High-strength stable PC / PBT alloy material and preparation method thereof
By using a combination of silicon-containing polycarbonate and weather-resistant toughening compatible modifier in PC/PBT alloys, the problem of insufficient cold resistance, weather resistance and hydrolysis resistance of materials is solved, and higher weather resistance and resistance are achieved Hydrolysis performance is suitable for high-performance materials needs in the new energy field.
Patent Information
- Application Number
- CN202411286158.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The existing PC/PBT alloys have shortcomings in terms of cold resistance, weather resistance and hydrolysis resistance, and are difficult to meet high-performance needs such as the new energy field.
Using a combination of silicon-containing polycarbonate and weather-resistant toughening compatible modifiers AES-g-GMA or EPDM-co-SAG, the weather resistance and hydrolysis resistance of the material are improved through the modification process, and the epoxy expansion is used. Ingredients such as chain agent and carbodiimide form a stable structure to improve the durability of the material.
It significantly improves the weather resistance, hydrolysis resistance and low temperature resistance of the material, extends its service life, is suitable for high-temperature and high-humidity environments, and meets the high-performance requirements in new energy and other fields.
Smart Images

Figure BDA0005043161040000021 
Figure BDA0005043161040000031 
Figure BDA0005043161040000032
Abstract
Description
Technical Field
[0001] The invention relates to a high-strength and stable PC / PBT alloy material and a preparation method thereof, belonging to the technical field of alloy material processing. Background Art
[0002] Polycarbonate, as an engineering plastic, generally refers to aromatic polycarbonate in amorphous copolymers. Its special molecular structure gives it excellent comprehensive properties, such as high impact resistance and creep resistance, excellent rigidity and good dimensional stability, and can meet certain low temperature resistance requirements. However, PC also has many shortcomings, such as poor fluidity and difficulty in processing into thin-walled parts, sensitivity to notches, prone to stress cracking, poor solvent resistance and wear resistance, etc.
[0003] As a semi-crystalline engineering plastic, polybutylene terephthalate has good processing fluidity and excellent chemical resistance, but it has a large molding shrinkage, a low glass transition temperature and poor heat resistance. Therefore, the PC / PBT alloy prepared by blending polycarbonate and polybutylene terephthalate has the advantages of dimensional stability, easy processing, high rigidity, creep resistance, heat resistance and chemical resistance.
[0004] Although PC / PBT alloy has the above advantages, it still has deficiencies in weather resistance, cold resistance and hydrolysis resistance. For example, Chinese patent CN104927335 discloses a high-toughness and high-heat-resistant PC / PBT resin composition. In this method, an acrylic toughening agent is selected, and the heat resistance and weather resistance need to be improved. In addition, during processing and use, the toughening agent will decompose small molecular substances that promote the ester exchange of the PC / PBT resin composition, reduce the material performance, and it is difficult to meet the use under long-term high and low temperature and high weather resistance conditions;
[0005] Chinese patent CN109265955 discloses a high-impact and high-weatherability PC / PBT resin composition and its preparation method, which selects POE-g-GMA as the toughening agent of the system. The amount of POE-g-GMA has a great influence on the performance of the material. When the amount added is insufficient, the low-temperature impact performance of the material needs to be further improved. When excessively added, the rigidity and heat resistance of the material will be significantly reduced, and the weather resistance and hydrolysis stability will also be significantly reduced;
[0006] Chinese patent CN104004339 discloses a PC / PBT / AES alloy material, which uses E-MA-GMA copolymer as a toughening agent. The reaction mechanism of the ternary alloy is more complicated. Using only E-MA-GMA copolymer cannot completely solve the compatibility problem. Moreover, the cold resistance, weather resistance and hydrolysis resistance obtained by using only AES need to be further improved.
[0007] The formula design and preparation technology of traditional PC / PBT alloy materials cannot meet the increasingly higher usage requirements. For example, new energy uses such as 5G antenna covers, charging piles, new energy vehicle exteriors, and IoT uses such as drone brackets all put forward higher requirements on material selection. Therefore, it is necessary to prepare PC / PBT alloys with better comprehensive performance. Summary of the invention
[0008] The object of the present invention is to provide a cold-resistant, weather-resistant, high-impact and high-hydrolysis stability PC / PBT alloy, which is used to solve the technical problem that the cold-resistant, weather-resistant and impact-resistant and hydrolysis-resistant properties of the PC / PBT alloy in the prior art need to be further improved.
