Flame-retardant polyolefin cable insulating material and preparation method thereof

By surface modification of magnesium hydroxide and adding composite modified boron nitride nanosheets and modified nanocellulose to the polymer matrix to form a composite system, the thermal stability and mechanics of polyolefin cable insulation materials are solved. The performance deficiencies have achieved a comprehensive improvement in flame retardant, thermal conductivity and mechanical properties.

CN118978756AInactive Publication Date: 2024-11-19GUANGZHOU ZHUJIANG CABLE CO LTD
View PDF 0 Cites 13 Cited by

Patent Information

Application Number
CN202411134458.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing polyolefin cable insulating materials have shortcomings in thermal stability and mechanical properties, especially the toughness and elongation of break of polypropylene materials are weak, making it difficult to meet the comprehensive performance requirements of cable applications.

Method used

Magnesium hydroxide is used as flame retardant filler and surface modified, combined with composite modified boron nitride nanosheets and modified nanocellulose, to form a composite system with flame retardant, thermal conductivity and mechanical enhancement effects, to improve Comprehensive properties of polyolefin cable insulation materials.

Benefits of technology

The flame retardant, thermal conductivity and mechanical properties of polyolefin cable insulation materials are significantly improved, and their stability and flame resistance at high temperatures are enhanced, and their service life is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978756A_ABST
    Figure CN118978756A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of cable insulating materials, and provides a flame-retardant polyolefin cable insulating material and a preparation method thereof. Comprising the following steps: putting low-density polyethylene, polypropylene, ethylene-vinyl acetate, grafted modified magnesium hydroxide powder, composite modified boron nitride nanosheets, modified nanocellulose, a lubricant, an antioxidant and a plasticizer into a mixing device, and stirring to obtain a mixed master batch; and carrying out melt extrusion by a screw extruder and then carrying out cooling molding so as to obtain the flame-retardant polyolefin cable insulation material. The graft modified magnesium hydroxide powder, the composite modified boron nitride nanosheets and the modified nanocellulose are doped into a polymer matrix to form a compound system with flame retardance, heat conduction and mechanical enhancement effects, and the flame-retardant polyolefin cable insulating material with excellent comprehensive performance is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cable insulation materials and relates to a flame retardant polyolefin cable insulation material and a preparation method thereof. Background Art

[0002] Due to changes in the power system and the increase in daily life needs, basic power facilities have become more important, which also requires that the cable insulation materials used in power facilities have excellent performance in terms of safe power capacity, stable power output, safety of use, service life, etc. Among them, polyolefin materials have become one of the commonly used materials due to their excellent electrical and mechanical properties.

[0003] Polyethylene material is the most commonly used polyolefin material, but with the expansion of its scope of use, the required properties are also gradually increasing, such as thermal stability. However, polyethylene material has natural defects in thermal stability, which has also made polypropylene material quickly become a substitute for insulation materials. However, polypropylene material has the disadvantages of weak toughness and elongation at break, and the mechanical properties of polymer materials are one of the feasibility of cable applications. Therefore, how to make up for the shortcomings and prepare polyolefin cable insulation materials with excellent mechanical properties, flame retardant properties and thermal conductivity is a technical problem that needs to be solved urgently. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a flame-retardant polyolefin cable insulation material and a preparation method thereof. The present invention uses magnesium hydroxide as a flame-retardant filler and performs surface modification on the magnesium hydroxide, thereby improving the interface compatibility between the magnesium hydroxide and the polymer matrix; in addition, the present invention incorporates composite modified boron nitride nanosheets and modified nanocellulose into the polymer matrix to form a composite system with flame retardancy, thermal conductivity and mechanical reinforcement, thereby preparing a flame-retardant polyolefin cable insulation material with excellent comprehensive performance.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a flame retardant polyolefin cable insulation material, the preparation method comprising:

[0007] Magnesium hydroxide is sequentially modified by sodium oleate and methyl methacrylate grafting to obtain grafted modified magnesium hydroxide powder; boron nitride nanosheets are sequentially modified by hydroxylation, hexadecyltrimethylammonium bromide and silane coupling agent to obtain composite modified boron nitride nanosheets; nanocellulose is modified by dopamine coating to obtain modified nanocellulose;

[0008] Low-density polyethylene, polypropylene, ethylene-vinyl acetate, the grafted modified magnesium hydroxide powder, the composite modified boron nitride nanosheets, the modified nanocellulose, a lubricant, an antioxidant and a plasticizer are put into a mixing device for stirring to obtain a mixed masterbatch; the mixed masterbatch is fed into a feeding port of a screw extruder, melt-extruded by the screw extruder, and then cooled and formed to obtain the flame-retardant polyolefin cable insulation material.

[0009] As a preferred technical solution of the present invention, the preparation method specifically comprises the following steps:

[0010] (I) dispersing magnesium hydroxide in an ethanol aqueous solution, ultrasonically dispersing to obtain a magnesium hydroxide dispersion, adding sodium oleate to the magnesium hydroxide dispersion, ultrasonically dispersing to obtain a modified magnesium hydroxide dispersion, filtering, washing, drying, grinding and sieving the modified magnesium hydroxide dispersion to obtain a modified magnesium hydroxide powder; dispersing the modified magnesium hydroxide powder and methyl methacrylate monomer in an ethanol solution of polyvinyl pyrrolidone, mixing to obtain a precursor solution, adding ammonium persulfate to the precursor solution under a nitrogen atmosphere and stirring and heating conditions to perform a reflux reaction, and after the reaction is completed, filtering, washing and drying the reaction product to obtain a grafted modified magnesium hydroxide powder;

[0011] (II) mixing sodium dodecyl sulfate, fatty acid ethanolamide, ethoxylated sodium sulfonate and deionized water to obtain a boron nitride stripping solution; adding boron nitride powder to the boron nitride stripping solution, ultrasonically dispersing and heating to strip the boron nitride powder to form a boron nitride dispersion, centrifuging, washing and drying the boron nitride dispersion to obtain boron nitride nanosheets; mixing the boron nitride nanosheets with sodium hydroxide solution, stirring and ultrasonically dispersing to obtain a mixed solution, transferring the mixed solution to a reactor for hydrothermal reaction, and after the reaction is completed, filtering, washing and drying the reaction product to obtain hydroxyl-modified boron nitride nanosheets;

[0012] (III) uniformly mixing the hydroxyl-modified boron nitride nanosheets obtained in step (II), zinc nitrate hexahydrate and deionized water to obtain a precursor solution, adding potassium hydroxide solution to the precursor solution, stirring uniformly to react and generate flocculent precipitates, obtaining a reaction mixture after the reaction is completed, adding hexadecyltrimethylammonium bromide to the reaction mixture, mixing uniformly and transferring to a reactor for hydrothermal reaction, filtering, washing and drying after the reaction to obtain composite boron nitride nanosheets loaded with zinc oxide; soaking the composite boron nitride nanosheets in a silane coupling agent solution, taking out the composite boron nitride nanosheets after soaking, washing and drying to obtain composite modified boron nitride nanosheets;

[0013] (IV) dissolving dopamine in a Tris-hydrochloric acid buffer solution to obtain a dopamine solution, soaking the nanocellulose powder in the dopamine solution so that dopamine self-polymerizes in situ on the surface of the nanocellulose powder to form polydopamine, and after the soaking, filtering, washing and freeze-drying to obtain modified nanocellulose;

[0014] (V) low-density polyethylene, polypropylene, ethylene-vinyl acetate, the grafted modified magnesium hydroxide powder obtained in step (I), the composite modified boron nitride nanosheets obtained in step (III), the modified nanocellulose obtained in step (IV), a lubricant, an antioxidant and a plasticizer are put into a mixing device for stirring to obtain a mixed masterbatch; the mixed masterbatch is fed into the feed port of a screw extruder, and the barrel of the screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction; after being melt-extruded by the screw extruder, the mixed masterbatch is cooled and formed to obtain the flame-retardant polyolefin cable insulation material.

[0015] The present invention adopts magnesium hydroxide as a flame retardant filler. Magnesium hydroxide has a high thermal decomposition temperature and needs to absorb a large amount of heat during the heating process, which can reduce the combustion temperature of the surface of the polyolefin cable insulation material. In addition, magnesium hydroxide will release a large amount of water when it is thermally decomposed. On the one hand, it can dilute the air on the surface of the polyolefin cable insulation material, so that the combustion speed of the polyolefin cable insulation material is slowed down. On the other hand, water vapor can also dilute the smoke and play a role in smoke elimination. At the same time, magnesium hydroxide is thermally decomposed to generate magnesium oxide. Magnesium oxide itself is a good refractory material, and magnesium oxide has a relatively large specific surface area, which can absorb a large amount of smoke and reduce smoke emissions. In addition, magnesium oxide covering the surface of the polyolefin cable insulation material can also isolate the air and play a heat insulation role, thereby preventing the polyolefin cable insulation material from continuing to burn.

[0016] However, the disadvantage of a single magnesium hydroxide flame retardant filler is that the flame retardant efficiency is low, and a certain amount of addition is required to achieve an ideal flame retardant effect. In addition, magnesium hydroxide has a strong hydrophilicity, while the polymer matrix material of the polyolefin cable insulation material provided by the present invention is hydrophobic. Therefore, magnesium hydroxide has poor compatibility with the polymer matrix and is not easy to disperse in the polymer matrix. The mechanical properties of the prepared polyolefin cable insulation material are poor, which affects the original mechanical properties of the polymer matrix. Therefore, on the one hand, the present invention performs sodium oleate surface modification and methyl methacrylate graft polymerization modification on magnesium hydroxide to improve the physical and chemical properties of its surface, thereby improving the interface compatibility between magnesium hydroxide and the polymer matrix; on the other hand, the present invention incorporates composite modified boron nitride nanosheets and modified nanocellulose into the polymer matrix to form a composite system with flame retardant, thermal conductivity and mechanical enhancement effects, and prepares a flame retardant polyolefin cable insulation material with excellent comprehensive performance by means of the synergistic effect between grafted modified magnesium hydroxide powder, composite modified boron nitride nanosheets and modified nanocellulose.

[0017] The present invention performs surface modification of magnesium hydroxide with sodium oleate and graft modification with methyl methacrylate, which can greatly improve the interface compatibility between magnesium hydroxide and the polymer matrix, thereby facilitating the full play of the flame retardant ability of magnesium hydroxide, and also enhancing the mechanical properties of polyolefin cable insulation materials to a certain extent. The present invention uses sodium oleate to perform surface modification of magnesium hydroxide. During the modification process, sodium oleate is hydrolyzed in an aqueous solution to generate C 17 H 33 COO-, in which the carboxylate is a hydrophilic functional group, C 17 H 33 COO- is adsorbed on the surface of magnesium hydroxide with a stable chemical bond, and the hydrophobic long-chain alkane is exposed on the outside. Therefore, the surface property of the modified magnesium hydroxide powder obtained after modification with sodium oleate can be changed from hydrophilic to hydrophobic, thereby improving the interfacial compatibility between the modified magnesium hydroxide powder and the polymer matrix.

[0018] Subsequently, the present invention uses methyl methacrylate as a polymerization monomer, polyvinyl pyrrolidone as a dispersant, and ammonium persulfate as an initiator, and carries out graft polymerization on the modified magnesium hydroxide powder after the surface modification of sodium oleate under the protection of a nitrogen atmosphere. Since the sodium oleate modification can introduce a carbon-carbon double bond (-C=C-) on the surface of the magnesium hydroxide, under the action of the initiator, the carbon-carbon double bond opens the unsaturated double bond under the action of the initiator ammonium persulfate and undergoes a polymerization reaction with the methyl methacrylate monomer, thereby realizing the grafting of the methyl methacrylate monomer on the magnesium hydroxide. As the graft polymerization reaction continues, the methyl methacrylate monomer initiates a polymerization reaction on the surface of the modified magnesium hydroxide powder to form a polymethyl methacrylate polymer chain with a considerable molecular weight. Since the polarity of polymethyl methacrylate is lower than that of sodium oleate, the hydrophobicity of the grafted modified magnesium hydroxide powder obtained after the graft polymerization modification is further improved, thereby further improving the interface compatibility between the grafted modified magnesium hydroxide powder and the polymer matrix.

[0019] Boron nitride itself has the advantages of high thermal conductivity, electrical insulation and thermal stability, and is often used as a thermal conductive and insulating filler. However, due to its high surface energy, boron nitride has poor dispersion in the polymer matrix and is easy to agglomerate. Therefore, it is necessary to modify boron nitride to further improve its dispersion stability in the polymer matrix while ensuring its own thermal conductivity. To this end, the present invention firstly carries out ultrasonic stripping of boron nitride powder in a boron nitride stripping solution to obtain boron nitride nanosheets; then, the boron nitride nanosheets are subjected to hydroxyl modification treatment by sodium hydroxide, so as to effectively alleviate the agglomeration phenomenon of the boron nitride nanosheets in a polymer matrix; then, sheet-like nano zinc oxide is in situ generated on the surface of the boron nitride nanosheets by a liquid phase precipitation method, so as to obtain composite boron nitride nanosheets loaded with zinc oxide; a stable, effective and continuous heat conduction path is formed by the composite of the boron nitride nanosheets and zinc oxide, so as to improve the thermal conductivity of the polyolefin cable insulation material; finally, the interface compatibility between the composite boron nitride nanosheets and the polymer matrix is ​​improved by surface treatment with a silane coupling agent, so as to obtain composite boron nitride nanosheets with both dispersion stability and interface compatibility.

