Shell powder / PBAT composite material and preparation method thereof
By using polyurethane prepolymer PBAPU as a compatibilizer in shell powder/PBAT composite materials, physical crosslinking and covalent bonds are formed, the problem of poor interface compatibility of materials is solved, the mechanical properties and toughness are significantly improved, and the further development is achieved. Good application potential.
Patent Information
- Application Number
- CN202410904089.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-19
AI Technical Summary
The mechanical properties of existing shell powder/PBAT composites are limited by the poor interface compatibility of shell powder fillers and PBAT matrix and the serious agglomeration, resulting in limited potential applications.
The polyurethane prepolymer PBAPU is used as a compatibilizer to form physical crosslinking with the PBAT matrix and form covalent bonds with the active groups in the shell powder to improve interface compatibility and enhance the mechanical properties of the composite material.
The elongation and mechanical properties of shell powder/PBAT composite materials are significantly improved, better compatibility and toughness are achieved, and the overall performance of the material is enhanced.
Smart Images

Figure CN118978793A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of composite materials, and in particular relates to a shell powder / PBAT composite material and a preparation method thereof. Background Art
[0002] Polybutylene adipate / terephthalate (PBAT) is a thermoplastic polymer made by direct polycondensation or chain extension polymerization. Its main raw materials are terephthalic acid, adipic acid, and 1,4-butanediol. It has both good mechanical properties and excellent biodegradability, and is one of the most popular and best biodegradable materials in the research of biodegradable plastics. It is mainly used to make film bag products, but the high cost of PBAT limits its industrial application. Therefore, how to reduce production costs and improve mechanical properties while maintaining the excellent properties of PBAT has become a key research issue in academia. Many researchers have explored the co-modification of PBAT, among which the co-modification of inorganic filler CaCO3 and PBAT is very popular.
[0003] The document "Study on Mechanical Properties of PBAT / CaCO3 Composite Materials" records that with the increase of CaCO3 content, the mechanical properties of the composite material change significantly, and the tensile strength first undergoes an increase process, and then gradually decreases. This is because in the blending system, a small amount of CaCO3 can increase the tensile strength of PBAT after addition due to its small particle size and high activation energy. With the increase of the filling amount, due to the poor compatibility of CaCO3 and PBAT, high content of CaCO3 will cause uneven dispersion and cluster distribution, resulting in decreased mechanical properties, affecting the mechanical properties and practicality of the product. Therefore, it is necessary to seek fillers with better compatibility on the basis of having the strength of CaCO3. Shell is a natural polymer containing a composite structure of CaCO3 and proteoglycan. On the basis of meeting the strength requirements, there are some organic groups that can be better compatible with PBAT. Therefore, shells can replace pure CaCO3 to become a more excellent performance agent, and it is green and environmentally friendly.
[0004] The invention patent of application number CN202210619325.2 discloses a fully biodegradable composite material and its preparation method. The preparation steps are as follows: PBAT and shell powder are mixed and stirred in a mass ratio of 100: (10-50) to obtain a mixture; the mixture is melt blended, extruded into strips, cooled, pelletized, and dried in sequence to obtain a PBAT / shell powder composite masterbatch; the PBAT / shell powder composite masterbatch is injection molded to obtain a fully biodegradable composite material; the method uses natural shells (such as oyster shells, etc.) as raw materials, utilizes the low price of shell powder, reduces costs, and improves the modulus and hardness of the PBAT matrix. The composite material is a fully biodegradable plastic. However, there are still problems such as poor interface compatibility and serious agglomeration between shell powder filler and matrix, which leads to unsatisfactory mechanical properties of the composite material and limits its potential application. Summary of the invention
[0005] The purpose of the present invention is to provide a shell powder / PBAT composite material and a method for using the shell powder / PBAT composite material to improve the interface compatibility between the shell powder filler and the PBAT matrix, in order to achieve the purpose of strengthening and toughening the shell powder / PBAT composite material.
[0006] To achieve the above objectives, the technical solution of the present invention is as follows:
[0007] In a first aspect, the present invention provides a shell powder / PBAT composite material, wherein the raw materials of the shell powder / PBAT composite material include: polybutylene adipate / terephthalate PBAT, shell powder, and polyurethane prepolymer PBAPU; wherein the polyurethane prepolymer PBAPU is obtained by reacting polybutylene adipate diol PBA and hexamethylene-1,6-diisocyanate HDI.
[0008] The mass ratio of the polybutylene adipate / terephthalate PBAT, shell powder and polyurethane prepolymer PBAPU is 50-90:10-50:1-5.
[0009] The mass ratio of the polybutylene adipate diol PBA to hexamethylene-1,6-diisocyanate HDI is 13.9-18.5:1.