[0009] The object of the present invention is achieved through the following technical scheme: A cold-resistant, weather-resistant, high-impact and high-hydrolysis-resistant PC / PBT alloy, comprising the following raw material components in parts by weight:
[0010]
[0011]
[0012] Furthermore, the viscosity average molecular weight of the polycarbonate is between 12000 and 30000, the silicon content in the silicon-containing polycarbonate is 5-10 wt %, and the intrinsic viscosity of the polybutylene terephthalate is 0.8-1.2 dl / g.
[0013] Furthermore, the polycarbonate is one or more of bisphenol A polycarbonate, tetrabromobisphenol A polycarbonate, tetrafluorobisphenol A polycarbonate, bisphenol S polycarbonate and bisphenol AP polycarbonate.
[0014] Further, silicon-containing polycarbonate refers to a copolymer of siloxane and polycarbonate;
[0015] Furthermore, the preparation method of the silicon-containing polycarbonate comprises the following steps:
[0016] A1. Put bisphenol A and N,N-dimethylformamide into a reaction kettle and stir at room temperature for 10-15 minutes. After stirring, raise the temperature of the reaction kettle to 50-100°C, slowly introduce phosgene into the reaction kettle, and keep the temperature for reaction for 2-4 hours to obtain a reaction precursor solution.
[0017] Reaction equation:
[0018]
[0019] Reaction principle: Phosgene reacts with the hydroxyl group of bisphenol A at high temperature to generate polycarbonate precursor.
[0020] A2. Add the reaction precursor liquid, hydroxy silicone oil with a molecular weight of 1200-3600 and sodium carbonate into the reactor, increase the temperature of the reactor to 100-150° C., keep the temperature for 2-4 hours, and post-treat to obtain silicon-containing polycarbonate.
[0021] Reaction equation:
[0022]
[0023] Reaction principle: Under alkaline conditions, the halogen groups in the polycarbonate precursor react with the hydroxyl groups in the hydroxyl silicone oil to produce a chain structure to obtain silicon-containing polycarbonate.
[0024] Furthermore, in step A1, the dosage ratio of bisphenol A, phosgene and N,N-dimethylformamide is 12-15g:8-9g:80-100mL, and the stirring rate is 120-180rpm; in step A2, the dosage ratio of hydroxy silicone oil with a molecular weight of 1200-3600, sodium carbonate and reaction precursor liquid is 6-13g:1-2g:18-20mL, and the stirring rate is 120-180rpm. The post-treatment includes: pouring the reaction solution into deionized water to form a polycarbonate precipitate, collecting the filter cake by suction, washing the filter cake with dichloromethane, placing the filter cake in a drying furnace at a temperature of 80°C and vacuum drying until the filter cake is constant weight, to obtain silicon-containing polycarbonate.
[0025] Furthermore, the weather-resistant toughening and compatibility modifier is one or both of AES-g-GMA and EPDM-co-SAG.
[0026] Further, the preparation method of AES-g-GMA comprises the following steps:
[0027] B1, adding azobisisobutyronitrile, glycidyl methacrylate and N,N-dimethylformamide into a reactor, raising the temperature of the reactor to 80-120° C., and keeping the temperature for 2-4 hours to obtain a reaction precursor solution;
[0028] B2, adding N-bromosuccinimide and the reaction precursor solution into the reaction kettle, raising the temperature of the reaction kettle to 80-120° C., and keeping the temperature for 2-4 hours to obtain a halogenated precursor solution;
[0029] Halogenated precursor synthesis reaction equation:
[0030]
[0031] Principle of halogenated precursor synthesis reaction: Azobisisobutyronitrile acts as a free radical initiator to initiate a free radical addition reaction after the double bond of the olefin is broken. N-bromosuccinimide selectively reacts with the free radical formed by the double bond break to form a halogenated chain structure.
[0032] B3. Add the halogenated precursor solution, acrylonitrile-ethylene propylene diene monomer rubber-styrene copolymer ring, anhydrous aluminum chloride and N,N-dimethylformamide into the reactor, increase the temperature of the reactor to 50-100°C, keep the reaction temperature for 2-4 hours, and obtain AES-g-GMA after post-treatment.
