Rice straw biomass carbon composite potassium polyacrylate water-retaining agent and preparation method thereof

By preparing a water-retaining agent composed of rice straw biomass carbon and potassium polyacrylate, the problems of short water retention time and low utilization rate of existing soil water-retaining agents were solved, achieving efficient soil water retention and improvement effects and reducing production costs.

CN118978779APending Publication Date: 2024-11-19SHAANXI UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411188232.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing soil water-retaining agents have insufficient water retention time and limited water retention rate, poor soil improvement properties, and low utilization rate of biomass waste, leading to serious problems of soil drought and compaction.

Method used

The preparation method of rice straw biomass carbon composite potassium polyacrylate water-retaining agent involves soaking crushed rice straw in an adhesive solution, carbonizing it, and then carrying out a hydrothermal reaction with a potassium acrylate mixed solution to form a porous water-retaining agent, which enhances adsorption and water retention.

Benefits of technology

It significantly improves the water absorption and retention capacity of water-retaining agents, prolongs water retention time, enhances soil water retention and fertility, improves soil structure, reduces production costs, and reduces the environmental burden of agricultural waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978779A_ABST
    Figure CN118978779A_ABST
Patent Text Reader

Abstract

The invention discloses a rice straw biomass carbon composite potassium polyacrylate water-retaining agent and a preparation method thereof, and belongs to the technical field of biomass materials.The preparation method comprises the steps that smashed and cleaned rice straw is soaked in an adhesive solution, and after standing, drying and carbonization, a carbonized product A is obtained; potassium acrylate powder and acrylic acid are mixed and dissolved in distilled water, a cross-linking agent and an initiator are added, and a mixed solution B is obtained after stirring reaction; slowly adding the carbonized product A into the mixed solution B, carrying out hydrothermal reaction, drying, grinding and sieving to obtain the rice straw biomass carbon composite potassium polyacrylate water-retaining agent. The waste rice straw is adopted as the raw material, so that the production cost of the water-retaining agent is greatly reduced; according to the invention, high-valued utilization of biomass resources is realized, the environmental burden of agricultural wastes is reduced, water can be slowly released under drought conditions, the water retention capacity of soil is improved, the structural stability is good, the mechanical strength is high, and the fertilizer has important significance for water-saving agriculture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomass materials, and particularly relates to a rice straw biomass carbon composite potassium polyacrylate water retaining agent and a preparation method thereof. Background Art

[0002] Soil drought occurs frequently in many places, especially due to insufficient precipitation and large daily evaporation of the land, which makes the soil prone to drought. In order to ensure the growth of crops, timely irrigation is required, which increases water consumption. On the other hand, due to the continuous use of chemical fertilizers, the soil becomes compacted, the soil voids decrease, and the water retention decreases, resulting in a decrease in crop yields. At the same time, rice is widely planted. As a by-product of rice, rice straw has abundant sources and low costs. At present, the main way to deal with rice straw is to burn it on the spot, which causes environmental pollution.

[0003] Research has found that rice straw has good fiber pipes. By using the adsorption principle of activated carbon and carbonizing rice straw, rice straw is transformed into a carbon material with a sponge-like structure, increasing the overall specific surface area and tubular structure of the material. By controlling the preparation process, the polarity of the material is increased, and the storage and adsorption of water molecules are enhanced. At present, similar soil water-retaining agents have the limitations of not retaining water for a long enough time, limited adsorption rate for water molecules, poor soil improvement, and low utilization rate of biological material waste.

[0004] In view of the technical problems that the water retention time of the existing technology is not long enough, the water retention rate needs to be further improved, the biomass waste is not effectively utilized, and long-term use will cause soil compaction, it is urgent to find a new water-retaining agent with developed pores, high adsorption capacity and long water retention time to improve the soil's water retention capacity and alleviate the drought problem. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a rice straw biomass carbon composite potassium polyacrylate water-retaining agent and a preparation method thereof, so as to solve the technical problems of enhancing the adsorption of water molecules, long-term water retention, enhancing the porous structure of the soil, and enhancing the adsorption of fertilizers.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The invention discloses a method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent, comprising:

[0008] The crushed and cleaned rice straw is immersed in an adhesive solution, and after standing, drying and carbonizing, a carbonized product A is obtained;

[0009] Potassium acrylate powder and acrylic acid are mixed and dissolved in distilled water, a crosslinking agent and an initiator are added, and after stirring and reacting, a mixed solution B is obtained;

[0010] The carbonized product A is slowly added into the mixed solution B to carry out a hydrothermal reaction, and then dried, ground and sieved to obtain a rice straw biomass carbon composite potassium polyacrylate water retaining agent.