[0020] The present invention uses sodium hydroxide to perform hydroxylation modification on boron nitride nanosheets. On the one hand, a large amount of -NH2 and B-OH can be formed at the edges of the boron nitride nanosheets. The hydrophilicity and hydration of these functional groups reduce the surface energy of the boron nitride nanosheets, making it difficult for the boron nitride nanosheets to agglomerate in the polymer matrix, thereby improving the dispersion stability of the boron nitride nanosheets in the polymer matrix. On the other hand, the modification treatment with sodium hydroxide also helps to peel off the boron nitride sheets, thereby reducing the thickness and lateral size of the boron nitride nanosheets. + Adsorption on the outer surface of BN nanosheets causes the edges of the sheets to curl, thus promoting OH- Penetrate into the boron nitride sheet, further causing the sheet to curl, and between the boron nitride nanosheet and OH - The adsorption and reaction between them lead to the complete exfoliation of the layers of boron nitride nanosheets.

[0021] The present invention loads zinc oxide on hydroxyl-modified boron nitride nanosheets, which can not only greatly improve the thermal conductivity of the polyolefin cable insulation material, but also further improve the flame retardant properties of the polyolefin cable insulation material, and at the same time, it is also helpful to improve the mechanical properties of the polyolefin cable insulation material. This is because, on the one hand, the improvement of thermal conductivity mainly depends on the interfacial thermal resistance between boron nitride nanosheets and the polymer matrix, which will have an adverse effect on the thermal conductivity of polyolefin cable insulation materials. After zinc oxide is loaded in boron nitride nanosheets, a thermal conductivity gradient can be formed between the boron nitride nanosheets and the polymer matrix, which alleviates the thermal conductivity mismatch between the polymer matrix and the boron nitride nanosheets, and is conducive to reducing the interfacial thermal resistance between the boron nitride nanosheets and the polymer matrix; at the same time, the flaky nano zinc oxide has a large aspect ratio, which can play a "bridge" role between the boron nitride nanosheets to promote phonon transfer, so that the composite modified boron nitride nanosheets form an effective and continuous thermal conduction path in the polymer matrix, and at the same time can inhibit the agglomeration of boron nitride nanosheets, so that the composite modified boron nitride nanosheets are uniformly dispersed in the polymer matrix, thereby effectively reducing phonon scattering and interfacial thermal resistance. Therefore, the synergistic effect produced by the composite of boron nitride nanosheets and zinc oxide can effectively improve the thermal conductivity of polyolefin cable insulation materials. On the other hand, the introduction of zinc oxide can greatly increase the amount of carbon residue after combustion of polyolefin cable insulation materials, and can generate more carbon layers during combustion to isolate heat and combustible gases, thereby significantly improving the flame retardant properties of polyolefin cable insulation materials. On the other hand, the tensile strength of polyolefin cable insulation materials will decrease with the increase of the addition amount of boron nitride nanosheets. This is because boron nitride nanosheets are prone to agglomeration in the polymer matrix, resulting in an increase in defects in the polymer matrix and a decrease in tensile strength. However, the addition of zinc oxide can bridge the surrounding polymer matrix into a force-bearing whole. The uniform dispersion of zinc oxide in the polymer matrix can quickly and evenly transmit stress and absorb energy, thereby effectively improving the mechanical properties of polyolefin cable insulation materials.

[0022] The present invention uses zinc nitrate and potassium hydroxide as raw materials, and generates sheet-like nano zinc oxide in situ on the surface of boron nitride nanosheets by liquid phase precipitation. The reaction principle is as follows:

[0023] Zn 2+ +2OH - →Zn(OH)2

[0024] Zn(OH)2→Zn(OH)4 2-

[0025] Zn(OH)4 2- →ZnO+H2O+2OH -

[0026] The formation process of flaky nano zinc oxide goes through four stages: dissolution-hydrolysis-nucleation-growth. Specifically, the zinc nitrate aqueous solution is mixed with the potassium hydroxide aqueous solution to form a white flocculent precipitate Zn(OH)2 precursor; during the hydrothermal reaction, the Zn(OH)2 precursors adhere to each other to form irregular ion aggregates. When the solution reaches supersaturation, these ion aggregates reach the critical nucleation concentration under hydrothermal conditions, and the Zn(OH)2 ion aggregates are rapidly hydrolyzed to form growth units Zn(OH)4 2- , along with Zn(OH)4 2- Adsorption, decomposition and desorption occur on the growth interface, making Zn(OH)4 2- Zinc oxide crystal nuclei are formed through oxygen bridge bonding and protonation reaction of anionic functional groups. The zinc oxide crystal nuclei regularly attach to each other, agglomerate and grow gradually. As the reaction continues, the ion concentration in the reaction system decreases, promoting the continued hydrolysis of Zn(OH)2 precursor to form Zn(OH)42-, providing more growth units for the growth of zinc oxide crystal nuclei.

[0027] Cellulose is the most abundant natural polymer in nature and is widely found in plants, algae and other organisms. Unlike traditional polymers, the one-dimensional structure of nanocellulose not only does not cover the grafted modified magnesium hydroxide powder and the composite modified boron nitride nanosheets, but also serves as the skeleton structure of the thermal conductivity path, so that the grafted modified magnesium hydroxide powder and the composite modified boron nitride nanosheets are evenly arranged along the nanocellulose for better contact, thereby forming a stable and continuous thermal conductivity path. In addition, the abundant hydroxyl groups and other polar functional groups on the surface of nanocellulose are easy to form a strong interface bonding effect with the grafted modified magnesium hydroxide powder and the composite modified boron nitride nanosheets, which helps to disperse the grafted modified magnesium hydroxide powder and the composite modified boron nitride nanosheets in the polymer matrix, thereby reducing the interfacial thermal resistance between the filler and the polymer matrix.

[0028] However, since nanocellulose has a very large specific surface area and is rich in hydroxyl groups, it is easy for the nanocellulose to agglomerate through hydrogen bonding during the melt extrusion process. Therefore, the present invention coats the nanocellulose with polydopamine through the oxidative self-polymerization of dopamine, thereby improving the dispersion stability of the nanocellulose in the polymer matrix.

[0029] Dopamine is an organic substance containing multiple functional groups, such as amino, hydroxyl and other groups. In a weakly alkaline environment, it will automatically polymerize into a long-chain polymer, namely polydopamine. Polydopamine has a strong adhesion ability, and the amino, hydroxyl and other groups it contains can form a stable covalent bond with nanocellulose. The present invention can effectively improve the mechanical properties of polyolefin cable insulation materials by incorporating modified nanocellulose into the polymer matrix, which is mainly due to the uniform dispersion of modified nanocellulose in the polymer matrix and the multiple physical crosslinking between the polymer macromolecular chain and the modified nanocellulose. The hydrogen bond interaction within the nanocellulose molecule is destroyed by the polydopamine coating modification treatment, the intermolecular hydrogen bond interaction between the nanocellulose and the polymer matrix is ​​reconstructed, and the formation of a physical crosslinking network is further promoted by the entanglement of the molecular chains between the nanocellulose and the polymer matrix. By constructing an interface area with strong multiple hydrogen bond interactions, energy can be effectively consumed, crack propagation of the polymer matrix during the stretching process is prevented, and the failure of the polymer matrix during the stretching process is delayed, thereby significantly improving the mechanical properties of the polyolefin cable insulation material.

[0030] The modified nanocellulose and the composite modified boron nitride nanosheets produce a synergistic effect, which is specifically reflected in:

[0031] (1) The addition of modified nanocellulose can significantly improve the dispersibility of the composite modified boron nitride nanosheets in the polymer matrix. This is because nanocellulose contains a large number of hydroxyl functional groups. The edges of the hydroxyl-modified boron nitride nanosheets obtained after ultrasonic stripping and hydroxylation treatment contain a large number of -OH and -NH2. The hydroxyl functional groups on nanocellulose can form strong hydrogen bonds with -NH2 and B-OH on the boron nitride nanosheets and tightly bind. At the same time, the CH bonds on the nanocellulose molecular chain and the BN hexacyclic rings in the boron nitride nanosheets are typical hydrophobic sites, and the two tend to bind together through hydrophobic-hydrophobic interactions. Since electrostatic repulsion occurs between nanocellulose and nanocellulose, and nanocellulose and boron nitride nanosheets can be tightly bound through hydrophobic-hydrophobic interaction and hydrogen bond interaction, electrostatic repulsion also occurs between composite fillers composed of nanocellulose and boron nitride nanosheets. At the same time, there is steric hindrance between the one-dimensional nanocellulose and the two-dimensional boron nitride nanosheets. Under the electrostatic repulsion and steric hindrance, the boron nitride nanosheets can remain stably dispersed in the polymer matrix.

[0032] (2) The addition of modified nanocellulose can significantly improve the thermal conductivity of polyolefin cable insulation materials. This is because the surface of boron nitride nanosheets is modified by surface hydroxylation with sodium hydroxide, and hydroxyl functional groups are modified on the surface of boron nitride nanosheets, which not only improves the dispersion stability of boron nitride nanosheets in the polymer matrix, but also enhances the interfacial compatibility between boron nitride nanosheets and modified nanocellulose, which is beneficial to reduce the interfacial thermal resistance between the composite modified boron nitride nanosheets and the modified nanocellulose and the polymer matrix; in addition, during the melt extrusion process, the composite modified boron nitride nanosheets can be uniformly dispersed in the modified nanocellulose along the planar direction, and the shearing action of the screw can significantly reduce the gap between the modified nanocellulose and the polymer matrix, so that the modified nanocellulose forms a more uniform and dense three-dimensional network structure, which helps the composite modified boron nitride nanosheets to form a continuous and stable heat conduction path, which helps the efficient transmission of phonons along the planar direction, significantly improving the thermal conductivity of polyolefin cable insulation materials.

[0033] There is also a synergistic effect between modified nanocellulose and grafted modified magnesium hydroxide powder, which is specifically reflected in:

[0034] (1) The addition of modified nanocellulose can significantly improve the dispersibility of the grafted modified magnesium hydroxide powder in the polymer matrix. This is because the surface of magnesium hydroxide is highly polarized and has a large specific surface area, and has a tendency to self-accumulate, which leads to the aggregation of magnesium hydroxide powder in the polymer matrix; at the same time, since the surface of magnesium hydroxide carries a positive charge and is hydrophilic, but has poor lipophilicity, the interfacial compatibility with the polymer is poor. After adding modified nanocellulose to the present invention, the grafted modified magnesium hydroxide powder can interact with the hydrophilic hydroxyl groups on the surface of the modified nanocellulose, so that the grafted modified magnesium hydroxide powder can be better dispersed in the polymer matrix.

[0035] (2) The addition of modified nanocellulose can significantly improve the flame retardant properties of polyolefin cable insulation materials. Although nanocellulose has no flame retardant function, the presence of modified nanocellulose can improve the dispersibility of grafted modified magnesium hydroxide powder in the polymer matrix, making it evenly dispersed in the polymer matrix, which helps the grafted modified magnesium hydroxide powder to better exert its flame retardant properties. At the same time, the addition of modified nanocellulose can significantly improve the adhesion and density of the carbon layer, reduce the overflow of combustible substances generated during the combustion of polyolefin cable insulation materials, inhibit heat release behavior, significantly increase the limiting oxygen index of polyolefin cable insulation materials, and effectively inhibit the vertical combustion behavior of polyolefin cable insulation materials. In addition, adding modified nanocellulose can also effectively prevent the flame explosion phenomenon of polyolefin cable insulation materials. This is because the water vapor generated inside the agglomerated magnesium hydroxide powder during thermal decomposition cannot be quickly discharged, thus forming a positive pressure that causes the magnesium hydroxide agglomerates to burst, and then the flame explosion phenomenon occurs. The addition of modified nanocellulose can effectively improve the dispersibility of the grafted modified magnesium hydroxide powder, so that the water vapor generated by the thermal decomposition of the magnesium hydroxide powder can be discharged in time.

[0036] As a preferred technical solution of the present invention, in step (I), the volume ratio of ethanol to deionized water in the ethanol aqueous solution is (8-9):(1-2), for example, it can be 8:2, 8.1:1.9, 8.2:1.8, 8.3:1.7, 8.4:1.6, 8.5:1.5, 8.6:1.4, 8.7:1.3, 8.8:1.2, 8.9:1.1 or 9:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] In some optional examples, the power of ultrasonic dispersion after dispersing the magnesium hydroxide in the ethanol aqueous solution is 700-800 W, for example, it can be 700 W, 710 W, 720 W, 730 W, 740 W, 750 W, 760 W, 770 W, 780 W, 790 W or 800 W; the time of ultrasonic dispersion is 10-20 min, for example, it can be 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min or 20 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] In some optional examples, the concentration of magnesium hydroxide in the magnesium hydroxide dispersion is 0.2 to 0.3 g / mL, for example, 0.2 g / mL, 0.21 g / mL, 0.22 g / mL, 0.23 g / mL, 0.24 g / mL, 0.25 g / mL, 0.26 g / mL, 0.27 g / mL, 0.28 g / mL, 0.29 g / mL or 0.3 g / mL, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0039] In some optional examples, the mass ratio of the magnesium hydroxide to the sodium oleate in the magnesium hydroxide dispersion is 1:(0.1-0.2), for example, it can be 1:0.1, 1:0.11, 1:0.12, 1:0.13, 1:0.14, 1:0.15, 1:0.16, 1:0.17, 1:0.18, 1:0.19 or 1:0.2, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] The present invention particularly limits the mass ratio of magnesium hydroxide and sodium oleate in the magnesium hydroxide dispersion to 1: (0.1-0.2). With the increase of the amount of sodium oleate, the hydrophobicity of magnesium hydroxide gradually increases. When the amount of sodium oleate reaches 1: 0.2, the water contact angle of the modified magnesium hydroxide powder reaches the maximum value. At this time, the hydrophobicity of the modified magnesium hydroxide powder reaches the maximum. If the amount of sodium oleate is further increased, the water contact angle of the modified magnesium hydroxide powder does not increase significantly. In addition, excessive sodium oleate will also affect the subsequent graft polymerization reaction of methyl methacrylate monomer. Since the reactants need to be continuously stirred and heated during the graft polymerization process, when the amount of sodium oleate exceeds the upper limit of the range defined by the present invention, sodium oleate will form multilayer adsorption on the surface of magnesium hydroxide, which will cause part of the sodium oleate adsorbed on the surface of magnesium hydroxide to desorb during the stirring process, so that the surface of magnesium hydroxide does not have enough oleate groups, and the methyl methacrylate monomer cannot be grafted and polymerized to the surface of magnesium hydroxide with the help of oleate groups, so that the grafting effect of methyl methacrylate is poor.