[0033] AES-g-GMA synthesis reaction equation:
[0034]
[0035] AES-g-GMA synthesis reaction principle: In the presence of anhydrous aluminum chloride Lewis acid anhydrous aluminum chloride, aromatic hydrocarbons react with alkyl halides to produce electrophilic substitution reactions on the aromatic rings, where the hydrogen atoms are replaced by halogens to generate aromatic hydrocarbons.
[0036] Further, in step B1, the ratio of azobisisobutyronitrile, glycidyl methacrylate and N,N-dimethylformamide is 1-2g:5-8g:40-50mL, and the stirring rate is 120-180rpm; in step B2, the ratio of N-bromosuccinimide and the reaction precursor solution is 4-5g:40-50mL; in step B3, the halogenated precursor solution, acrylonitrile-ethylene propylene rubber-styrene copolymer ring, anhydrous aluminum chloride and N The dosage ratio of N-dimethylformamide is 40-50mL:50-400g:20g:1000mL. The post-treatment includes: after the reaction is completed, the reaction solution is placed in a rotary evaporator, the speed is adjusted to 100-150rpm, the temperature is set to 30-40℃, and the system is rotary evaporated to constant weight to obtain a residue. The residue is washed with deionized water 3-5 times and then placed in a drying oven at 80℃ for vacuum drying until the residue is constant weight to obtain AES-g-GMA.
[0037] Further, the preparation method of EPDM-co-SAG comprises the following steps:
[0038] C1. Add styrene, acrylonitrile, glycidyl methacrylate and toluene into a reaction kettle, and stir for 15-20 minutes at room temperature to obtain a reaction solution;
[0039] C2, adding the reaction solution and benzoyl peroxide into a reactor, raising the temperature of the reactor to 70-80°C, keeping the temperature for reaction for 6-12h, and post-treating to obtain a styrene-acrylonitrile-glycidyl methacrylate ternary random copolymer;
[0040] Reaction equation:
[0041]
[0042] Reaction principle: Benzoyl peroxide acts as a free radical initiator to initiate a free radical addition reaction after the double bonds of styrene, acrylonitrile and glycidyl methacrylate are broken, thereby preparing a styrene-acrylonitrile-glycidyl methacrylate ternary random copolymer.
[0043] C3. Add styrene-acrylonitrile-glycidyl methacrylate terpolymer, ethylene propylene diene rubber, toluene and benzoyl peroxide into a reactor, increase the temperature of the reactor to 120-150° C., keep the reaction warm for 4-6 hours, and obtain EPDM-co-SAG by post-treatment.
[0044] Principle of EPDM-co-SAG synthesis reaction: Benzoyl peroxide acts as a free radical initiator to initiate a free radical addition reaction after the double bonds of EPDM rubber are broken, and further addition reaction occurs with the free radicals on the styrene-acrylonitrile-glycidyl methacrylate terpolymer to prepare EPDM-co-SAG.
[0045] Further, in step C1, the amount ratio of styrene, acrylonitrile, glycidyl methacrylate and toluene is 8-10g:3-5g:3-5g:50mL, and the stirring rate is 120-180rpm; in step C2, the amount ratio of benzoyl peroxide to the reaction solution is 0.2g:50mL, and the post-treatment is as follows: after the reaction is completed, the reaction solution is placed in a rotary evaporator, the speed is adjusted to 100-150rpm, the temperature is set to 70-80°C, and the system is rotary evaporated to constant weight to obtain a residue, and the residue is washed with deionized water 3-5 times and then placed in a drying oven at a temperature of 80°C and vacuum dried until the residue is constant weight , obtaining a styrene-acrylonitrile-GMA ternary random copolymer; in step C3, the amount ratio of the styrene-acrylonitrile-GMA ternary random copolymer, ethylene propylene rubber, toluene and benzoyl peroxide is 5-6g:10-15g:0.2g:50mL, and the subsequent operation includes: after the reaction is completed, placing the reaction solution in a rotary evaporator, adjusting the speed to 100-150rpm, setting the temperature to 70-80°C, and rotary evaporating until the system is constant weight to obtain a residue, washing the residue with deionized water 3-5 times, and then placing it in a drying oven at a temperature of 80°C and vacuum drying until the residue is constant weight to obtain EPDM-co-SAG.
[0046] Furthermore, the weather-resistant toughening compatibility modifier is at least one of AES-g-GMA or EPDM-co-SAG, in which the content of glycidyl methacrylate in AES-g-GMA is 2-10wt%; in EPDM-co-SAG, the content of ethylene propylene diene monomer rubber is 60-75wt%, in which the content of glycidyl methacrylate is 3-12%.
