
Silicone rubber composite material with water vapor barrier function and preparation method thereof
CN113462161A
Bio-based full-degradable thin-wall injection molding material and preparation method thereof
CN114790325A
Hydrolysis-resistant high-barrier biodegradable film and preparation method thereof
CN115260711A
Cited By
PLA-based heat shrink film
CN118955784A