[0041] In some optional examples, the power of ultrasonic dispersion after adding sodium oleate to the magnesium hydroxide dispersion is 900-1000 W, for example, it can be 900 W, 910 W, 920 W, 930 W, 940 W, 950 W, 960 W, 970 W, 980 W, 990 W or 1000 W; the time of ultrasonic dispersion is 30-40 min, for example, it can be 30 min, 31 min, 32 min, 33 min, 34 min, 35 min, 36 min, 37 min, 38 min, 39 min or 40 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] In some optional examples, the mesh size of the sieve is 200-300 mesh, for example, it can be 200 mesh, 210 mesh, 220 mesh, 230 mesh, 240 mesh, 250 mesh, 260 mesh, 270 mesh, 280 mesh, 290 mesh or 300 mesh, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] In some optional examples, the mass fraction of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 8 to 10 wt%, for example, it can be 8.0 wt%, 8.2 wt%, 8.4 wt%, 8.6 wt%, 8.8 wt%, 9.0 wt%, 9.2 wt%, 9.4 wt%, 9.6 wt%, 9.8 wt% or 10.0 wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] In some optional examples, the mass ratio of the modified magnesium hydroxide powder to the polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 1:(0.04-0.05), for example, it can be 1:0.04, 1:0.041, 1:0.042, 1:0.043, 1:0.044, 1:0.045, 1:0.046, 1:0.047, 1:0.048, 1:0.049 or 1:0.05, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] In some optional examples, the mass ratio of the modified magnesium hydroxide powder to the methyl methacrylate monomer is 1:(0.4-0.5), for example, it can be 1:0.4, 1:0.41, 1:0.42, 1:0.43, 1:0.44, 1:0.45, 1:0.46, 1:0.47, 1:0.48, 1:0.49 or 1:0.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] The present invention particularly limits the mass ratio of the modified magnesium hydroxide powder to the methyl methacrylate monomer to 1: (0.4-0.5). When the mass ratio of the modified magnesium hydroxide powder to the methyl methacrylate monomer is within the numerical range defined in the present invention, the hydrophobicity of the obtained modified magnesium hydroxide powder reaches a higher level. If the amount of the methyl methacrylate monomer is further increased, the water contact angle of the modified magnesium hydroxide powder decreases instead, and the hydrophobicity becomes worse. This is because, after sodium oleate modification, the number of grafting polymerization sites provided on the surface of magnesium hydroxide powder is limited. When the methyl methacrylate monomer exceeds the number of grafting polymerization sites, the methyl methacrylate monomer not grafted to the surface of magnesium hydroxide powder will undergo self-polymerization to form free polymethyl methacrylate. As the reaction continues, the free polymethyl methacrylate will remain on the surface of magnesium hydroxide powder in a physically attached manner and gradually agglomerate to form large-sized polymer agglomerates. These polymer agglomerates will not only affect the surface hydrophobicity of the modified magnesium hydroxide powder, but also form defects such as holes and gaps between the grafted modified magnesium hydroxide powder and the polymer matrix, affecting the interfacial bonding strength between the grafted modified magnesium hydroxide powder and the polymer matrix, causing stress concentration at the interface, and ultimately leading to a decrease in the mechanical properties of the polyolefin cable insulation material.

[0047] In some optional examples, the mass ratio of the methyl methacrylate monomer in the precursor solution to the ammonium persulfate is 1:(0.005-0.015), for example, it can be 1:0.005, 1:0.006, 1:0.007, 1:0.008, 1:0.009, 1:0.01, 1:0.011, 1:0.012, 1:0.013, 1:0.014 or 1:0.015, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] In some optional examples, the temperature of the reflux reaction is 70-80°C, for example, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] In some optional examples, the reflux reaction time is 5 to 8 hours, for example, it can be 5.0h, 5.2h, 5.4h, 5.6h, 5.8h, 6.0h, 6.2h, 6.4h, 6.6h, 6.8h, 7.0h, 7.2h, 7.4h, 7.6h, 7.8h or 8.0h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] As a preferred technical solution of the present invention, in step (II), the concentration of sodium dodecyl sulfate in the boron nitride stripping solution is 12 to 15wt%, for example, it can be 12wt%, 12.2wt%, 12.4wt%, 12.6wt%, 12.8wt%, 13wt%, 13.2wt%, 13.4wt%, 13.6wt%, 13.8wt%, 14wt%, 14.2wt%, 14.6wt%, 14.8wt% or 15wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0051] In some optional examples, the concentration of fatty acid ethanolamide in the boron nitride stripping solution is 5 to 8wt%, for example, it can be 5.0wt%, 5.2wt%, 5.4wt%, 5.6wt%, 5.8wt%, 6.0wt%, 6.2wt%, 6.4wt%, 6.6wt%, 6.8wt%, 7.0wt%, 7.2wt%, 7.4wt%, 7.6wt%, 7.8wt% or 8.0wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] In some optional examples, the concentration of sodium ethoxylate sulfonate in the boron nitride stripping solution is 4 to 5wt%, for example, it can be 4.0wt%, 4.1wt%, 4.2wt%, 4.3wt%, 4.4wt%, 4.5wt%, 4.6wt%, 4.7wt%, 4.8wt%, 4.9wt% or 5.0wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] In some optional examples, the ratio of the boron nitride powder to the boron nitride stripping solution is 1g:(30-40)mL, for example, it can be 1g:30mL, 1g:31mL, 1g:32mL, 1g:33mL, 1g:34mL, 1g:35mL, 1g:36mL, 1g:37mL, 1g:38mL, 1g:39mL or 1g:40mL, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] In some optional examples, the power of ultrasonic dispersion after adding boron nitride powder to the boron nitride stripping solution is 1000-1200 W, for example, it can be 1000 W, 1100 W, 1200 W, 1300 W, 1400 W, 1500 W, 1600 W, 1700 W, 1800 W, 1900 W or 2000 W; the time of ultrasonic dispersion is 1-2 h, for example, it can be 1.0 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h, 1.5 h, 1.6 h, 1.7 h, 1.8 h, 1.9 h or 2.0 h, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0055] In some optional examples, the heating temperature after adding boron nitride powder to the boron nitride stripping solution is 30-40°C, for example, it can be 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C or 40°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0056] In some optional examples, the concentration of the sodium hydroxide solution is 3 to 8 mol / L, for example, 3.0 mol / L, 3.5 mol / L, 4.0 mol / L, 4.5 mol / L, 5.0 mol / L, 5.5 mol / L, 6.0 mol / L, 6.5 mol / L, 7.0 mol / L, 7.5 mol / L or 8.0 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] In some optional examples, the mass ratio of the boron nitride nanosheets to the sodium hydroxide in the sodium hydroxide solution is 1:(15-25), for example, it can be 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, 1:21, 1:22, 1:23, 1:24 or 1:25, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0058] In some optional examples, the power of ultrasonic dispersion when the boron nitride nanosheets are mixed with the sodium hydroxide solution is 800-1000 W, for example, it can be 800 W, 820 W, 840 W, 860 W, 880 W, 900 W, 920 W, 940 W, 960 W, 980 W or 1000 W; the time of ultrasonic dispersion is 1-2 h, for example, it can be 1.0 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h, 1.5 h, 1.6 h, 1.7 h, 1.8 h, 1.9 h or 2.0 h, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0059] In some optional examples, the temperature of the hydrothermal reaction is 110-130°C, for example, it can be 110°C, 112°C, 114°C, 116°C, 118°C, 120°C, 122°C, 124°C, 126°C, 128°C or 130°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0060] In some optional examples, the hydrothermal reaction time is 24 to 48 hours, for example, it can be 24h, 26h, 28h, 30h, 32h, 34h, 36h, 38h, 40h, 42h, 44h, 46h or 48h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] As a preferred technical solution of the present invention, in step (III), the concentration of the hydroxyl-modified boron nitride nanosheets in the precursor solution is 10 to 20 g / L, for example, it can be 10 g / L, 11 g / L, 12 g / L, 13 g / L, 14 g / L, 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L or 20 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0062] In some optional examples, the molar concentration of the zinc nitrate hexahydrate in the precursor solution is 1 to 2 mol / L, for example, 1.0 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L or 2.0 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0063] In some optional examples, the molar concentration of the potassium hydroxide solution is 1 to 2 mol / L, for example, it can be 1.0 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L or 2.0 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0064] Zinc oxide generated by potassium hydroxide solutions of different concentrations will show completely different morphologies. In order to improve the thermal conductivity of polyolefin cable insulation materials, it is necessary to generate zinc oxide with a regular shape, flat surface and uniform distribution in a sheet structure to "bridge" the boron nitride nanosheets to form a continuous thermal conductive path. To this end, the present invention specifically limits the molar concentration of the potassium hydroxide solution to 1-2 mol / L. When the molar concentration of the potassium hydroxide solution is lower than 1 mol / L, the zinc oxide nanosheets formed present an irregular lotus petal shape. This is because when there is less OH-, Zn(OH)4 2 -The concentration is low, the coordination on the (0001) crystal plane is incomplete, and the reaction speed of each position of the reaction crystal plane is inconsistent, so it is impossible to obtain a sheet structure with a regular shape. When the molar concentration of the potassium hydroxide solution is in the range of 1 to 2 mol / L, the (0001) crystal plane is completely coordinated, and the reaction speed of the crystal plane is very low, so the (1120) and (1010) crystal planes grow rapidly, thereby obtaining a crystalline product with a sheet structure. When the molar concentration of the potassium hydroxide solution continues to increase to more than 2 mol / L, since the sheet layer of the nano zinc oxide is thin, it is easy to gather together to form spherical agglomerates, which is not conducive to the "bridging" effect on the boron nitride nanosheets; in addition, with the increase of the molar concentration of the potassium hydroxide solution, the sheet structure of the nano zinc oxide no longer continues to increase, but the thickness of the sheet structure will become thinner, so the nano zinc oxide crystal will be softer, and its edge will curl, which is more unfavorable for the establishment of a heat conduction path.

[0065] In some optional examples, the molar ratio of potassium hydroxide in the potassium hydroxide solution to zinc nitrate hexahydrate in the precursor solution is 2:1.

[0066] In some optional examples, the reaction time of the precursor solution and the potassium hydroxide solution is 3 to 4 hours, for example, it can be 3.0 hours, 3.1 hours, 3.2 hours, 3.3 hours, 3.4 hours, 3.5 hours, 3.6 hours, 3.7 hours, 3.8 hours, 3.9 hours or 4.0 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0067] In some optional examples, the mass ratio of the hexadecyltrimethylammonium bromide to the zinc nitrate hexahydrate is 1:(8-9), for example, 1:8.0, 1:8.1, 1:8.2, 1:8.3, 1:8.4, 1:8.5, 1:8.6, 1:8.7, 1:8.8, 1:8.9 or 1:9.0, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0068] In some optional examples, the heating temperature of the hydrothermal reaction is 120-130°C, for example, it can be 120°C, 121°C, 122°C, 123°C, 124°C, 125°C, 126°C, 127°C, 128°C, 129°C or 130°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0069] In order to obtain zinc oxide with a regular shape, a flat surface and uniform distribution of a flaky structure, the present invention specifically limits the heating temperature of the hydrothermal reaction to 120-130°C. When the hydrothermal temperature is lower than 120°C, no flaky structure is generated. This is because the hydrothermal temperature is low, and the power for crystal nucleation and crystal growth is insufficient, so a flocculent structure is formed. As the hydrothermal temperature increases, the energy of the hydrothermal system increases, and the driving force for nucleation and grain growth increases, which is beneficial to promote the growth of zinc oxide grains. At the same time, the atomic arrangement is more orderly and the degree of crystallization is better. When the hydrothermal temperature exceeds 130°C, agglomeration occurs between zinc oxide crystals, and the agglomerated crystals disperse to form nuclei, that is, secondary nucleation, which reduces the size of zinc oxide grains and is not conducive to the formation of a continuous heat conduction path.