[0011] Preferably, the mass ratio of the carbonized product A, potassium acrylate, acrylic acid, crosslinking agent and initiator is 1:(0.2-1):(0.2-1):(0.01-0.3):(0.02-0.18).

[0012] Preferably, the mass percentage of the adhesive solution is 0.5%-1.5%; the adhesive is any one of sodium carboxymethyl cellulose, polyvinylidene fluoride and polyvinyl alcohol.

[0013] Preferably, the crosslinking agent is any one of diethylenetriamine, N,N-dimethylformamide and N,N-methylenebisacrylamide; the initiator is any one of potassium persulfate, ammonium persulfate, ammonium persulfate-sodium bisulfite and 2-ketoglutaric acid.

[0014] Preferably, the standing time is 0.5-2h; the drying temperature is 50-70°C; and the drying time is 12-24h.

[0015] Preferably, the carbonization conditions are: in a nitrogen atmosphere, gradually raising the temperature to 1100-1400° C. at a rate of 10-30° C. / min, and keeping the temperature for 3-5 h.

[0016] Preferably, the stirring reaction conditions are: heating to 20-80° C. at a heating rate of 5-7° C. / min, and keeping warm for 1-4 h.

[0017] Preferably, the conditions of the hydrothermal reaction are: heating to 150-200° C. at a heating rate of 10-30° C. / min, and keeping the temperature for 3-5 h.

[0018] Preferably, the drying temperature is 60-70°C; and the sieving condition is 100-500 mesh.

[0019] The invention also discloses a rice straw biomass carbon composite potassium polyacrylate water retaining agent, which is prepared by adopting the above preparation method.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The invention discloses a method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent, wherein the rice straw after crushing and cleaning is soaked in an adhesive solution, and after standing, drying and carbonization, a carbonization product A is obtained; by soaking in an adhesive solution, not only the adhesion of the straw is enhanced, but also the subsequent combination with potassium polyacrylate is convenient, thereby improving the structural stability and mechanical strength of the composite material. Moreover, through carbonization treatment, the originally discarded straw is converted into biomass carbon with high carbon content and developed pore structure, realizing the high-value utilization of biomass resources and effectively reducing the burden of agricultural waste on the environment. The carbonization process also makes the internal pores of the biomass carbon more loose and unobstructed, thereby greatly increasing its adsorption rate and providing more water absorption sites for the water retaining agent. Potassium acrylate powder is mixed with acrylic acid and dissolved in distilled water, a crosslinking agent and an initiator are added, and a mixed solution B is obtained after stirring and reacting; by mixing potassium acrylate powder with acrylic acid, and adding a crosslinking agent and an initiator, a potassium polyacrylate solution with excellent water absorption and water retention capacity is formed after stirring and reacting. This provides a basis for the subsequent combination with the carbonized product A, ensuring that the water retainer has good water absorption and water retention. The carbonized product A is slowly added to the mixed solution B, a hydrothermal reaction is carried out, and after drying, grinding, and sieving, a rice straw biomass carbon composite polyacrylate potassium water retainer is obtained. Potassium polyacrylate has excellent water absorption and water retention capacity. By compounding with the carbonized product A, the prepared water retainer can slowly release water under drought conditions. By slowly adding the carbonized product A to the mixed solution B and carrying out a hydrothermal reaction, the two can be firmly combined to form a water retainer with excellent performance. Subsequent processing steps such as drying, grinding and sieving further improve the stability and mechanical strength of the water retainer. The water retainer finally obtained not only has excellent water absorption and water retention capacity, but also has strong adsorption to fertilizer particles, which is of great significance for improving soil water retention, maintaining fertility and improving soil.