[0047] Furthermore, the hydrolysis stabilizer is one or more of an epoxy chain extender and a carbodiimide, the epoxy chain extender is one or more of styrene-acrylic acid-glycidyl methacrylate, styrene-acrylate-glycidyl methacrylate, acrylate-glycidyl methacrylate, styrene-acrylonitrile-glycidyl methacrylate, and styrene-glycidyl methacrylate copolymer, and has a weight average molecular weight of 5000-100000 and an epoxy equivalent of 200-500 g / mol; and the carbodiimide is a polymeric carbodiimide.
[0048] Furthermore, the transesterification inhibitor is a phosphate or phosphate ester transesterification inhibitor, including but not limited to one or more of dioctyl phosphate, disodium dihydrogen pyrophosphate, diisooctyl phosphate, sodium dihydrogen phosphate, and triphenyl phosphite.
[0049] Furthermore, the light stabilizer is one or more of benzotriazole, benzophenone, salicylate, benzoate, cyanoacrylate, organic nickel complex and hindered amine light stabilizer.
[0050] Furthermore, the antioxidant is one or more of phosphite antioxidants and hindered phenol antioxidants, and the lubricant is one or more of silicone, stearate, polyethylene wax, pentaerythritol stearate, and ethylene bisstearamide.
[0051] The present invention also provides a method for preparing a high-strength and stable PCPBT alloy material, comprising the following steps:
[0052] S1, polycarbonate, silicon-containing polycarbonate, polybutylene terephthalate, weather-resistant toughening compatibility modifier, hydrolysis stabilizer, transesterification inhibitor, light stabilizer, antioxidant and lubricant are mixed uniformly in proportion to obtain a premix;
[0053] S2. The premix is fed into the main feed port of a twin-screw extruder, and the modified alloy material is obtained through melt blending, devolatilization extrusion, cooling and granulation.
[0054] Furthermore, the melt blending process parameters are: the feeding section temperature is 180-220°C, the plasticizing section temperature is 200-240°C, the homogenizing section temperature is 220-260°C, the screw speed is 300-600rpm, the extruder aspect ratio is 36:1-60:1, and at least one vacuum devolatilization port is set at the end of the extruder.
[0055] The present invention has the following beneficial effects:
[0056] 1. In the process of preparing a high-strength and stable PC / PBT alloy material, the present invention selects to use a silicon-containing polycarbonate copolymer to partially replace the traditional polycarbonate to make up for the disadvantages of the traditional polycarbonate in many aspects. Although the traditional polycarbonate performs well in many applications, it has some limitations in terms of weather resistance, hydrolysis resistance, low temperature resistance and chemical corrosion resistance. Silicon polycarbonate copolymers not only maintain the excellent physical properties and processability of polycarbonate, but also significantly improve the overall performance of the material; Silicon polycarbonate copolymers have excellent weather resistance and can be exposed to outdoor environments for a long time without losing performance stability, which makes them have a longer service life and less maintenance requirements in outdoor use; Silicon polycarbonate copolymers show excellent resistance to hydrolysis and are not easily degraded by moisture, making them suitable for applications in humid or high humidity environments; Silicon polycarbonate copolymers also have excellent low-temperature resistance and can maintain their physical properties at extremely low temperatures, so they have wide application potential in cold areas or cooling equipment; The use of silicon polycarbonate copolymers blended with polybutylene terephthalate not only expands the application range of the material, but also further optimizes its physical properties and processing characteristics. This alloy material is not only more stable and reliable in structure, but also shows better overall performance in practical applications, meeting the market demand for high-performance and multifunctional materials.
[0057] 2. In the process of preparing a high-strength and stable PC / PBT alloy material, the present invention selects the copolymer and (or) graft copolymer of AES and GMA with originality as the toughening and compatibility modifier of the material through the optimization design of the formula, and utilizes the special molecular structure characteristics and impact resistance of AES. By grafting GMA, GMA can form a cross-linked structure in the matrix, which can effectively absorb and disperse stress, thereby improving the toughness of the material, and the vinyl and epoxy groups in the molecule have high reactivity, and these functional groups can react with polycarbonate to form a cross-linked structure. It fully reacts with the terminal carboxyl group of polybutylene terephthalate to provide better compatibility and toughness, forming a covalent bond. This chemical reaction can firmly bind the modifier to the base material, thereby enhancing the mechanical properties and compatibility of the material. Compared with traditional MBS, POE-g-GMA, EMA-co-GMA and EBA-co-GMA, it has excellent weather resistance and excellent thermal stability, and will not decompose small molecules that promote the degradation of polycarbonate and polybutylene terephthalate during processing and use, reducing the service life of the material. The weather resistance and cold resistance of PC / PBT alloy are further improved by the composite use of this compatible toughening modifier and silicon-containing polycarbonate.