[0070] In some optional examples, the insulation time of the hydrothermal reaction is 1 to 3 hours, for example, it can be 1.0h, 1.2h, 1.4h, 1.6h, 1.8h, 2.0h, 2.2h, 2.4h, 2.6h, 2.8h or 3.0h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0071] In some optional examples, the silane coupling agent solution is composed of a silane coupling agent and an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is (8-9):(1-2), for example, it can be 8:2, 8.1:1.9, 8.2:1.8, 8.3:1.7, 8.4:1.6, 8.5:1.5, 8.6:1.4, 8.7:1.3, 8.8:1.2, 8.9:1.1 or 9:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0072] In some optional examples, the mass fraction of the silane coupling agent in the silane coupling agent solution is 5 to 10 wt%, for example, it can be 5.0 wt%, 5.5 wt%, 6.0 wt%, 6.5 wt%, 7.0 wt%, 7.5 wt%, 8.0 wt%, 8.5 wt%, 9.0 wt%, 9.5 wt% or 10.0 wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0073] In some optional examples, the immersion time of the composite boron nitride nanosheets in the silane coupling agent solution is 3 to 5 hours, for example, it can be 3.0 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours, 4.0 hours, 4.2 hours, 4.4 hours, 4.6 hours, 4.8 hours or 5.0 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0074] As a preferred technical solution of the present invention, in step (IV), the concentration of the Tris-hydrochloric acid buffer solution is 30-40 g / L, for example, it can be 30 g / L, 31 g / L, 32 g / L, 33 g / L, 34 g / L, 35 g / L, 36 g / L, 37 g / L, 38 g / L, 39 g / L or 40 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0075] In some optional examples, the concentration of dopamine in the dopamine solution is 1 to 5 g / L, for example, it can be 1.0 g / L, 1.5 g / L, 2.0 g / L, 2.5 g / L, 3.0 g / L, 3.5 g / L, 4.0 g / L, 4.5 g / L or 5.0 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0076] In some optional examples, the mass ratio of the nanocellulose powder to dopamine in the dopamine solution is (4-5):1, for example, it can be 4.0:1, 4.1:1, 4.2:1, 4.3:1, 4.4:1, 4.5:1, 4.6:1, 4.7:1, 4.8:1, 4.9:1 or 5.0:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0077] In some optional examples, the immersion time of the nanocellulose in the dopamine solution is 12 to 24 hours, for example, it can be 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours or 24 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0078] In some optional embodiments, the freeze-drying temperature is -20 to -30°C, for example, it can be -20°C, -21°C, -22°C, -23°C, -24°C, -25°C, -26°C, -27°C, -28°C, -29°C or -30°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0079] In some optional examples, the freeze-drying time is 20 to 30 hours, for example, it can be 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours, 28 hours, 29 hours or 30 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0080] As a preferred technical solution of the present invention, in step (V), the stirring speed is 1200-1500 rpm, for example, it can be 1200 rpm, 1220 rpm, 1240 rpm, 1260 rpm, 1280 rpm, 1300 rpm, 1320 rpm, 1340 rpm, 1360 rpm, 1380 rpm, 1400 rpm, 1420 rpm, 1440 rpm, 1460 rpm, 1480 rpm or 1500 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0081] In some optional examples, the stirring time is 5 to 10 min, for example, it can be 5.0 min, 5.5 min, 6.0 min, 6.5 min, 7.0 min, 7.5 min, 8.0 min, 8.5 min, 9.0 min, 9.5 min or 10.0 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0082] The weight parts of each component in the mixed masterbatch are as follows:

[0083]

[0084] The weight proportion of low-density polyethylene can be 30, 31, 32, 33, 34, 35, 36, 37, 38, 39 or 40 parts; the weight proportion of polypropylene can be 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20 parts; the weight proportion of ethylene-vinyl acetate can be 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20 parts. The weight parts of the grafted modified magnesium hydroxide powder can be 8.0 parts, 8.2 parts, 8.4 parts, 8.6 parts, 8.8 parts, 9.0 parts, 9.2 parts, 9.4 parts, 9.6 parts, 9.8 parts or 10.0 parts; the weight parts of the composite modified boron nitride nanosheets can be 10 parts, 10.2 parts, 10.4 parts, 10.6 parts, 10.8 parts, 11.0 parts, 11.2 parts, 11.4 parts, 11.6 parts, 11.7 parts, 11.8 parts, 11.9 parts, 11.9 parts, 11.1 parts, 11.2 parts, 11.3 parts, 11.4 parts, 11.6 parts, 11.7 parts, 11.8 parts, 11.9 ...1 parts, 11.2 parts, 11.4 parts, 11.6 parts, 11.8 parts, 11.9 parts, 11.8 parts, 11.9 parts, 11. .6 parts, 11.8 parts or 12.0 parts; the weight parts of modified nanocellulose can be 3.0 parts, 3.2 parts, 3.4 parts, 3.6 parts, 3.8 parts, 4.0 parts, 4.2 parts, 4.4 parts, 4.6 parts, 4.8 parts or 5.0 parts; the weight parts of lubricant can be 1.0 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts or 2.0 parts; the weight parts of antioxidant can be 1.0 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts or 2.0 parts; the weight parts of The weight parts of the plasticizer can be 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2.0 parts, but are not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0085] The present invention specifically limits the addition amount of the grafted modified magnesium hydroxide powder to 8 to 10 parts. When the addition amount of the grafted modified magnesium hydroxide powder is within the numerical range defined in the present invention, the grafted modified magnesium hydroxide powder can be dispersed relatively evenly in the polymer matrix, which helps to improve the flame retardant properties and mechanical properties of the polyolefin cable insulation material; however, when the addition amount of the grafted modified magnesium hydroxide powder exceeds 10 parts, the grafted modified magnesium hydroxide powder is prone to agglomeration in the polymer matrix, thereby reducing the flame retardant properties and mechanical properties of the polyolefin cable insulation material. In addition, a small amount of grafted modified magnesium hydroxide powder helps to connect the composite modified boron nitride nanosheets, but when the grafted modified magnesium hydroxide powder exceeds 10 parts, it will have an adverse effect on the connection of the composite modified boron nitride nanosheets, and will block the mutual connection of boron nitride in the radial direction, thereby causing the polyolefin cable insulation material to exhibit a lower radial thermal conductivity.

[0086] The present invention specifically limits the addition amount of the composite modified boron nitride nanosheets to 10 to 12 parts. When the addition amount of the composite modified boron nitride nanosheets is less than 10 parts, the composite modified boron nitride nanosheets cannot be completely connected, so a continuous heat conduction path cannot be formed in the polymer matrix. As the addition amount of the composite modified boron nitride nanosheets increases, the composite modified boron nitride nanosheets are connected to each other and overlapped to form a continuously filled heat conduction network structure in the polymer matrix. However, due to the surface stability of the composite modified boron nitride nanosheets and the weak interaction with the polymer matrix, agglomeration of the composite modified boron nitride nanosheets and interface voids may occur. Therefore, the addition amount of the composite modified boron nitride nanosheets should not exceed 12 parts.

[0087] The present invention specifically limits the addition amount of modified nanocellulose to 3 to 5 parts. Since nanocellulose has a high degree of crystallinity, it is beneficial to phonon transmission and highly ordered arrangement. As the addition amount of modified nanocellulose increases, the thermal conductivity of the polyolefin cable insulation material gradually increases. This is because the hydroxyl groups on the surface of the composite modified boron nitride nanosheets enhance the compatibility between the composite modified boron nitride nanosheets and the modified nanocellulose, thereby reducing the interface thermal resistance and improving the thermal conductivity of the polyolefin cable insulation material. However, when the addition amount of modified nanocellulose exceeds 5 parts, the thermal conductivity of the polyolefin cable insulation material will show a downward trend. This is because, when 3 to 5 parts of modified nanocellulose are added, a good heat conduction path has been formed in the polymer matrix. When more modified nanocellulose is added, more filler-matrix interfaces will be introduced, and defects such as voids and holes are easily generated at the filler-matrix interface, which will cause serious phonon scattering, making the interface thermal resistance between fillers and between fillers and polymer matrices too large, thereby reducing the thermal conductivity of the polyolefin cable insulation material.

[0088] In some optional examples, the temperature of the first zone is 160-170°C, for example, it can be 160°C, 161°C, 162°C, 163°C, 164°C, 165°C, 166°C, 167°C, 168°C, 169°C or 170°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0089] In some optional examples, the temperature of the second zone is 170-180°C, for example, it can be 170°C, 171°C, 172°C, 173°C, 174°C, 175°C, 176°C, 177°C, 178°C, 179°C or 180°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0090] In some optional examples, the temperature of the third zone is 175-185°C, for example, it can be 175°C, 176°C, 177°C, 178°C, 179°C, 180°C, 181°C, 182°C, 183°C, 184°C or 185°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0091] In some optional examples, the temperature of the fourth zone is 185-195°C, for example, it can be 185°C, 186°C, 187°C, 188°C, 189°C, 190°C, 191°C, 192°C, 193°C, 194°C or 195°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0092] In some optional examples, the temperature of the fifth zone is 180-190°C, for example, it can be 180°C, 181°C, 182°C, 183°C, 184°C, 185°C, 186°C, 187°C, 188C, 189°C or 190°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0093] In some optional examples, the screw speed of the screw extruder is 80-100 rpm, for example, it can be 80 rpm, 82 rpm, 84 rpm, 86 rpm, 88 rpm, 90 rpm, 92 rpm, 94 rpm, 96 rpm, 98 rpm or 100 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0094] In a second aspect, the present invention provides a flame-retardant polyolefin cable insulation material prepared by the preparation method described in the first aspect, wherein the flame-retardant polyolefin cable insulation material includes low-density polyethylene, polypropylene, ethylene-vinyl acetate, grafted modified magnesium hydroxide powder, composite modified boron nitride nanosheets, modified nanocellulose, lubricant, antioxidant and plasticizer.

[0095] As a preferred technical solution of the present invention, the grafted modified magnesium hydroxide powder is prepared by sequentially modifying magnesium hydroxide with sodium oleate and then grafting with methyl methacrylate.

[0096] In some optional examples, the composite modified boron nitride nanosheets are prepared by sequentially subjecting boron nitride powder to ultrasonic exfoliation, sodium hydroxide hydroxyl modification, and zinc oxide in-situ loading.

[0097] In some optional examples, the modified nanocellulose is prepared by modifying nanocellulose powder with dopamine.

[0098] As a preferred technical solution of the present invention, the flame-retardant polyolefin cable insulation material comprises the following components in parts by weight:

[0099]

[0100]

[0101] In some optional examples, the lubricant is any one of stearic acid, zinc stearate, calcium stearate, polyethylene wax, or a combination of at least two thereof.

[0102] In some optional examples, the antioxidant is any one of the antioxidant 1010, the antioxidant 626, and the antioxidant 168, or a combination of at least two of them.

[0103] In some optional examples, the plasticizer is any one of glycerol, epoxidized soybean oil, paraffin oil, or a combination of at least two thereof.

[0104] Compared with the prior art, the present invention has the following beneficial effects:

[0105] The present invention adopts magnesium hydroxide as a flame retardant filler and performs surface modification on the magnesium hydroxide, thereby improving the interface compatibility between the magnesium hydroxide and a polymer matrix; in addition, the present invention incorporates composite modified boron nitride nanosheets and modified nanocellulose into the polymer matrix to form a composite system having flame retardancy, thermal conductivity and mechanical reinforcement effects, thereby preparing a flame retardant polyolefin cable insulation material with excellent comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0106] Figure 1 A process flow chart for preparing the flame-retardant polyolefin cable insulation material provided in Examples 1-5 of the present invention;

[0107] Figure 2 This is a scanning electron microscope image of the modified magnesium hydroxide powder prepared in Example 1 of the present invention;

[0108] Figure 3 This is a transmission electron micrograph of the modified magnesium hydroxide powder prepared in Example 1 of the present invention;

[0109] Figure 4 This is a scanning electron microscope image of the grafted modified magnesium hydroxide powder prepared in Example 1 of the present invention;

[0110] Figure 5 This is a scanning electron microscope image of the grafted modified magnesium hydroxide powder prepared in Comparative Example 2 of the present invention;

[0111] Figure 6 The infrared spectra of unmodified magnesium hydroxide and the grafted modified magnesium hydroxide powder prepared in Example 1 of the present invention;

[0112] Figure 7 This is a transmission electron microscope image of boron nitride powder without ultrasonic exfoliation;

[0113] Figure 8 is a transmission electron microscope image of the boron nitride nanosheets obtained after ultrasonic exfoliation in Example 1 of the present invention;

[0114] Fig. 9 This is a scanning electron microscope image of the composite modified boron nitride nanosheets prepared in Example 1 of the present invention at a low magnification;

[0115] Fig.10 This is a scanning electron microscope image of the composite modified boron nitride nanosheets prepared in Example 1 of the present invention at a high magnification;

[0116] Fig.11 This is an infrared spectrum of the composite modified boron nitride nanosheets prepared in Example 1 of the present invention;

[0117] Fig.12 is the transmission electron microscopy image of unmodified nanocellulose;

[0118] Fig.13 This is a transmission electron microscopy image of the modified nanocellulose prepared in Example 1 of the present invention;

[0119] Fig.14 The infrared spectra of unmodified nanocellulose and modified nanocellulose prepared in Example 1 of the present invention are shown. DETAILED DESCRIPTION

[0120] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and their accompanying drawings. The embodiments recorded herein are specific embodiments of the present invention, which are used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary and should not be construed as limitations on the embodiments of the present invention and the scope of protection of the present invention. In addition to the embodiments recorded herein, those skilled in the art can also adopt other obvious technical solutions based on the contents disclosed in the claims of this application and its specification, including technical solutions that adopt any obvious replacements and modifications to the embodiments recorded herein.

[0121] The chemical reagents used in the embodiments provided by the present invention are all commercially available products, and their brands, specifications and manufacturer information are as follows:

[0122] Magnesium hydroxide: S24256-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0123] Ethanol: industrial grade, purity >99%, purchased from Nanjing Chemical Reagent Co., Ltd.;

[0124] Sodium oleate: S30245-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0125] Methyl methacrylate monomer: industrial grade, purity >99%, purchased from Shandong Jinyueyuan New Materials Co., Ltd.;

[0126] Polyvinyl pyrrolidone: S30268-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0127] Ammonium persulfate: industrial grade, purity>99%, purchased from Nanjing Sifanke Chemical Co., Ltd.;

[0128] Sodium dodecyl sulfate: S15012-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0129] Fatty acid ethanolamide: S67465-500g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0130] Sodium ethoxylate sulfonate: industrial grade, purity >99%, purchased from Hubei Yongkuo Technology Co., Ltd.;

[0131] Boron nitride powder: industrial grade, purity> 99%, purchased from Tianyuan Aerospace Materials (Yingkou) Technology Co., Ltd.;

[0132] Sodium hydroxide: industrial grade, purity>99%, purchased from Nanjing Chemical Reagent Co., Ltd.;

[0133] Zinc nitrate hexahydrate: industrial grade, purity >99%, purchased from Nanjing Chemical Reagent Co., Ltd.;

[0134] Potassium hydroxide: industrial grade, purity>99%, purchased from Nanjing Chemical Reagent Co., Ltd.;

[0135] Hexadecyltrimethylammonium bromide: S15001-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0136] Silane coupling agent KH550: S15028-500ml, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0137] Silane coupling agent KH560: S15029-500ml, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0138] Silane coupling agent KH570: S15030-500ml, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0139] Dopamine: purity>99%, purchased from Hubei Xinkang Pharmaceutical Chemical Co., Ltd.;

[0140] Tris-HCl buffer solution: SRCA-JPH533, purchased from Shanghai Sai Ke Rui Biotechnology Co., Ltd.;

[0141] Nanocellulose powder: purity >99%, purchased from Shanghai Jingkang Bioengineering Co., Ltd.;

[0142] Low-density polyethylene: M202, purchased from Dongguan Nabaichuan Plastic Chemical Co., Ltd.;

[0143] Polypropylene: S51655-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0144] Ethylene vinyl acetate: industrial grade, purity >99%, purchased from Henan Weitixi Chemical Technology Co., Ltd.;

[0145] Stearic acid: S30473-500g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0146] Zinc stearate: S24319-500g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0147] Calcium stearate: S24307-250g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0148] Polyethylene wax: Y45330-25 g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0149] Antioxidant 1010: S67391-25g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0150] Antioxidant 626: S99546-25g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0151] Antioxidant 168: S31114-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0152] Glycerol: R21114-100ml, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0153] Epoxidized soybean oil: S50881-100ml, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0154] Paraffin oil: WD0384, purchased from Hubei Wonder Chemical Co., Ltd.