[0022] The present invention also discloses a rice straw biomass carbon composite potassium polyacrylate water retaining agent prepared by the above-mentioned preparation method, which significantly reduces the production cost, converts the originally discarded straw into biomass carbon with high carbon content and developed pore structure, and realizes the high-value utilization of biomass resources, effectively reducing the burden of agricultural waste on the environment. Not only the adsorption capacity of the material is improved, but also the internal pores of the biomass carbon are made looser and smoother, thereby greatly increasing its adsorption rate. This porous structure provides more water absorption sites for the water retaining agent, making it perform well in retaining moisture. By introducing carboxymethyl cellulose (CMC) as an adhesive, the bonding ability between potassium polyacrylate and straw biomass carbon is improved. The addition of CMC enhances the structural stability of the composite material, significantly improves its mechanical strength, and improves the stability of the water retaining agent. The bond between biomass carbon and potassium polyacrylate is more firm, thereby effectively improving the grafting ability of the material. It shows good performance in water absorption, water retention and degradation, and can absorb water up to four times its own weight. It has a longer water retention time than existing water retaining agents (24h water retention rate of 83.6%), has strong adsorption capacity for fertilizer particles, and has a good effect and application scenario on improving soil water retention, maintaining fertility, and improving soil. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a comparison curve diagram of the water retention rate of the rice straw biomass carbon composite potassium polyacrylate water retaining agent prepared in Examples 1, 2 and 6 of the present invention and the carbonized product prepared in the comparative example;

[0024] Figure 2 This is a graph showing the water absorption performance of the rice straw biomass carbon composite potassium polyacrylate water retaining agent prepared in Examples 2 and 6 of the present invention and the carbonized product prepared in the comparative example;

[0025] Figure 3 The present invention provides scanning electron microscope images of the rice straw biomass carbon composite potassium polyacrylate water retaining agent prepared in Example 1 and Example 7 of the present invention; wherein, (a) is a 20,000-fold scanning image when the mass ratio of carbonized product A to potassium acrylate is 1 / 1; (b) is a 20,000-fold scanning image when the mass ratio of carbonized product A to potassium acrylate is 2 / 1; (c) is a 50,000-fold scanning image when the mass ratio of carbonized product A to potassium acrylate is 1 / 1; (d) is a 50,000-fold scanning image when the mass ratio of carbonized product A to potassium acrylate is 2 / 1. DETAILED DESCRIPTION

[0026] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0027] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0028] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0029] The invention discloses a method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent, which specifically comprises the following steps:

[0030] Weigh 5-15g of adhesive and add it to 1000ml of deionized water. Stir until completely dissolved to form a uniform 0.5%-1.5% solution. Take 1kg of rice straw material that has been crushed and dried using a grinder, rinse it with clean water, soak it in the prepared adhesive solution, and let it stand at room temperature for 0.5-2h. Then place it in an oven and dry it at 50-70℃ for 12-24h to remove moisture. Evenly spread the pretreated straw in a tubular furnace, introduce nitrogen into the tubular furnace and gradually heat it to 1100-1400℃ at a rate of 10-30℃ / min, maintain this temperature for 3-5h, and carbonize the straw. A carbonized product A with a high carbon content and developed pores is obtained.

[0031] 5-60g of potassium acrylate (SAP) powder and 5-60g of acrylic acid are mixed in distilled water, and 0.5-18g of crosslinking agent diethylenetriamine (DETA) and 1-8.8g of initiator potassium persulfate are added. After sufficient stirring, the mixture is heated to 20-80°C at a heating rate of 5-7°C / min using a thermostatic stirrer and maintained for 1-4h to ensure that the mixture is completely dissolved and reacted, and finally a uniform mixed solution B is formed.

[0032] Take 50-60g of the carbonized product A and slowly add it to the mixed solution B to obtain a mixed solution C, then add it to a high temperature resistant container and place the container in a hydrothermal kettle, and synthesize it by a hydrothermal method at 150-200°C with a heating rate of 10-30°C / min and keep it warm for 3-5 hours. Then dry it in an oven at 60-70°C, crush and grind the solid and sieve it through 100-500 mesh to obtain a solid rice straw biomass carbon composite potassium polyacrylate water retaining agent.

[0033] The binder is any one of sodium carboxymethyl cellulose, polyvinylidene fluoride and polyvinyl alcohol.