[0010] In a second aspect, the present invention provides a method for preparing a shell powder / PBAT composite material, the preparation method comprising the following steps:
[0011] S1, mixing polybutylene adipate diol PBA and hexamethylene-1,6-diisocyanate HDI, and reacting to obtain a polyurethane prepolymer PBAPU;
[0012] S2. First, fully mix polybutylene adipate / terephthalate PBAT and shell powder in a desired proportion, and then fully mix the obtained mixture with polyurethane prepolymer PBAPU in a desired proportion to obtain a shell powder / PBAT composite material.
[0013] The mass ratio of the polybutylene adipate / terephthalate PBAT, shell powder and polyurethane prepolymer PBAPU is 50-90:10-50:1-5.
[0014] The mass ratio of the polybutylene adipate diol PBA to hexamethylene-1,6-diisocyanate HDI is 13.9-18.5:1.
[0015] In the step S1, the reaction temperature is 75-85°C;
[0016] In step S2, the mixing temperature is 150-170°C.
[0017] The preparation method further comprises an impurity removal step, which is located before step S1. The impurity removal step is specifically as follows: stirring polybutylene adipate diol PBA under vacuum and 80-100° C. for 0.5-1.5 h.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The raw materials of a shell powder / PBAT composite material of the present invention include: polybutylene adipate / terephthalate PBAT, shell powder, and polyurethane prepolymer PBAPU; the polyurethane prepolymer PBAPU is obtained by reacting polybutylene adipate diol PBA and hexamethylene-1,6-diisocyanate HDI; in the above design, the polyurethane prepolymer PBAPU uses PBA diol having a structural unit similar to that of polybutylene adipate / terephthalate PBAT as a soft segment structure, and uses the polyurethane prepolymer PBAPU having such a soft segment structure as a compatibilizer, which can form physical crosslinks with the PBAT matrix continuous phase through the similar compatibility principle on the one hand, and form covalent bonds with active groups such as -OH and -NH2 in the shell powder through the -NCO group on the other hand, thereby achieving the purpose of improving the interface compatibility, and playing the role of strengthening and toughening the shell powder / PBAT composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is the reaction principle diagram of the present invention. DETAILED DESCRIPTION
[0021] The present invention is further described in detail below in conjunction with specific implementations and drawings.
[0022] Table 1 Chemical reagents
[0023]
[0024] Embodiment 1:
[0025] The raw material composition of a shell powder / PBAT composite material includes: 50 parts of polybutylene adipate / terephthalate PBAT, 10 parts of shell powder, and 1 part of polyurethane prepolymer PBAPU; wherein the polyurethane prepolymer PBAPU is obtained by reacting 13.9 parts of polybutylene adipate diol PBA and 1 part of hexamethylene-1,6-diisocyanate HDI. The shell powder / PBAT composite material has the following characteristics: Figure 1 The composite structure shown.
[0026] The preparation method of the above-mentioned shell powder / PBAT composite material is carried out in the following steps:
[0027] S1. Add hexamethylene-1,6-diisocyanate HDI to the polybutylene adipate diol PBA after impurities are removed according to the required proportion, stir at 800r / min and 80°C for 1h, and react to obtain a colorless, transparent and viscous polyurethane prepolymer PBAPU, remove the air in the polyurethane prepolymer PBAPU, and cool it for standby use; wherein the impurity removal step is specifically as follows: first set the oil bath temperature to 100°C, stir at 200r / min under vacuum conditions until the polybutylene adipate diol PBA melts from a waxy solid into a colorless, transparent liquid and the oil bath temperature rises to 80°C, then adjust the speed to 300r / min, continue stirring for 1h, and finally cool to 50°C;
[0028] S2. Set the temperature of the internal mixer to 160°C. When the temperature of each plate of the internal mixer rises to 160°C, first mix polybutylene adipate / terephthalate PBAT and shell powder in the required proportion and pour them into the internal mixer, and adjust the speed of the internal mixer to 10r / min; then put the polyurethane prepolymer PBAPU into the internal mixer in the required proportion, adjust the speed of the internal mixer to 34r / min, and obtain the shell powder / PBAT composite material after sufficient stirring.
[0029] Embodiment 2:
[0030] The difference from Example 1 is that:
[0031] 90 parts of polybutylene adipate / terephthalate PBAT, 50 parts of shell powder, and 5 parts of polyurethane prepolymer PBAPU;
[0032] The polybutylene adipate diol PBA comprises 18.5 parts and hexamethylene-1,6-diisocyanate HDI comprises 1 part.
[0033] Embodiment 3:
[0034] The difference from Example 1 is that:
[0035] 60 parts of polybutylene adipate / terephthalate PBAT, 20 parts of shell powder, and 2 parts of polyurethane prepolymer PBAPU;
[0036] The polybutylene adipate diol PBA is 14.9 parts, and the hexamethylene-1,6-diisocyanate HDI is 1 part.