[0155] Example 1

[0156] This embodiment provides a method for preparing a flame retardant polyolefin cable insulation material. Figure 1 As shown, the preparation method comprises:

[0157] (1) dispersing magnesium hydroxide in an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 8:2, and ultrasonically dispersing the solution for 20 minutes at an ultrasonic power of 700 W to obtain a magnesium hydroxide dispersion with a concentration of 0.2 g / mL, adding sodium oleate to the magnesium hydroxide dispersion, wherein the mass ratio of magnesium hydroxide to sodium oleate is 1:0.1, and ultrasonically dispersing the solution for 40 minutes at an ultrasonic power of 900 W to obtain a modified magnesium hydroxide dispersion, and filtering the modified magnesium hydroxide dispersion, washing, drying, grinding, and passing through a 200-mesh sieve to obtain a modified magnesium hydroxide powder;

[0158] Dispersing modified magnesium hydroxide powder and methyl methacrylate monomer in an ethanol solution of polyvinyl pyrrolidone, wherein the mass fraction of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 8wt%, the mass ratio of modified magnesium hydroxide powder to polyvinyl pyrrolidone is 1:0.04, and the mass ratio of modified magnesium hydroxide powder to methyl methacrylate monomer is 1:0.4. After uniform mixing, a precursor solution is obtained. Under nitrogen atmosphere and stirring and heating conditions, ammonium persulfate is added to the precursor solution, and the mass ratio of methyl methacrylate monomer to ammonium persulfate is 1:0.005. The mixture is refluxed at 70°C for 8h. After the reaction is completed, the reaction product is filtered, washed and dried to obtain grafted modified magnesium hydroxide powder.

[0159] (2) mixing sodium dodecyl sulfate, fatty acid ethanolamide, ethoxylated sodium sulfonate and deionized water to obtain a boron nitride stripping solution, wherein the concentration of sodium dodecyl sulfate in the boron nitride stripping solution is 12wt%, the concentration of fatty acid ethanolamide is 8wt%, and the concentration of ethoxylated sodium sulfonate is 4wt%; adding boron nitride powder to the boron nitride stripping solution, the ratio of boron nitride powder to boron nitride stripping solution is 1g:30mL, performing ultrasonic dispersion at an ultrasonic power of 1000W for 2h and heating to 30°C to strip the boron nitride powder to form a boron nitride dispersion, centrifuging, washing and drying the boron nitride dispersion to obtain boron nitride nanosheets;

[0160] The boron nitride nanosheets were mixed and stirred with a sodium hydroxide solution having a concentration of 3 mol / L, with the mass ratio of the boron nitride nanosheets to the sodium hydroxide being 1:15, and then ultrasonically dispersed for 2 h at an ultrasonic power of 800 W to obtain a mixed solution, which was transferred to a reactor and subjected to a hydrothermal reaction at 110° C. for 48 h. After the reaction was completed, the reaction product was filtered, washed and dried to obtain hydroxyl-modified boron nitride nanosheets;

[0161] (3) mixing the hydroxyl-modified boron nitride nanosheets obtained in step (2), zinc nitrate hexahydrate and deionized water uniformly to obtain a precursor solution, wherein the concentration of the hydroxyl-modified boron nitride nanosheets in the precursor solution is 10 g / L, and the molar concentration of the zinc nitrate hexahydrate is 1 mol / L; adding a potassium hydroxide solution with a molar concentration of 1 mol / L to the precursor solution, wherein the molar ratio of the potassium hydroxide in the potassium hydroxide solution to the zinc nitrate hexahydrate in the precursor solution is 2:1, stirring for 3 hours to react to generate a flocculent precipitate, and obtaining a reaction mixture after the reaction is completed; adding hexadecyltrimethylammonium bromide to the reaction mixture, wherein the mass ratio of hexadecyltrimethylammonium bromide to zinc nitrate hexahydrate is 1:8, mixing uniformly, transferring to a reactor, and performing a hydrothermal reaction at 120° C. for 3 hours. After the reaction is completed, filtering, washing and drying are performed to obtain composite boron nitride nanosheets loaded with zinc oxide;

[0162] The composite boron nitride nanosheets are immersed in a silane coupling agent solution, wherein the silane coupling agent solution is composed of a silane coupling agent KH550 and an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 8:2, and the mass fraction of the silane coupling agent KH550 in the silane coupling agent solution is 5wt%. After immersion for 5 hours, the composite boron nitride nanosheets are taken out, and after washing and drying, composite modified boron nitride nanosheets are obtained;

[0163] (4) dissolving dopamine in a 30 g / L Tris-hydrochloric acid buffer solution to obtain a dopamine solution, wherein the concentration of dopamine in the dopamine solution is 1 g / L, and immersing nanocellulose powder in the dopamine solution, wherein the mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is 4:1, so that dopamine self-polymerizes in situ on the surface of the nanocellulose to form polydopamine, and after immersion for 12 hours, filtering, washing, and freeze-drying at -20°C for 30 hours to obtain modified nanocellulose;

[0164] (5) 30 parts of low-density polyethylene, 19 parts of polypropylene, 18 parts of ethylene-vinyl acetate, 10 parts of the grafted modified magnesium hydroxide powder obtained in step (1), 12 parts of the composite modified boron nitride nanosheets obtained in step (3), 5 parts of the modified nanocellulose obtained in step (4), 2 parts of stearic acid, 2 parts of antioxidant 1010 and 2 parts of epoxidized soybean oil were added into a mixing device, and stirred at a rotation speed of 1200 rpm for 10 minutes to obtain a mixed masterbatch;

[0165] The mixed masterbatch is fed into the feed port of a screw extruder, and the barrel of the screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction, wherein the temperature of the first zone is 160° C., the temperature of the second zone is 170° C., the temperature of the third zone is 175° C., the temperature of the fourth zone is 185° C., the temperature of the fifth zone is 180° C., the screw speed is 80 rpm, and after being melt-extruded by the screw extruder, the mixture is cooled and formed to obtain the flame-retardant polyolefin cable insulation material.

[0166] Figure 2 and Figure 3 The figures are scanning electron microscope images and transmission electron microscope images of the modified magnesium hydroxide powder prepared in Example 1 of the present invention, respectively. It can be seen from the figures that the modified magnesium hydroxide powder prepared in this example is a hexagonal flake structure.

[0167] Figure 4 This is a scanning electron microscope image of the grafted modified magnesium hydroxide powder prepared in Example 1 of the present invention. It can be seen from the figure that a protruding structure appears on the surface of the grafted modified magnesium hydroxide powder, which is a polymer agglomerate formed by methyl methacrylate grafted on the surface of the modified magnesium hydroxide powder.

[0168] Figure 6 The infrared spectra of unmodified magnesium hydroxide and grafted modified magnesium hydroxide powders are shown in Figure 1. Compared with the infrared spectrum of unmodified magnesium hydroxide, the infrared spectrum of grafted modified magnesium hydroxide powder is 1735cm- 1 The new characteristic absorption peak at 1440cm corresponds to the stretching vibration of C=O; -1 The new characteristic absorption peak at 1279cm -1 、1262cm -1 、1200cm -1 and 1165cm -1 The new characteristic absorption peak that appears at corresponds to the stretching vibration of COC, which indicates that methyl methacrylate has been successfully grafted onto the surface of magnesium hydroxide powder.

[0169] Figure 7 and Figure 8 They are transmission electron microscope images of boron nitride powder before ultrasonic exfoliation and boron nitride nanosheets obtained after ultrasonic exfoliation in this embodiment. It can be seen from the figures that the boron nitride flakes after ultrasonic exfoliation are exfoliated and dispersed more evenly to form boron nitride nanosheets.

[0170] Fig. 9 and Fig.10The scanning electron microscope images of the composite modified boron nitride nanosheets prepared in this example at different magnifications show that a large amount of flaky zinc oxide is uniformly loaded on the surface of the hydroxyl-modified boron nitride nanosheets. This is because the surface of the hydroxyl-modified boron nitride nanosheets contains a large number of defects and negative charges, and thus easily adsorbs zinc ions, making it easier for the liquid phase precipitation reaction of sodium hydroxide and zinc nitrate to occur on the surface of the hydroxyl-modified boron nitride nanosheets.

[0171] Fig.11 This is the infrared spectrum of the composite modified boron nitride nanosheets. It can be seen from the figure that 1387cm- 1 and 785cm- 1 The characteristic absorption peaks at 421cm correspond to the vibration of the BN bond in the plane of boron nitride and the bending mode vibration of the BNB bond out of the plane; -1 and 546cm -1 The characteristic absorption peak appearing at is the stretching vibration peak of Zn-O in zinc oxide, which indicates that a composite of boron nitride nanosheets and zinc oxide is formed in the composite modified boron nitride nanosheets.

[0172] Fig.12 and Fig.13 The transmission electron micrographs of the unmodified nanocellulose and the modified nanocellulose prepared in this example are shown. It can be seen from the figure that there is no obvious difference in the appearance of the nanocellulose before and after modification, but the diameter of the modified nanocellulose increases, which indicates that a polydopamine coating layer is formed on the surface of the nanocellulose.

[0173] Fig.14 The infrared spectra of unmodified nanocellulose and modified nanocellulose are shown in Figure 1. Compared with the infrared spectrum curve of unmodified nanocellulose, the infrared spectrum curve of modified nanocellulose has a higher peak at 1513 cm- 1 and 1734cm- 1 The new characteristic absorption peaks that appear at correspond to the shear vibration peak of NH and the stretching vibration peak of C=O on the benzene ring. This is because the formation of polydopamine will introduce benzene rings and amino groups on the surface of nanocellulose, which indicates that nanocellulose is modified by polydopamine.

[0174] Example 2

[0175] This embodiment provides a method for preparing a flame retardant polyolefin cable insulation material. Figure 1 As shown, the preparation method comprises:

[0176] (1) dispersing magnesium hydroxide in an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 8.2:1.8, and ultrasonically dispersing the solution for 18 minutes at an ultrasonic power of 720 W to obtain a magnesium hydroxide dispersion with a concentration of 0.22 g / mL, adding sodium oleate to the magnesium hydroxide dispersion, wherein the mass ratio of magnesium hydroxide to sodium oleate is 1:0.12, and ultrasonically dispersing the solution for 38 minutes at an ultrasonic power of 920 W to obtain a modified magnesium hydroxide dispersion, and filtering the modified magnesium hydroxide dispersion, washing, drying, grinding, and passing through a 220-mesh sieve to obtain a modified magnesium hydroxide powder;

[0177] Dispersing modified magnesium hydroxide powder and methyl methacrylate monomer in an ethanol solution of polyvinyl pyrrolidone, wherein the mass fraction of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 8.5wt%, the mass ratio of modified magnesium hydroxide powder to polyvinyl pyrrolidone is 1:0.042, and the mass ratio of modified magnesium hydroxide powder to methyl methacrylate monomer is 1:0.42. After uniform mixing, a precursor solution is obtained. Under nitrogen atmosphere and stirring and heating conditions, ammonium persulfate is added to the precursor solution, and the mass ratio of methyl methacrylate monomer to ammonium persulfate is 1:0.008. The mixture is refluxed at 72°C for 7h. After the reaction is completed, the reaction product is filtered, washed and dried to obtain grafted modified magnesium hydroxide powder.

[0178] (2) mixing sodium dodecyl sulfate, fatty acid ethanolamide, ethoxylated sodium sulfonate and deionized water to obtain a boron nitride stripping solution, wherein the concentration of sodium dodecyl sulfate in the boron nitride stripping solution is 13wt%, the concentration of fatty acid ethanolamide is 7wt%, and the concentration of ethoxylated sodium sulfonate is 4.2wt%; adding boron nitride powder to the boron nitride stripping solution, the ratio of boron nitride powder to boron nitride stripping solution is 1g:32mL, ultrasonically dispersing for 1.8h at an ultrasonic power of 1050W and heating to 32°C to strip the boron nitride powder to form a boron nitride dispersion, centrifuging, washing and drying the boron nitride dispersion to obtain boron nitride nanosheets;

[0179] The boron nitride nanosheets were mixed and stirred with a sodium hydroxide solution having a concentration of 4 mol / L, and the mass ratio of the boron nitride nanosheets to the sodium hydroxide was 1:18. The mixed solution was then ultrasonically dispersed at an ultrasonic power of 850 W for 1.8 h to obtain a mixed solution. The mixed solution was transferred to a reactor and subjected to a hydrothermal reaction at 115° C. for 42 h. After the reaction was completed, the reaction product was filtered, washed and dried to obtain hydroxyl-modified boron nitride nanosheets.