[0034] The cross-linking agent is any one of diethylenetriamine, N,N-dimethylformamide and N,N-methylenebisacrylamide.

[0035] The initiator is any one of potassium persulfate, ammonium persulfate, ammonium persulfate-sodium bisulfite and 2-oxoglutaric acid.

[0036] The mass ratio of carbonization product A to potassium acrylate is 1:(0.2-1).

[0037] The mass ratio of the carbonized product A to acrylic acid is 1:(0.2-1).

[0038] The mass ratio of the carbonized product A to the cross-linking agent is 1:(0.01-0.3).

[0039] The mass ratio of the carbonization product A to the initiator is: 1:(0.02-0.18).

[0040] The invention discloses a method for preparing a rice straw biomass carbon composite potassium polyacrylate water retainer, which is prepared by using rice straw-based biomass carbon and potassium polyacrylate as main raw materials, adding an adhesive, a crosslinking agent and an initiator for crosslinking polymerization. The invention uses discarded rice straw as raw material, which greatly reduces the production cost of the water retainer; the prepared degradable water retainer has good water absorption and degradation properties. Specifically, it has the following advantages:

[0041] 1. Efficient utilization of biomass carbon: By converting rice straw, an agricultural waste, into carbonized product A with high carbon content and developed pores, high-value utilization of biomass resources is achieved, reducing the environmental burden of agricultural waste.

[0042] 2. Enhanced water retention performance: Potassium polyacrylate (SAP) has excellent water absorption and water retention capacity. By compounding with carbonized product A, the prepared water retainer can slowly release water under drought conditions and improve the water retention capacity of the soil, which is of great significance for water-saving agriculture.

[0043] 3. Structural optimization: By introducing carboxymethyl cellulose (CMC) as a binder, the bonding ability of potassium polyacrylate and straw biomass carbon is enhanced, and the structural stability and mechanical strength of the composite material are improved.

[0044] The present invention also discloses a rice straw biomass carbon composite potassium polyacrylate water retaining agent prepared by the above preparation method.

[0045] See also Figure 1 The present invention provides a comparative curve diagram of the water retention rates of the rice straw biomass carbon composite potassium polyacrylate water retaining agent prepared in Examples 1, 2 and 6 of the present invention and the carbonized product prepared in the comparative example; as can be seen from the figure, when the amount of biomass porous carbon added and the amount of potassium polyacrylate added are 1:(0.2-1), the water retention time can reach a 24-hour water retention rate of 83.6%.

[0046] Figure 2 The water absorption performance diagram of the rice straw biomass carbon composite potassium polyacrylate water retaining agent prepared in Examples 2 and 6 of the present invention and the carbonized product prepared in the comparative example; Figure 2 It can be seen that when the amount of added carbonized product is similar to that of potassium polyacrylate, the water absorption increases significantly.

[0047] Figure 3 The scanning electron microscope images of the rice straw biomass carbon composite potassium polyacrylate water retaining agent prepared in Example 1 and Example 7 of the present invention; wherein, (a) is a 20,000-fold scanning image when the carbonization product / potassium acrylate is 1 / 1; (b) is a 20,000-fold scanning image when the mass ratio of carbonization product A / potassium acrylate is 2 / 1; (c) is a 50,000-fold scanning image when the carbonization product / potassium acrylate is 1 / 1; (d) is a 50,000-fold scanning image when the mass ratio of carbonization product A / potassium acrylate is 2 / 1; it can be seen that more potassium polyacrylate SAP is attached to the porous carbon surface. Since the porous carbon has a larger surface area and more active sites, more SAP is attached to the surface. It can be seen from the figure that the SAP on the porous carbon grows larger, providing a larger surface area and better water holding capacity.

[0048] Example 1

[0049] A method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent comprises the following steps:

[0050] Weigh 5g of the adhesive sodium carboxymethyl cellulose and add it to 1000ml of deionized water. Stir until completely dissolved to form a uniform 0.5% solution. Take 1kg of rice straw material that has been crushed and dried using a grinder, rinse it with clean water, soak it in the prepared adhesive solution, and let it stand at room temperature for 2h. Then place it in an oven and dry it at 50℃ for 24h to remove moisture. Evenly spread the pretreated straw in a tubular furnace, introduce nitrogen into the tubular furnace and gradually raise the temperature to 1100℃ at a rate of 10℃ / min, maintain this temperature for 5h, and carbonize the straw. A carbonized product A with a high carbon content and developed pores is obtained.