[0037] Embodiment 4:
[0038] The difference from Example 1 is that:
[0039] 70 parts of polybutylene adipate / terephthalate PBAT, 30 parts of shell powder, and 3 parts of polyurethane prepolymer PBAPU;
[0040] The polybutylene adipate diol PBA is 15.9 parts, and the hexamethylene-1,6-diisocyanate HDI is 1 part.
[0041] Embodiment 5:
[0042] The difference from Example 1 is that:
[0043] 80 parts of polybutylene adipate / terephthalate PBAT, 40 parts of shell powder, and 4 parts of polyurethane prepolymer PBAPU;
[0044] The polybutylene adipate diol PBA is 16.9 parts, and the hexamethylene-1,6-diisocyanate HDI is 1 part.
[0045] Performance Verification:
[0046] The shell powder / PBAT composite material of Example 1 was used as a test example, the composite material obtained by simply compounding shell powder with PBAT without adding a compatibilizer was used as Comparative Example 1, the composite material obtained by compounding shell powder with PBAT and adding deactivated PBAPU (deactivated PBAPU is obtained by reacting PBAPU with ethanol and water, consuming the active group NCO and then drying it) was used as Comparative Example 2, and the composite material obtained by compounding shell powder with PBAT and adding other compatibilizers (MDI and PBA are synthesized, and the synthesis steps are the same as S1 in Example 1) was used as Comparative Example 3, and the mechanical properties were compared. The comparison results are shown in Table 2:
[0047] Table 2 Mechanical properties of test examples and comparative examples 1-3
[0048]
[0049]
[0050] As shown in Table 2, the elongation at break of the test example is the highest, up to 365.72%. This is mainly because the -NCO group in the PBAPU polyurethane prepolymer reacts with the -OH group on the shell powder to form an urethane bond, resulting in a strong chemical crosslinking, showing a good elongation at break; in contrast, the elongations at break of Comparative Examples 1 and 2 are only 57.80% and 98.84%, respectively. Comparative Example 1 does not add a compatibilizer, and its elongation at break is the worst, which shows that the compatibilization of PBAPU significantly improves the elongation at break. Comparative Example 2 uses the deactivated PBAPU without NCO groups as a compatibilizer, and its elongation at break is only slightly higher than that of Comparative Example 1, but much lower than that of the test example, further illustrating the importance of the NCO active group in the compatibilizer. In addition, Comparative Example 3 uses a material synthesized from MDI and PBA as a compatibilizer, and its elongation at break is not as good as that of the test example. It can be seen that the MDI molecule, which mainly contains a rigid structure of benzene rings, has a poorer compatibilization effect on the PBAT matrix than the HDI molecule with a flexible long-chain structure.
Claims
1. A shell powder / PBAT composite material, Features: The raw materials of the shell powder / PBAT composite material include: polybutylene adipate / terephthalate PBAT, shell powder, and polyurethane prepolymer PBAPU; wherein the polyurethane prepolymer PBAPU is obtained by reacting polybutylene adipate diol PBA and hexamethylene-1,6-diisocyanate HDI.
2. A shell powder / PBAT composite material according to claim 1, Features: The mass ratio of the polybutylene adipate / terephthalate PBAT, shell powder and polyurethane prepolymer PBAPU is 50-90:10-50:1-5.
3. A shell powder / PBAT composite material according to claim 1 or 2, Features: The mass ratio of the polybutylene adipate diol PBA to hexamethylene-1,6-diisocyanate HDI is 13.9-18.5:
1.
4. A method for preparing a shell powder / PBAT composite material, Features: The preparation method comprises the following steps: S1, mixing polybutylene adipate diol PBA and hexamethylene-1,6-diisocyanate HDI, and reacting to obtain a polyurethane prepolymer PBAPU; S2. First, fully mix polybutylene adipate / terephthalate PBAT and shell powder in a desired proportion, and then fully mix the obtained mixture with polyurethane prepolymer PBAPU in a desired proportion to obtain a shell powder / PBAT composite material.
5. A method for preparing a shell powder / PBAT composite material according to claim 4, Features: The mass ratio of the polybutylene adipate / terephthalate PBAT, shell powder and polyurethane prepolymer PBAPU is 50-90:10-50:1-5.
6. A method for preparing a shell powder / PBAT composite material according to claim 4 or 5, Features: The mass ratio of the polybutylene adipate diol PBA to hexamethylene-1,6-diisocyanate HDI is 13.9-18.5:
1.
7. A method for preparing a shell powder / PBAT composite material according to claim 4 or 5, Features: In the step S1, the reaction temperature is 75-85°C; In step S2, the mixing temperature is 150-170°C.
8. A method for preparing a shell powder / PBAT composite material according to claim 4 or 5, Features: The preparation method further comprises an impurity removal step, which is located before step S1. The impurity removal step is specifically as follows: stirring polybutylene adipate diol PBA under vacuum and 80-100° C. for 0.5-1.5 h.