[0180] (3) mixing the hydroxyl-modified boron nitride nanosheets obtained in step (2), zinc nitrate hexahydrate and deionized water uniformly to obtain a precursor solution, wherein the concentration of the hydroxyl-modified boron nitride nanosheets in the precursor solution is 12 g / L, and the molar concentration of the zinc nitrate hexahydrate is 1.2 mol / L; adding a potassium hydroxide solution with a molar concentration of 1.2 mol / L to the precursor solution, wherein the molar ratio of the potassium hydroxide in the potassium hydroxide solution to the zinc nitrate hexahydrate in the precursor solution is 2:1, stirring for 3.2 hours to react to generate a flocculent precipitate, and obtaining a reaction mixture after the reaction is completed; adding hexadecyltrimethylammonium bromide to the reaction mixture, wherein the mass ratio of hexadecyltrimethylammonium bromide to zinc nitrate hexahydrate is 1:8.2, mixing uniformly, transferring to a reactor, and performing a hydrothermal reaction at 122° C. for 2.5 hours. After the reaction is completed, filtering, washing and drying are performed to obtain composite boron nitride nanosheets loaded with zinc oxide;

[0181] The composite boron nitride nanosheets are immersed in a silane coupling agent solution, wherein the silane coupling agent solution is composed of a silane coupling agent KH550 and an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 8.2:1.8, and the mass fraction of the silane coupling agent KH550 in the silane coupling agent solution is 6wt%. After immersion for 4.5 hours, the composite boron nitride nanosheets are taken out, and after washing and drying, composite modified boron nitride nanosheets are obtained;

[0182] (4) dissolving dopamine in a 32 g / L Tris-hydrochloric acid buffer solution to obtain a dopamine solution, wherein the concentration of dopamine in the dopamine solution is 2 g / L, and immersing nanocellulose powder in the dopamine solution, wherein the mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is 4.2:1, so that dopamine self-polymerizes in situ on the surface of the nanocellulose to form polydopamine, and after immersion for 15 hours, filtering, washing, and freeze-drying at -22°C for 28 hours to obtain modified nanocellulose;

[0183] (5) 32 parts of low-density polyethylene, 20 parts of polypropylene, 18 parts of ethylene-vinyl acetate, 10 parts of the grafted modified magnesium hydroxide powder obtained in step (1), 10 parts of the composite modified boron nitride nanosheets obtained in step (3), 5 parts of the modified nanocellulose obtained in step (4), 1 part of zinc stearate, 2 parts of antioxidant 1010 and 2 parts of epoxidized soybean oil were added into a mixing device, and stirred at a rotation speed of 1300 rpm for 8 minutes to obtain a mixed masterbatch;

[0184] The mixed masterbatch is fed into the feed port of a screw extruder, and the barrel of the screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction, wherein the temperature of the first zone is 162° C., the temperature of the second zone is 172° C., the temperature of the third zone is 178° C., the temperature of the fourth zone is 188° C., the temperature of the fifth zone is 182° C., the screw speed is 85 rpm, and after being melt-extruded by the screw extruder, the mixture is cooled and formed to obtain the flame-retardant polyolefin cable insulation material.

[0185] Example 3

[0186] This embodiment provides a method for preparing a flame retardant polyolefin cable insulation material. Figure 1 As shown, the preparation method comprises:

[0187] (1) dispersing magnesium hydroxide in an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 8.5:1.5, and ultrasonically dispersing the solution for 15 minutes at an ultrasonic power of 750 W to obtain a magnesium hydroxide dispersion with a concentration of 0.25 g / mL, adding sodium oleate to the magnesium hydroxide dispersion, wherein the mass ratio of magnesium hydroxide to sodium oleate is 1:0.15, and ultrasonically dispersing the solution for 35 minutes at an ultrasonic power of 950 W to obtain a modified magnesium hydroxide dispersion, and filtering the modified magnesium hydroxide dispersion, washing, drying, grinding, and passing through a 250-mesh sieve to obtain a modified magnesium hydroxide powder;

[0188] Dispersing modified magnesium hydroxide powder and methyl methacrylate monomer in an ethanol solution of polyvinyl pyrrolidone, wherein the mass fraction of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 9wt%, the mass ratio of modified magnesium hydroxide powder to polyvinyl pyrrolidone is 1:0.045, and the mass ratio of modified magnesium hydroxide powder to methyl methacrylate monomer is 1:0.45. After uniform mixing, a precursor solution is obtained. Under nitrogen atmosphere and stirring and heating conditions, ammonium persulfate is added to the precursor solution, and the mass ratio of methyl methacrylate monomer to ammonium persulfate is 1:0.01. The mixture is refluxed at 75°C for 7h. After the reaction is completed, the reaction product is filtered, washed and dried to obtain grafted modified magnesium hydroxide powder.

[0189] (2) mixing sodium dodecyl sulfate, fatty acid ethanolamide, ethoxylated sodium sulfonate and deionized water and stirring them uniformly to obtain a boron nitride stripping solution, wherein the concentration of sodium dodecyl sulfate in the boron nitride stripping solution is 13wt%, the concentration of fatty acid ethanolamide is 7wt%, and the concentration of ethoxylated sodium sulfonate is 4.5wt%; adding boron nitride powder to the boron nitride stripping solution, the ratio of boron nitride powder to boron nitride stripping solution is 1g:35mL, performing ultrasonic dispersion at an ultrasonic power of 1100W for 1.5h and heating to 35°C to strip the boron nitride powder to form a boron nitride dispersion, centrifuging, washing and drying the boron nitride dispersion to obtain boron nitride nanosheets;

[0190] The boron nitride nanosheets were mixed and stirred with a sodium hydroxide solution having a concentration of 5 mol / L, with the mass ratio of the boron nitride nanosheets to the sodium hydroxide being 1:20, and then ultrasonically dispersed for 1.5 h at an ultrasonic power of 900 W to obtain a mixed solution, which was transferred to a reactor and subjected to a hydrothermal reaction at 120° C. for 36 h. After the reaction was completed, the reaction product was filtered, washed and dried to obtain hydroxyl-modified boron nitride nanosheets;

[0191] (3) mixing the hydroxyl-modified boron nitride nanosheets obtained in step (2), zinc nitrate hexahydrate and deionized water uniformly to obtain a precursor solution, wherein the concentration of the hydroxyl-modified boron nitride nanosheets in the precursor solution is 15 g / L, and the molar concentration of the zinc nitrate hexahydrate is 1.5 mol / L; adding a potassium hydroxide solution with a molar concentration of 1.5 mol / L to the precursor solution, wherein the molar ratio of the potassium hydroxide in the potassium hydroxide solution to the zinc nitrate hexahydrate in the precursor solution is 2:1, stirring for 3.5 hours to react to generate a flocculent precipitate, and obtaining a reaction mixture after the reaction is completed; adding hexadecyltrimethylammonium bromide to the reaction mixture, wherein the mass ratio of hexadecyltrimethylammonium bromide to zinc nitrate hexahydrate is 1:8.5, mixing uniformly, transferring to a reactor, and performing a hydrothermal reaction at 125° C. for 2 hours. After the reaction is completed, filtering, washing and drying are performed to obtain composite boron nitride nanosheets loaded with zinc oxide;

[0192] The composite boron nitride nanosheets are immersed in a silane coupling agent solution, wherein the silane coupling agent solution is composed of a silane coupling agent KH560 and an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 8.5:1.5, and the mass fraction of the silane coupling agent KH560 in the silane coupling agent solution is 7wt%. After immersion for 4 hours, the composite boron nitride nanosheets are taken out, and after washing and drying, composite modified boron nitride nanosheets are obtained;

[0193] (4) dissolving dopamine in a 35 g / L Tris-hydrochloric acid buffer solution to obtain a dopamine solution, wherein the concentration of dopamine in the dopamine solution is 3 g / L, and immersing nanocellulose powder in the dopamine solution, wherein the mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is 4.5:1, so that dopamine self-polymerizes in situ on the surface of the nanocellulose to form polydopamine, and after immersion for 18 hours, filtering, washing, and freeze-drying at -25°C for 25 hours to obtain modified nanocellulose;

[0194] (5) 36 parts of low-density polyethylene, 16 parts of polypropylene, 18 parts of ethylene-vinyl acetate, 9 parts of the grafted modified magnesium hydroxide powder obtained in step (1), 11 parts of the composite modified boron nitride nanosheets obtained in step (3), 4 parts of the modified nanocellulose obtained in step (4), 2 parts of calcium stearate, 2 parts of antioxidant 626 and 2 parts of paraffin oil were added into a mixing device, and stirred at a rotation speed of 1350 rpm for 7 minutes to obtain a mixed masterbatch;

[0195] The mixed masterbatch is fed into the feed port of a screw extruder, and the barrel of the screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction, wherein the temperature of the first zone is 165° C., the temperature of the second zone is 175° C., the temperature of the third zone is 180° C., the temperature of the fourth zone is 190° C., the temperature of the fifth zone is 185° C., the screw speed is 90 rpm, and after being melt-extruded by the screw extruder, the mixture is cooled and formed to obtain the flame-retardant polyolefin cable insulation material.

[0196] Example 4

[0197] This embodiment provides a method for preparing a flame retardant polyolefin cable insulation material. Figure 1 As shown, the preparation method comprises:

[0198] (1) dispersing magnesium hydroxide in an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 8.8:1.2, and ultrasonically dispersing the solution for 12 minutes at an ultrasonic power of 780 W to obtain a magnesium hydroxide dispersion with a concentration of 0.28 g / mL, adding sodium oleate to the magnesium hydroxide dispersion, wherein the mass ratio of magnesium hydroxide to sodium oleate is 1:0.18, and ultrasonically dispersing the solution for 32 minutes at an ultrasonic power of 980 W to obtain a modified magnesium hydroxide dispersion, and filtering the modified magnesium hydroxide dispersion, washing, drying, grinding, and passing through a 280-mesh sieve to obtain a modified magnesium hydroxide powder;

[0199] Dispersing modified magnesium hydroxide powder and methyl methacrylate monomer in an ethanol solution of polyvinyl pyrrolidone, wherein the mass fraction of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 9.5wt%, the mass ratio of modified magnesium hydroxide powder to polyvinyl pyrrolidone is 1:0.048, and the mass ratio of modified magnesium hydroxide powder to methyl methacrylate monomer is 1:0.48. After uniform mixing, a precursor solution is obtained. Under nitrogen atmosphere and stirring and heating conditions, ammonium persulfate is added to the precursor solution, and the mass ratio of methyl methacrylate monomer to ammonium persulfate is 1:0.012. The mixture is refluxed at 78°C for 6 hours. After the reaction is completed, the reaction product is filtered, washed and dried to obtain grafted modified magnesium hydroxide powder.

[0200] (2) mixing sodium dodecyl sulfate, fatty acid ethanolamide, ethoxylated sodium sulfonate and deionized water and stirring them uniformly to obtain a boron nitride stripping solution, wherein the concentration of sodium dodecyl sulfate in the boron nitride stripping solution is 14wt%, the concentration of fatty acid ethanolamide is 6wt%, and the concentration of ethoxylated sodium sulfonate is 4.8wt%; adding boron nitride powder to the boron nitride stripping solution, the ratio of boron nitride powder to boron nitride stripping solution is 1g:38mL, ultrasonically dispersing the boron nitride powder at an ultrasonic power of 1150W for 1.2h and heating to 38°C to strip the boron nitride powder to form a boron nitride dispersion, centrifuging the boron nitride dispersion, washing and drying the boron nitride nanosheets;

[0201] The boron nitride nanosheets were mixed and stirred with a sodium hydroxide solution having a concentration of 6 mol / L, and the mass ratio of the boron nitride nanosheets to the sodium hydroxide was 1:22. The mixed solution was then ultrasonically dispersed at an ultrasonic power of 950 W for 1.2 h to obtain a mixed solution. The mixed solution was transferred to a reactor and subjected to a hydrothermal reaction at 125 ° C for 30 h. After the reaction was completed, the reaction product was filtered, washed and dried to obtain hydroxyl-modified boron nitride nanosheets.

[0202] (3) mixing the hydroxyl-modified boron nitride nanosheets, zinc nitrate hexahydrate and deionized water obtained in step (2) uniformly to obtain a precursor solution, wherein the concentration of the hydroxyl-modified boron nitride nanosheets in the precursor solution is 18 g / L, and the molar concentration of the zinc nitrate hexahydrate is 1.8 mol / L; adding a potassium hydroxide solution with a molar concentration of 1.8 mol / L to the precursor solution, wherein the molar ratio of the potassium hydroxide in the potassium hydroxide solution to the zinc nitrate hexahydrate in the precursor solution is 2:1, stirring for 3.8 hours to react to generate a flocculent precipitate, and obtaining a reaction mixture after the reaction is completed; adding hexadecyltrimethylammonium bromide to the reaction mixture, wherein the mass ratio of hexadecyltrimethylammonium bromide to zinc nitrate hexahydrate is 1:8.8, mixing uniformly, transferring to a reactor, and performing a hydrothermal reaction at 128° C. for 1.5 hours. After the reaction is completed, filtering, washing and drying are performed to obtain composite boron nitride nanosheets loaded with zinc oxide;

[0203] The composite boron nitride nanosheets are immersed in a silane coupling agent solution, wherein the silane coupling agent solution is composed of a silane coupling agent KH570 and an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 8.8:1.2, and the mass fraction of the silane coupling agent KH570 in the silane coupling agent solution is 8wt%. After immersion for 3.5 hours, the composite boron nitride nanosheets are taken out, and after washing and drying, composite modified boron nitride nanosheets are obtained;

[0204] (4) dissolving dopamine in a 38 g / L Tris-HCl buffer solution to obtain a dopamine solution, wherein the concentration of dopamine in the dopamine solution is 4 g / L, and immersing nanocellulose powder in the dopamine solution, wherein the mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is 4.8:1, so that dopamine self-polymerizes in situ on the surface of the nanocellulose to form polydopamine, and after immersion for 20 hours, filtering, washing, and freeze-drying at -28°C for 22 hours to obtain modified nanocellulose;

[0205] (5) 38 parts of low-density polyethylene, 15 parts of polypropylene, 20 parts of ethylene-vinyl acetate, 8 parts of the grafted modified magnesium hydroxide powder obtained in step (1), 12 parts of the composite modified boron nitride nanosheets obtained in step (3), 3 parts of the modified nanocellulose obtained in step (4), 2 parts of polyethylene wax, 1 part of antioxidant 168 and 1 part of paraffin oil were added into a mixing device, and stirred at a rotation speed of 1400 rpm for 6 minutes to obtain a mixed masterbatch;

[0206] The mixed masterbatch is fed into the feed port of a screw extruder, and the barrel of the screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction, wherein the temperature of the first zone is 168° C., the temperature of the second zone is 178° C., the temperature of the third zone is 182° C., the temperature of the fourth zone is 192° C., the temperature of the fifth zone is 188° C., the screw speed is 95 rpm, and the mixture is melt-extruded by the screw extruder and then cooled and formed to obtain the flame-retardant polyolefin cable insulation material.