[0051] 10g of potassium acrylate (SAP) powder and 10g of acrylic acid were mixed in distilled water, and 0.2g of crosslinking agent diethylenetriamine (DETA) and 0.4g of initiator potassium persulfate were added. After sufficient stirring, the mixture was heated to 80°C at a heating rate of 5°C / min using a constant temperature stirrer and maintained for 4h to ensure that the mixture was completely dissolved and reacted, and finally a uniform mixed solution B was formed.

[0052] Take 20g of the carbonized product A and slowly add it to the mixed solution B to obtain a mixed solution C, which is then added to a high temperature resistant container and placed in a hydrothermal kettle. The temperature is raised to 200°C at a heating rate of 10°C / min by a hydrothermal method and kept warm for 3 hours for synthesis. It is then dried in an oven at 60°C, ground and sieved through 100 mesh to obtain a solid rice straw biomass carbon composite potassium polyacrylate water retaining agent.

[0053] Example 2

[0054] A method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent comprises the following steps:

[0055] Weigh 10g of adhesive polyvinylidene fluoride and add it to 1000ml of deionized water. Stir until completely dissolved to form a uniform 1% solution. Take 1kg of rice straw material that has been crushed and dried using a grinder, rinse it with clean water, soak it in the prepared adhesive solution, and let it stand at room temperature for 0.5h. Then place it in an oven and dry it at 65℃ for 16h to remove moisture. Evenly spread the pretreated straw in a tubular furnace, introduce nitrogen into the tubular furnace and gradually heat it to 1300℃ at a rate of 15℃ / min, maintain this temperature for 3h, and carbonize the straw. A carbonized product A with a high carbon content and developed pores is obtained.

[0056] 50g of potassium acrylate (SAP) powder and 50g of acrylic acid were mixed in distilled water, and 0.5g of crosslinking agent N,N-dimethylformamide and 0.1g of initiator ammonium persulfate were added. After sufficient stirring, the mixture was heated to 50°C at a heating rate of 7°C / min using a thermostatic stirrer and maintained for 2h to ensure that the mixture was completely dissolved and reacted, and finally a uniform mixed solution B was formed.

[0057] Take 50g of the carbonized product A and slowly add it to the mixed solution B to obtain a mixed solution C, which is then added to a high temperature resistant container and placed in a hydrothermal kettle. The temperature is raised to 150°C by a hydrothermal method at a heating rate of 25°C / min and kept warm for 3 hours for synthesis. It is then dried in an oven at 70°C, the ground solid is sieved through 100 mesh, and the solid is obtained as a rice straw biomass carbon composite potassium polyacrylate water retaining agent.

[0058] Example 3

[0059] A method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent comprises the following steps:

[0060] Weigh 15g of adhesive polyvinyl alcohol and add it to 1000ml of deionized water. Stir until completely dissolved to form a uniform 1.5% solution. Take 1kg of rice straw material that has been crushed and dried using a grinder, rinse it with clean water, soak it in the prepared adhesive solution, and let it stand at room temperature for 2h. Then place it in an oven and dry it at 70℃ for 12h to remove moisture. Evenly spread the pretreated straw in a tubular furnace, introduce nitrogen into the tubular furnace and gradually heat it to 1200℃ at a rate of 30℃ / min, maintain this temperature for 3h, and carbonize the straw. A carbonized product A with a high carbon content and developed pores is obtained.

[0061] 60g of potassium acrylate (SAP) powder and 60g of acrylic acid were mixed in distilled water, and 12g of crosslinking agent N,N-methylenebisacrylamide and 10g of initiator ammonium persulfate-sodium bisulfite were added. After sufficient stirring, the mixture was heated to 70°C at a heating rate of 7°C / min using a thermostatic stirrer and maintained for 2h to ensure that the mixture was completely dissolved and reacted, and finally a uniform mixed solution B was formed.