[0058] 3. In the process of preparing a high-strength and stable PC / PBT alloy material, the present invention introduces an organic silicon group into the carbonate, increases the length of the structural unit, reduces the rigidity of the huge benzene ring, and increases the flexibility of the molecular chain. Therefore, the fluidity of the polycarbonate material is significantly improved. In addition, the structural characteristics of the siloxane also greatly improve the hydrolysis resistance of the polycarbonate, and it has excellent characteristics such as high and low temperature resistance, electrical insulation, oxidation stability, weather resistance, flame retardancy, hydrophobicity, corrosion resistance, non-toxicity, tastelessness, and physiological inertness; epoxy chain extenders are selected as the PC / PBT alloy. The hydrolysis stabilizer significantly improves the material's resistance to hydrolysis. The high reactivity of the epoxy chain extender can undergo a cross-linking reaction with the matrix material to enhance the material's structural stability. At the same time, the synergistic effect of the epoxy chain extender and carbodiimide enables the PC / PBT alloy material to exhibit better durability and stability in harsh environments, thereby effectively preventing the hydrolysis reaction. This optimization scheme not only improves the hydrolysis resistance of the PC / PBT alloy material, but also broadens its application range, especially in application scenarios that require long-term exposure to high temperature and high humidity environments, showing broad prospects. DETAILED DESCRIPTION
[0059] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0060] It should be noted that the raw materials used in the following examples and comparative examples are shown in Table 1 below:
[0061] Table 1 - Raw materials used in the examples and comparative examples
[0062]
[0063]
[0064] Example 1
[0065] This embodiment provides a method for preparing a high-strength and stable silicon-containing polycarbonate for PC / PBT alloy material, comprising the following steps:
[0066] Bisphenol A, N,N-dimethylformamide and phosgene were taken in a dosage ratio of 12g:8g:100mL, and bisphenol A and N,N-dimethylformamide were put into a reaction kettle, and stirred at room temperature for 10 minutes at a stirring rate of 120rpm. After the stirring was completed, the temperature of the reaction kettle was increased to 50°C, and phosgene was slowly introduced therein, and the reaction was kept warm for 2 hours to obtain a reaction precursor solution;
[0067] Hydroxy silicone oil with a molecular weight of 1653.24, sodium carbonate and reaction precursor liquid were added to the reactor in a dosage ratio of 3g:2g:20mL. The temperature of the reactor was raised to 100°C and the reaction was kept warm for 2 hours. The reaction liquid was poured into deionized water to form a polycarbonate precipitate. The filter cake was collected by filtration, and the filter cake was washed with dichloromethane. The filter cake was placed in a drying furnace at a temperature of 80°C and vacuum dried until the filter cake had a constant weight to obtain silicon-containing polycarbonate.
[0068] Example 2
[0069] This embodiment provides a method for preparing a high-strength and stable silicon-containing polycarbonate for PC / PBT alloy material, comprising the following steps:
[0070] Bisphenol A, N,N-dimethylformamide and phosgene were taken in a dosage ratio of 12 g:8 g:100 mL, and bisphenol A and N,N-dimethylformamide were put into a reaction kettle, and stirred at room temperature for 15 min at a stirring rate of 180 rpm. After the stirring was completed, the temperature of the reaction kettle was increased to 100° C., and phosgene was slowly introduced therein, and the reaction was kept warm for 4 h to obtain a reaction precursor solution;
[0071] Hydroxy silicone oil with a molecular weight of 2468.73, sodium carbonate and reaction precursor liquid were added to the reactor in a dosage ratio of 13g:2g:18mL. The temperature of the reactor was raised to 150°C and the reaction was kept warm for 4 hours. The reaction liquid was poured into deionized water to form a polycarbonate precipitate. The filter cake was collected by filtration, and the filter cake was washed with dichloromethane. The filter cake was placed in a drying furnace at a temperature of 80°C and vacuum dried until the filter cake had a constant weight to obtain silicon-containing polycarbonate.