[0207] Example 5

[0208] This embodiment provides a method for preparing a flame retardant polyolefin cable insulation material. Figure 1 As shown, the preparation method comprises:

[0209] (1) dispersing magnesium hydroxide in an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 9:1, and ultrasonically dispersing the solution for 10 min at an ultrasonic power of 800 W to obtain a magnesium hydroxide dispersion having a concentration of 0.3 g / mL, adding sodium oleate to the magnesium hydroxide dispersion, wherein the mass ratio of magnesium hydroxide to sodium oleate is 1:0.2, and ultrasonically dispersing the solution for 30 min at an ultrasonic power of 1000 W to obtain a modified magnesium hydroxide dispersion, and filtering the modified magnesium hydroxide dispersion, washing, drying, grinding, and passing through a 300-mesh sieve to obtain a modified magnesium hydroxide powder;

[0210] Dispersing modified magnesium hydroxide powder and methyl methacrylate monomer in an ethanol solution of polyvinyl pyrrolidone, wherein the mass fraction of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 10wt%, the mass ratio of modified magnesium hydroxide powder to polyvinyl pyrrolidone is 1:0.05, and the mass ratio of modified magnesium hydroxide powder to methyl methacrylate monomer is 1:0.5, and mixing them evenly to obtain a precursor solution, adding ammonium persulfate to the precursor solution under nitrogen atmosphere and stirring and heating conditions, wherein the mass ratio of methyl methacrylate monomer to ammonium persulfate is 1:0.015, and performing reflux reaction at 80°C for 5h. After the reaction is completed, filtering, washing and drying the reaction product to obtain grafted modified magnesium hydroxide powder;

[0211] (2) mixing sodium dodecyl sulfate, fatty acid ethanolamide, ethoxylated sodium sulfonate and deionized water to obtain a boron nitride stripping solution, wherein the concentration of sodium dodecyl sulfate in the boron nitride stripping solution is 15wt%, the concentration of fatty acid ethanolamide is 5wt%, and the concentration of ethoxylated sodium sulfonate is 5wt%; adding boron nitride powder to the boron nitride stripping solution, the ratio of boron nitride powder to boron nitride stripping solution is 1g:40mL, ultrasonically dispersing the boron nitride powder at an ultrasonic power of 1200W for 1h and heating to 40°C to strip the boron nitride powder to form a boron nitride dispersion, centrifuging the boron nitride dispersion, washing and drying the boron nitride nanosheets;

[0212] The boron nitride nanosheets were mixed and stirred with a sodium hydroxide solution having a concentration of 8 mol / L, with the mass ratio of the boron nitride nanosheets to the sodium hydroxide being 1:25, and then ultrasonically dispersed for 1 h at an ultrasonic power of 1000 W to obtain a mixed solution, which was transferred to a reactor and subjected to a hydrothermal reaction at 130° C. for 24 h. After the reaction was completed, the reaction product was filtered, washed and dried to obtain hydroxyl-modified boron nitride nanosheets;

[0213] (3) mixing the hydroxyl-modified boron nitride nanosheets obtained in step (2), zinc nitrate hexahydrate and deionized water uniformly to obtain a precursor solution, wherein the concentration of the hydroxyl-modified boron nitride nanosheets in the precursor solution is 20 g / L, and the molar concentration of the zinc nitrate hexahydrate is 2 mol / L; adding a potassium hydroxide solution with a molar concentration of 2 mol / L to the precursor solution, wherein the molar ratio of the potassium hydroxide in the potassium hydroxide solution to the zinc nitrate hexahydrate in the precursor solution is 2:1, stirring for 4 hours to react to generate a flocculent precipitate, and obtaining a reaction mixture after the reaction is completed; adding hexadecyltrimethylammonium bromide to the reaction mixture, wherein the mass ratio of hexadecyltrimethylammonium bromide to zinc nitrate hexahydrate is 1:9, mixing uniformly, transferring to a reactor, and performing a hydrothermal reaction at 130° C. for 1 hour. After the reaction is completed, filtering, washing and drying are performed to obtain composite boron nitride nanosheets loaded with zinc oxide;

[0214] The composite boron nitride nanosheets are immersed in a silane coupling agent solution, wherein the silane coupling agent solution is composed of a silane coupling agent KH570 and an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is 9:1, and the mass fraction of the silane coupling agent KH570 in the silane coupling agent solution is 10wt%. After immersion for 3 hours, the composite boron nitride nanosheets are taken out, and after washing and drying, composite modified boron nitride nanosheets are obtained;

[0215] (4) dissolving dopamine in a 40 g / L Tris-hydrochloric acid buffer solution to obtain a dopamine solution, wherein the concentration of dopamine in the dopamine solution is 5 g / L, and immersing nanocellulose powder in the dopamine solution, wherein the mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is 5:1, so that dopamine self-polymerizes in situ on the surface of the nanocellulose to form polydopamine, and after immersion for 24 hours, filtering, washing, and freeze-drying at -30°C for 20 hours to obtain modified nanocellulose;

[0216] (5) 40 parts of low-density polyethylene, 13 parts of polypropylene, 14 parts of ethylene-vinyl acetate, 10 parts of the grafted modified magnesium hydroxide powder obtained in step (1), 12 parts of the composite modified boron nitride nanosheets obtained in step (3), 5 parts of the modified nanocellulose obtained in step (4), 2 parts of zinc stearate, 2 parts of antioxidant 168 and 2 parts of glycerol were added into a mixing device, and stirred at a rotation speed of 1500 rpm for 5 minutes to obtain a mixed masterbatch;

[0217] The mixed masterbatch is fed into the feed port of a screw extruder, and the barrel of the screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction, wherein the temperature of the first zone is 170°C, the temperature of the second zone is 180°C, the temperature of the third zone is 185°C, the temperature of the fourth zone is 195°C, the temperature of the fifth zone is 190°C, the screw speed is 100rpm, and after being melt-extruded by the screw extruder, the mixture is cooled and formed to obtain the flame-retardant polyolefin cable insulation material.

[0218] Comparative Example 1

[0219] This comparative example provides a method for preparing a flame-retardant polyolefin cable insulation material. The difference from Example 1 is that in step (1), the mass ratio of modified magnesium hydroxide powder to methyl methacrylate monomer is adjusted to 1:0.3, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0220] Comparative Example 2

[0221] This comparative example provides a method for preparing a flame-retardant polyolefin cable insulation material. The difference from Example 1 is that in step (1), the mass ratio of modified magnesium hydroxide powder to methyl methacrylate monomer is adjusted to 1:0.6, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0222] Figure 5 This is a scanning electron microscope image of the grafted modified magnesium hydroxide powder prepared in this comparative example. It can be seen from the figure that a large number of polymer agglomerates are formed on the surface of the modified magnesium hydroxide powder. This is because the methyl methacrylate monomer that is not grafted to the surface of the magnesium hydroxide powder undergoes self-polymerization to form free polymethyl methacrylate, and the polymethyl methacrylate is physically attached to the surface of the magnesium hydroxide powder and gradually agglomerates to form large-sized polymer agglomerates.

[0223] Comparative Example 3

[0224] This comparative example provides a method for preparing a flame-retardant polyolefin cable insulation material. The difference from Example 1 is that in step (3), the molar concentration of the potassium hydroxide solution is adjusted to 0.5 mol / L, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0225] Comparative Example 4

[0226] This comparative example provides a method for preparing a flame-retardant polyolefin cable insulation material. The difference from Example 1 is that in step (3), the molar concentration of the potassium hydroxide solution is adjusted to 2.5 mol / L, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0227] Comparative Example 5

[0228] This comparative example provides a method for preparing a flame-retardant polyolefin cable insulation material. The difference from Example 1 is that in step (5), the weight portion of the grafted modified magnesium hydroxide powder is adjusted to 6 parts, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0229] Comparative Example 6

[0230] This comparative example provides a method for preparing a flame-retardant polyolefin cable insulation material. The difference from Example 1 is that in step (5), the weight portion of the grafted modified magnesium hydroxide powder is adjusted to 12 parts, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0231] Comparative Example 7

[0232] This comparative example provides a method for preparing a flame-retardant polyolefin cable insulation material. The difference from Example 1 is that in step (5), the weight portion of the composite modified boron nitride nanosheets is adjusted to 8 parts, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0233] Comparative Example 8

[0234] This comparative example provides a method for preparing a flame-retardant polyolefin cable insulation material. The difference from Example 1 is that in step (5), the weight of the composite modified boron nitride nanosheets is adjusted to 15 parts, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0235] Comparative Example 9

[0236] This comparative example provides a method for preparing a flame-retardant polyolefin cable insulation material. The difference from Example 1 is that in step (5), the weight portion of modified nanocellulose is adjusted to 2 parts, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0237] Comparative Example 10

[0238] This comparative example provides a method for preparing a flame-retardant polyolefin cable insulation material. The difference from Example 1 is that in step (5), the weight portion of the modified nanocellulose is adjusted to 6 parts, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0239] The flame-retardant polyolefin cable insulation materials prepared in Examples 1-5 and Comparative Examples 1-10 were subjected to tensile strength test, oxygen index test, vertical burning test and thermal conductivity test. The specific test steps are as follows:

[0240] (1) Tensile strength test

[0241] With reference to the national standard GBT1040-2006 "Determination of tensile properties of plastics", a universal material testing machine was used to test the tensile strength of a sample with a length, width and thickness of 180 mm × 10 mm × 3 mm. The test speed was set to 2 mm / min, and the stretching was stopped when the sample broke. Five samples were prepared for each embodiment and comparative example, and the average value was taken.

[0242] The tensile strength of the sample (σ, MPa) is calculated according to the following formula:

[0243]

[0244] In the formula, F max is the tensile limit load of the specimen (N), A is the cross-sectional area of ​​the specimen (m 2 ).

[0245] (2) Limiting oxygen index test

[0246] With reference to the national standard GB / T2406.2-2009 "Determination of Combustion Behavior of Plastics by Oxygen Index Method Part 2: Room Temperature Test", a JF-3 oxygen index tester was used to perform an oxygen index test on a sample with a length, width and thickness of 80 mm × 6.5 mm × 3 mm. Five samples were prepared for each embodiment and comparative example, and the average value was taken.

[0247] The limiting oxygen index refers to the minimum oxygen concentration required for a sample to maintain balanced combustion in an oxygen-nitrogen mixture under specified test conditions. The higher the limiting oxygen index, the less flammable the material; conversely, the lower the limiting oxygen index, the more flammable the material.

[0248] (3) Vertical combustion test

[0249] According to the national standard GB / T10707-2008 "Determination of Rubber Combustion Performance", a vertical combustion test was performed on a sample with a length, width and thickness of 130 mm×13 mm×3 mm. Five samples were prepared for each embodiment and comparative example, and the average value was taken.

[0250] Vertical combustion performance is divided into three levels: (1) FV-0: flaming and flameless combustion time is less than 30 seconds, no flammable dripping; (2) FV-1: flaming and flameless combustion time is less than 60 seconds, no flammable dripping; (3) FV-2: flaming and flameless combustion time is less than 60 seconds, there are flammable dripping. If the total burning time is greater than 60 seconds, there is no flame retardant grade.

[0251] (4) Thermal conductivity test

[0252] The thermal conductivity of disc-shaped samples with a diameter of 25 mm and a thickness of 1 mm was tested by the single plate method provided in the national standard GB / T3399-1982 "Test method for thermal conductivity of plastics - guarded plate method". Five samples were prepared for each embodiment and comparative example, and the average value was taken.

[0253] The test results are shown in Table 1.

[0254] Table 1 Test results of flame-retardant polyolefin cable insulation materials prepared in Examples 1-5 and Comparative Examples 1-10

[0255]

[0256]

[0257] It can be seen from the data in Table 1 that the tensile strength, limiting oxygen index and thermal conductivity of the flame-retardant polyolefin cable insulation materials prepared in Examples 1-5 are higher than those in Comparative Examples 1-10, and the vertical burning grade is also better than that in Comparative Examples 1-10, which indicates that the flame-retardant polyolefin cable insulation material prepared by the preparation method provided by the present invention has excellent mechanical properties, flame retardant properties and thermal conductivity.