[0062] 60g of the carbonized product A was slowly added to the mixed solution B to obtain a mixed solution C, which was then added to a high temperature resistant container and placed in a hydrothermal kettle. The temperature was raised to 200°C by a hydrothermal method at a heating rate of 20°C / min and kept for 5 hours for synthesis. The product was then dried in an oven at 70°C, ground and sieved through 400 mesh to obtain a solid rice straw biomass carbon composite potassium polyacrylate water retaining agent.

[0063] Example 4

[0064] A method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent comprises the following steps:

[0065] Weigh 10g of the adhesive sodium carboxymethyl cellulose and add it to 1000ml of deionized water. Stir until completely dissolved to form a uniform 1% solution. Take 1kg of rice straw material that has been crushed and dried using a grinder, rinse it with clean water, soak it in the prepared adhesive solution, and let it stand at room temperature for 2h. Then place it in an oven and dry it at 70℃ for 12h to remove moisture. Evenly spread the pretreated straw in a tubular furnace, introduce nitrogen into the tubular furnace and gradually heat it to 1400℃ at a rate of 20℃ / min, maintain this temperature for 3h, and carbonize the straw. A carbonized product A with a high carbon content and developed pores is obtained.

[0066] 20g of potassium acrylate (SAP) powder and 20g of acrylic acid were mixed in distilled water, and 0.5g of crosslinking agent diethylenetriamine (DETA) and 1g of initiator 2-ketoglutaric acid were added. After sufficient stirring, the mixture was heated to 60°C at a heating rate of 5°C / min using a thermostatic stirrer and maintained for 2h to ensure that the mixture was completely dissolved and reacted, and finally a uniform mixed solution B was formed.

[0067] Take 20g of the carbonized product A and slowly add it to the mixed solution B to obtain a mixed solution C, which is then added to a high temperature resistant container and placed in a hydrothermal kettle. The temperature is raised to 150°C by a hydrothermal method at a heating rate of 30°C / min and kept warm for 3 hours for synthesis. It is then dried in an oven at 60°C, and the ground solid is sieved through 300 mesh to obtain a solid rice straw biomass carbon composite potassium polyacrylate water retaining agent.

[0068] Example 5

[0069] A method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent comprises the following steps:

[0070] Weigh 15g of the adhesive sodium carboxymethyl cellulose and add it to 1000ml of deionized water. Stir until completely dissolved to form a uniform 1.5% solution. Take 1kg of rice straw material that has been crushed and dried using a grinder, rinse it with clean water, soak it in the prepared adhesive solution, and let it stand at room temperature for 2h. Then place it in an oven and dry it at 70℃ for 12h to remove moisture. Evenly spread the pretreated straw in a tubular furnace, introduce nitrogen into the tubular furnace and gradually heat it to 1200℃ at a rate of 20℃ / min, maintain this temperature for 4h, and carbonize the straw. A carbonized product A with a high carbon content and developed pores is obtained.

[0071] 20g of potassium acrylate (SAP) powder and 20g of acrylic acid were mixed in distilled water, and 2g of crosslinking agent diethylenetriamine (DETA) and 3g of initiator potassium persulfate were added. After sufficient stirring, the mixture was heated to 20°C at a heating rate of 5°C / min using a thermostatic stirrer and maintained for 1h to ensure that the mixture was completely dissolved and reacted, and finally a uniform mixed solution B was formed.

[0072] Take 20g of carbonized product A and slowly add it to mixed solution B to obtain mixed solution C, then add it to a high temperature resistant container and place the container in a hydrothermal kettle, heat it to 200°C at a heating rate of 20°C / min by hydrothermal method, and keep it warm for 3h to synthesize. Then dry it in an oven at 70°C, crush and grind the solid and sieve it through 500 mesh to obtain a solid rice straw biomass carbon composite potassium polyacrylate water retaining agent.

[0073] Example 6

[0074] A method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent comprises the following steps:

[0075] Weigh 12g of adhesive sodium carboxymethyl cellulose and add it to 1000ml of deionized water. Stir until completely dissolved to form a uniform 1.2% solution. Take 1kg of rice straw material that has been crushed and dried using a grinder, rinse it with clean water, soak it in the prepared adhesive solution, and let it stand at room temperature for 1h. Then place it in an oven and dry it at 55°C for 20h to remove moisture. Evenly spread the pretreated straw in a tubular furnace, introduce nitrogen into the tubular furnace and gradually heat it to 1200°C at a rate of 25°C / min, maintain this temperature for 4h, and carbonize the straw. A carbonized product A with a high carbon content and developed pores is obtained.