[0258] It can be seen from the test data of Example 1, Comparative Example 1 and Comparative Example 2 that the tensile strength, limiting oxygen index and thermal conductivity of the flame-retardant polyolefin cable insulation materials prepared in Comparative Example 1 and Comparative Example 2 are lower than those in Example 1. This is because the amount of methyl methacrylate monomer in Comparative Example 1 is too low, while the amount of methyl methacrylate monomer in Comparative Example 2 is too high, which affects the improvement of the surface hydrophobicity of the grafted modified magnesium hydroxide powder, resulting in poor interface compatibility between the grafted modified magnesium hydroxide powder and the polymer matrix, which ultimately leads to reduced mechanical properties, flame retardant properties and thermal conductivity of the flame-retardant polyolefin cable insulation material.

[0259] It can be seen from the test data of Example 1, Comparative Example 3 and Comparative Example 4 that the tensile strength, limiting oxygen index and thermal conductivity of the flame-retardant polyolefin cable insulation materials prepared in Comparative Example 3 and Comparative Example 4 are lower than those in Example 1. This is because the molar concentration of the potassium hydroxide solution in Comparative Example 3 is too low, while the molar concentration of the potassium hydroxide solution in Comparative Example 4 is too high, which affects the flaky structure of zinc oxide generated by the liquid phase precipitation reaction, thereby failing to form a continuous and stable heat conduction path in the polymer matrix, which not only affects the thermal conductivity of the flame-retardant polyolefin cable insulation material, but also affects its mechanical properties and flame retardant properties to a certain extent.

[0260] It can be seen from the test data of Example 1, Comparative Example 5 and Comparative Example 6 that the tensile strength, limiting oxygen index and thermal conductivity of the flame-retardant polyolefin cable insulation materials prepared in Comparative Examples 5 and 6 are lower than those in Example 1. This is because the addition amount of the grafted modified magnesium hydroxide powder in Comparative Example 5 is too low, while the addition amount of the grafted modified magnesium hydroxide powder in Comparative Example 6 is too high, which affects the mechanical properties, flame retardant properties and thermal conductivity of the flame-retardant polyolefin cable insulation materials.

[0261] It can be seen from the test data of Example 1, Comparative Example 7 and Comparative Example 8 that the tensile strength, limiting oxygen index and thermal conductivity of the flame-retardant polyolefin cable insulation materials prepared in Comparative Examples 7 and 8 are lower than those in Example 1. This is because the addition amount of the composite modified boron nitride nanosheets in Comparative Example 7 is too low, while the addition amount of the composite modified boron nitride nanosheets in Comparative Example 8 is too high, which affects the mechanical properties, flame retardant properties and thermal conductivity of the flame-retardant polyolefin cable insulation materials.

[0262] It can be seen from the test data of Example 1, Comparative Example 9 and Comparative Example 10 that the tensile strength, limiting oxygen index and thermal conductivity of the flame-retardant polyolefin cable insulation materials prepared in Comparative Example 9 and Comparative Example 10 are lower than those in Example 1. This is because the amount of modified nanocellulose added in Comparative Example 9 is too low, while the amount of modified nanocellulose added in Comparative Example 10 is too high, which affects the mechanical properties, flame retardant properties and thermal conductivity of the flame-retardant polyolefin cable insulation materials.

[0263] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a flame-retardant polyolefin cable insulation material, characterized in that: The preparation method comprises: Magnesium hydroxide is sequentially modified by sodium oleate and methyl methacrylate grafting to obtain grafted modified magnesium hydroxide powder; boron nitride nanosheets are sequentially modified by hydroxylation, hexadecyltrimethylammonium bromide and silane coupling agent to obtain composite modified boron nitride nanosheets; nanocellulose is modified by dopamine coating to obtain modified nanocellulose; Low-density polyethylene, polypropylene, ethylene-vinyl acetate, the grafted modified magnesium hydroxide powder, the composite modified boron nitride nanosheets, the modified nanocellulose, a lubricant, an antioxidant and a plasticizer are put into a mixing device for stirring to obtain a mixed masterbatch; the mixed masterbatch is fed into a feeding port of a screw extruder, melt-extruded by the screw extruder, and then cooled and formed to obtain the flame-retardant polyolefin cable insulation material.

2. The method for preparing a flame-retardant polyolefin cable insulation material according to claim 1, characterized in that: The preparation method specifically comprises the following steps: (I) dispersing magnesium hydroxide in an ethanol aqueous solution, ultrasonically dispersing to obtain a magnesium hydroxide dispersion, adding sodium oleate to the magnesium hydroxide dispersion, ultrasonically dispersing to obtain a modified magnesium hydroxide dispersion, filtering, washing, drying, grinding and sieving the modified magnesium hydroxide dispersion to obtain a modified magnesium hydroxide powder; dispersing the modified magnesium hydroxide powder and methyl methacrylate monomer in an ethanol solution of polyvinyl pyrrolidone, mixing to obtain a precursor solution, adding ammonium persulfate to the precursor solution under a nitrogen atmosphere and stirring and heating conditions to perform a reflux reaction, and after the reaction is completed, filtering, washing and drying the reaction product to obtain a grafted modified magnesium hydroxide powder; (II) mixing sodium dodecyl sulfate, fatty acid ethanolamide, ethoxylated sodium sulfonate and deionized water to obtain a boron nitride stripping solution; adding boron nitride powder to the boron nitride stripping solution, ultrasonically dispersing and heating to strip the boron nitride powder to form a boron nitride dispersion, centrifuging, washing and drying the boron nitride dispersion to obtain boron nitride nanosheets; mixing the boron nitride nanosheets with sodium hydroxide solution, stirring and ultrasonically dispersing to obtain a mixed solution, transferring the mixed solution to a reactor for hydrothermal reaction, and after the reaction is completed, filtering, washing and drying the reaction product to obtain hydroxyl-modified boron nitride nanosheets; (III) uniformly mixing the hydroxyl-modified boron nitride nanosheets obtained in step (II), zinc nitrate hexahydrate and deionized water to obtain a precursor solution, adding potassium hydroxide solution to the precursor solution, stirring uniformly to react and generate flocculent precipitates, obtaining a reaction mixture after the reaction is completed, adding hexadecyltrimethylammonium bromide to the reaction mixture, mixing uniformly and transferring to a reactor for hydrothermal reaction, filtering, washing and drying after the reaction to obtain composite boron nitride nanosheets loaded with zinc oxide; soaking the composite boron nitride nanosheets in a silane coupling agent solution, taking out the composite boron nitride nanosheets after soaking, washing and drying to obtain composite modified boron nitride nanosheets; (IV) dissolving dopamine in a Tris-hydrochloric acid buffer solution to obtain a dopamine solution, soaking the nanocellulose powder in the dopamine solution so that dopamine self-polymerizes in situ on the surface of the nanocellulose powder to form polydopamine, and after the soaking, filtering, washing and freeze-drying to obtain modified nanocellulose; (V) low-density polyethylene, polypropylene, ethylene-vinyl acetate, the grafted modified magnesium hydroxide powder obtained in step (I), the composite modified boron nitride nanosheets obtained in step (III), the modified nanocellulose obtained in step (IV), a lubricant, an antioxidant and a plasticizer are put into a mixing device for stirring to obtain a mixed masterbatch; the mixed masterbatch is fed into the feed port of a screw extruder, and the barrel of the screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction; after being melt-extruded by the screw extruder, the mixed masterbatch is cooled and formed to obtain the flame-retardant polyolefin cable insulation material.

3. The method for preparing a flame-retardant polyolefin cable insulation material according to claim 2, characterized in that: In step (I), the volume ratio of ethanol to deionized water in the ethanol aqueous solution is (8-9): (1N2); The power of ultrasonic dispersion after dispersing the magnesium hydroxide in the ethanol aqueous solution is 700 to 800 W, and the time of ultrasonic dispersion is 10 to 20 minutes; The concentration of magnesium hydroxide in the magnesium hydroxide dispersion is 0.2-0.3 g / mL; The mass ratio of the magnesium hydroxide to the sodium oleate in the magnesium hydroxide dispersion is 1:(0.1-0.2); The power of ultrasonic dispersion after adding sodium oleate to the magnesium hydroxide dispersion is 900-1000W, and the time of ultrasonic dispersion is 30-40min; The mesh number of the sieve is 200 to 300 meshes; The mass fraction of polyvinyl pyrrolidone in the polyvinyl pyrrolidone ethanol solution is 8-10wt%; The mass ratio of the modified magnesium hydroxide powder to the polyvinyl pyrrolidone in the polyvinyl pyrrolidone ethanol solution is 1:(0.04-0.05); The mass ratio of the modified magnesium hydroxide powder to the methyl methacrylate monomer is 1:(0.4-0.5); The mass ratio of the methyl methacrylate monomer in the precursor solution to the ammonium persulfate is 1:(0.005-0.015); The temperature of the reflux reaction is 70-80°C; The reflux reaction time is 5 to 8 hours.

4. The method for preparing a flame-retardant polyolefin cable insulation material according to claim 2, characterized in that: In step (II), the concentration of sodium dodecyl sulfate in the boron nitride stripping solution is 12 to 15 wt %; The concentration of fatty acid ethanolamide in the boron nitride stripping solution is 5 to 8 wt %; The concentration of sodium ethoxylate sulfonate in the boron nitride stripping solution is 4 to 5 wt %; The ratio of the boron nitride powder to the boron nitride stripping solution is 1 g: (30-40) mL; The power of ultrasonic dispersion after adding boron nitride powder to the boron nitride stripping solution is 1000-1200W, and the time of ultrasonic dispersion is 1-2h; The heating temperature after adding the boron nitride powder to the boron nitride stripping solution is 30 to 40° C.; The concentration of the sodium hydroxide solution is 3-8 mol / L; The mass ratio of the boron nitride nanosheets to the sodium hydroxide in the sodium hydroxide solution is 1:(15-25); The power of ultrasonic dispersion when the boron nitride nanosheets are mixed with the sodium hydroxide solution is 800-1000W, and the time of ultrasonic dispersion is 1-2h; The temperature of the hydrothermal reaction is 110-130°C; The hydrothermal reaction time is 24 to 48 hours.

5. The method for preparing a flame-retardant polyolefin cable insulation material according to claim 2, characterized in that: In step (III), the concentration of the hydroxyl-modified boron nitride nanosheets in the precursor solution is 10 to 20 g / L: The molar concentration of the zinc nitrate hexahydrate in the precursor solution is 1-2 mol / L: The molar concentration of the potassium hydroxide solution is 1-2 mol / L; The molar ratio of potassium hydroxide in the potassium hydroxide solution to zinc nitrate hexahydrate in the precursor solution is 2:1; The reaction time of the precursor solution and the potassium hydroxide solution is 3 to 4 hours; The mass ratio of the hexadecyltrimethylammonium bromide to the zinc nitrate hexahydrate is 1:(8-9); The heating temperature of the hydrothermal reaction is 120-130°C; The holding time of the hydrothermal reaction is 1 to 3 hours; The silane coupling agent solution is composed of a silane coupling agent and an ethanol aqueous solution, wherein the volume ratio of ethanol to deionized water in the ethanol aqueous solution is (8-9): (1-2); The mass fraction of the silane coupling agent in the silane coupling agent solution is 5 to 10 wt %; The composite boron nitride nanosheets are immersed in the silane coupling agent solution for 3 to 5 hours.

6. The method for preparing a flame-retardant polyolefin cable insulation material according to claim 2, characterized in that: In step (IV), the concentration of the Tris-hydrochloric acid buffer solution is 30-40 g / L; The concentration of dopamine in the dopamine solution is 1 to 5 g / L; The mass ratio of the nanocellulose powder to the dopamine in the dopamine solution is (4-5):1; The nanocellulose is immersed in the dopamine solution for 12 to 24 hours; The freeze drying temperature is -20 to -30°C; The freeze-drying time is 20 to 30 hours.

7. The method for preparing a flame-retardant polyolefin cable insulation material according to claim 2, characterized in that: In step (V), the stirring speed is 1200-1500 rpm; The stirring time is 5 to 10 minutes. n ; The weight parts of each component in the mixed masterbatch are as follows: The temperature of the first zone is 160-170°C; The temperature of the second zone is 170-180°C; The temperature of the third zone is 175-185°C; The temperature of the fourth zone is 185-195°C; The temperature of the fifth zone is 180-190°C; The screw speed of the screw extruder is 80-100 rpm.

8. A flame-retardant polyolefin cable insulation material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The flame-retardant polyolefin cable insulation material comprises low-density polyethylene, polypropylene, ethylene-vinyl acetate, grafted modified magnesium hydroxide powder, composite modified boron nitride nanosheets, modified nanocellulose, lubricant, antioxidant and plasticizer.

9. The flame-retardant polyolefin cable insulation material according to claim 8, characterized in that: The grafted modified magnesium hydroxide powder is prepared by sequentially modifying magnesium hydroxide with sodium oleate and then grafting with methyl methacrylate; The composite modified boron nitride nanosheets are prepared by sequentially subjecting boron nitride powder to ultrasonic exfoliation, sodium hydroxide hydroxyl modification, and zinc oxide in-situ loading. The modified nanocellulose is prepared by modifying nanocellulose powder with dopamine.

10. The flame-retardant polyolefin cable insulation material according to claim 8, characterized in that: The flame retardant polyolefin cable insulation material comprises the following components in parts by weight: The lubricant is any one of stearic acid, zinc stearate, calcium stearate, and polyethylene wax, or a combination of at least two thereof; The antioxidant is any one of antioxidant 1010, antioxidant 626, and antioxidant 168, or a combination of at least two thereof; The plasticizer is any one of glycerol, epoxidized soybean oil, and paraffin oil, or a combination of at least two of them.

Citation Information

Cited By

  • Inorganic anti-corrosion anti-freezing flame retardant and preparation method thereof

    CN119799050A

  • Preparation process of high-strength halogen-free flame-retardant electric wire

    CN120424439A

  • Preparation process of high-strength halogen-free flame-retardant electric wire

    CN120424439B

  • Cellulose composite waterproof flame retardant and preparation method thereof

    CN120443508A

  • Graphene aluminum alloy cable and preparation method thereof

    CN120511108A