[0076] 5g of potassium acrylate (SAP) powder and 5g of acrylic acid were mixed in distilled water, and 0.6g of crosslinking agent diethylenetriamine (DETA) and 0.36g of initiator potassium persulfate were added. After sufficient stirring, the mixture was heated to 40°C at a heating rate of 6°C / min using a thermostatic stirrer and maintained for 3h to ensure that the mixture was completely dissolved and reacted, and finally a uniform mixed solution B was formed.

[0077] Take 25g of carbonized product A and slowly add it to mixed solution B to obtain mixed solution C, then add it to a high temperature resistant container and place the container in a hydrothermal kettle, heat it to 180°C at a heating rate of 15°C / min by hydrothermal method, and keep it warm for 4 hours to synthesize. Then dry it in an oven at 65°C, crush and grind the solid and sieve it through 200 mesh to obtain a solid rice straw biomass carbon composite potassium polyacrylate water retaining agent.

[0078] Example 7

[0079] A method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent comprises the following steps:

[0080] Weigh 15g of the adhesive sodium carboxymethyl cellulose and add it to 1000ml of deionized water. Stir until completely dissolved to form a uniform 1.5% solution. Take 1kg of rice straw material that has been crushed and dried using a grinder, rinse it with clean water, soak it in the prepared adhesive solution, and let it stand at room temperature for 2h. Then place it in an oven and dry it at 60℃ for 18h to remove moisture. Evenly spread the pretreated straw in a tubular furnace, introduce nitrogen into the tubular furnace and gradually heat it to 1200℃ at a rate of 20℃ / min, maintain this temperature for 4h, and carbonize the straw. A carbonized product A with a high carbon content and developed pores is obtained.

[0081] 60g of potassium acrylate (SAP) powder and 60g of acrylic acid were mixed in distilled water, and 18g of crosslinking agent diethylenetriamine (DETA) and 8.8g of initiator potassium persulfate were added. After sufficient stirring, the mixture was heated to 30°C at a heating rate of 5°C / min using a thermostatic stirrer and maintained for 1h to ensure that the mixture was completely dissolved and reacted, and finally a uniform mixed solution B was formed.

[0082] 60g of carbonized product A was slowly added to mixed solution B to obtain mixed solution C, which was then added to a high temperature resistant container and placed in a hydrothermal kettle. The mixture was heated to 190°C at a heating rate of 20°C / min by a hydrothermal method and kept warm for 3 hours for synthesis. The mixture was then dried in an oven at 70°C, ground and sieved through 500 mesh to obtain a solid rice straw biomass carbon composite potassium polyacrylate water retaining agent.

[0083] Comparative Example (Blank)

[0084] Take 1kg of rice straw material that was crushed and dried using a pulverizer, rinse it with clean water, and then place it in an oven at 70°C for 24 hours to remove moisture. The pretreated straw was evenly spread in a tubular furnace, and nitrogen was introduced into the tubular furnace to gradually increase the temperature to 1400°C at a rate of 10°C / min. This temperature was maintained for 5 hours to carbonize the straw, and a carbonized product with a high carbon content and developed pores was obtained.

[0085] The present invention uses rice straw as a raw material to convert it into a highly efficient water-retaining agent, which significantly reduces production costs. By mixing these agricultural wastes with an adhesive and then carbonizing them in a tubular furnace, the originally discarded straw is converted into biomass carbon with a high carbon content and a developed pore structure, and the high-value utilization of biomass resources is achieved, effectively reducing the burden of agricultural waste on the environment. Not only does it improve the adsorption capacity of the material, but it also makes the internal pores of the biomass carbon looser and more unobstructed, thereby greatly increasing its adsorption rate. This porous structure provides more water absorption sites for the water-retaining agent, making it perform well in retaining moisture. It can significantly improve the water retention rate and water retention time of the water-retaining agent, restore the porous structure of the soil, utilize the natural degradation of biomass materials, reduce soil compaction, and improve the water absorption and fertility absorption of the soil.

[0086] The present invention improves the bonding ability between potassium polyacrylate and straw biomass carbon by introducing carboxymethyl cellulose (CMC) as an adhesive. The addition of CMC enhances the structural stability of the composite material, significantly improves its mechanical strength, and improves the stability of the water retaining agent. The bond between biomass carbon and potassium polyacrylate is more firm, thereby effectively improving the grafting ability of the material. The water retaining agent prepared by the method of the present invention exhibits good performance in terms of water absorption, water retention and degradation performance.

[0087] The rice straw biomass carbon composite potassium polyacrylate water retaining agent prepared in the embodiment of the present invention has a water absorption multiple of up to four times its own weight; the water retention time is longer than that of the existing water retaining agent (24h water retention rate is 83.6%), and it has a strong adsorption capacity for fertilizer particles, and has a good effect and application scenario on improving soil water retention, maintaining fertility, and improving soil.

[0088] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a rice straw biomass carbon composite potassium polyacrylate water retaining agent, characterized in that: include: The crushed and cleaned rice straw is immersed in an adhesive solution, and after standing, drying and carbonizing, a carbonized product A is obtained; Potassium acrylate powder and acrylic acid are mixed and dissolved in distilled water, a crosslinking agent and an initiator are added, and after stirring and reacting, a mixed solution B is obtained; The carbonized product A is slowly added into the mixed solution B to carry out a hydrothermal reaction, and then dried, ground and sieved to obtain a rice straw biomass carbon composite potassium polyacrylate water retaining agent.

2. The method for preparing the rice straw biomass carbon composite potassium polyacrylate water retaining agent according to claim 1, characterized in that: The mass ratio of the carbonized product A, potassium acrylate, acrylic acid, crosslinking agent and initiator is 1:(0.2-1):(0.2-1):(0.01-0.3):(0.02-0.18).

3. The method for preparing the rice straw biomass carbon composite potassium polyacrylate water retaining agent according to claim 1, characterized in that: The mass percentage of the adhesive solution is 0.5%-1.5%; the adhesive is any one of sodium carboxymethyl cellulose, polyvinylidene fluoride and polyvinyl alcohol.

4. The method for preparing the rice straw biomass carbon composite potassium polyacrylate water retaining agent according to claim 1, characterized in that: The crosslinking agent is any one of diethylenetriamine, N,N-dimethylformamide and N,N-methylenebisacrylamide; the initiator is any one of potassium persulfate, ammonium persulfate, ammonium persulfate-sodium bisulfite and 2-ketoglutaric acid.

5. The method for preparing the rice straw biomass carbon composite potassium polyacrylate water retaining agent according to claim 1, characterized in that: The standing time is 0.5-2h; the drying temperature is 50-70°C; and the drying time is 12-24h.

6. The method for preparing the rice straw biomass carbon composite potassium polyacrylate water retaining agent according to claim 1, characterized in that: The carbonization conditions are: in a nitrogen atmosphere, gradually heating to 1100-1400° C. at a rate of 10-30° C. / min, and keeping the temperature for 3-5 hours.

7. The method for preparing the rice straw biomass carbon composite potassium polyacrylate water retaining agent according to claim 1, characterized in that: The stirring reaction conditions are: heating to 20-80° C. at a heating rate of 5-7° C. / min and keeping warm for 1-4 h.

8. The method for preparing the rice straw biomass carbon composite potassium polyacrylate water retaining agent according to claim 1, characterized in that: The conditions of the hydrothermal reaction are: heating to 150-200° C. at a heating rate of 10-30° C. / min and keeping the temperature for 3-5 hours.

9. The method for preparing the rice straw biomass carbon composite potassium polyacrylate water retaining agent according to claim 1, characterized in that: The drying temperature is 60-70°C; the sieving condition is 100-500 mesh.

10. A rice straw biomass carbon composite potassium polyacrylate water retaining agent, characterized in that: The method is prepared by any one of claims 1 to 9.

Citation Information

Patent Citations

  • Crop straw active carbon fiber production method

    CN104131364A

  • Rice husk carbon-based water retention agent preparation method and rice husk carbon-based water retention agent

    CN105131208A

  • Method for directly preparing functional biochar through straw pyrolysis

    CN107500265A

  • Biocarbon blends with optimized fixed carbon content, and methods for making and using the same