[0072] Example 3
[0073] This embodiment provides a method for preparing a high-strength and stable silicon-containing polycarbonate for PC / PBT alloy material, comprising the following steps:
[0074] Bisphenol A, N,N-dimethylformamide and phosgene were taken in a dosage ratio of 12g:9g:80mL, and bisphenol A and N,N-dimethylformamide were put into a reaction kettle, and stirred at room temperature for 15min at a stirring rate of 180rpm. After the stirring was completed, the temperature of the reaction kettle was increased to 100°C, and phosgene was slowly introduced therein, and the reaction was kept warm for 4h to obtain a reaction precursor solution;
[0075] Hydroxy silicone oil with a molecular weight of 3261.45, sodium carbonate and reaction precursor liquid were added to the reactor in a dosage ratio of 9g:2g:18mL. The temperature of the reactor was raised to 150°C and the reaction was kept warm for 4 hours. The reaction liquid was poured into deionized water to form a polycarbonate precipitate. The filter cake was collected by filtration, and the filter cake was washed with dichloromethane. The filter cake was placed in a drying furnace at a temperature of 80°C and vacuum dried until the filter cake had a constant weight to obtain silicon-containing polycarbonate.
[0076] Example 4
[0077] This embodiment provides a method for preparing AES-g-GMA for high-strength and stable PC / PBT alloy material, comprising the following steps:
[0078] Azobisisobutyronitrile, glycidyl methacrylate and N,N-dimethylformamide were added into the reactor at a ratio of 2 g:5 g:50 mL, the temperature of the reactor was raised to 80° C., and the reaction was carried out for 2 hours to obtain a reaction precursor solution;
[0079] N-bromosuccinimide and the reaction precursor solution were added into the reactor at a ratio of 4 g:50 mL, the temperature of the reactor was raised to 80° C., and the reaction was kept warm for 2 hours to obtain a halogenated precursor solution.
[0080] The halogenated precursor solution, acrylonitrile-ethylene propylene rubber-styrene copolymer ring, anhydrous aluminum chloride and N,N-dimethylformamide were added to the reactor in a dosage ratio of 40mL:400g:20g:1000mL. The temperature of the reactor was raised to 50°C and the reaction was kept warm for 2 hours. After the reaction was completed, the reaction solution was placed in a rotary evaporator, the speed was adjusted to 100rpm, the temperature was set to 30°C, and the system was rotary evaporated to constant weight to obtain a residue. The residue was washed three times with deionized water and placed in a drying oven at 80°C for vacuum drying until the residue had constant weight to obtain AES-g-GMA.
[0081] Example 5
[0082] This embodiment provides a method for preparing AES-g-GMA for high-strength and stable PC / PBT alloy material, comprising the following steps:
[0083] Azobisisobutyronitrile, glycidyl methacrylate and N,N-dimethylformamide were added into the reactor at a ratio of 2 g:58 g:40 mL, the temperature of the reactor was raised to 120° C., and the reaction was carried out for 4 hours to obtain a reaction precursor solution;
[0084] N-bromosuccinimide and the reaction precursor solution were added into the reactor at a ratio of 5 g:50 mL, the temperature of the reactor was raised to 120° C., and the reaction was kept warm for 4 hours to obtain a halogenated precursor solution.
[0085] The halogenated precursor solution, acrylonitrile-ethylene propylene rubber-styrene copolymer ring, anhydrous aluminum chloride and N,N-dimethylformamide were added to the reactor in a dosage ratio of 50mL:50g:20g:1000mL. The temperature of the reactor was raised to 100°C and the reaction was kept warm for 4 hours. After the reaction was completed, the reaction solution was placed in a rotary evaporator, the speed was adjusted to 150rpm, the temperature was set to 40°C, and the system was rotary evaporated to constant weight to obtain a residue. The residue was washed 5 times with deionized water and placed in a drying oven at 80°C for vacuum drying until the residue was constant weight to obtain AES-g-GMA.
[0086] Example 6
[0087] This embodiment provides a method for preparing AES-g-GMA for high-strength and stable PC / PBT alloy material, comprising the following steps:
[0088] Azobisisobutyronitrile, glycidyl methacrylate and N,N-dimethylformamide were added into the reactor at a ratio of 2 g:6 g:45 mL, the temperature of the reactor was raised to 100° C., and the reaction was carried out for 4 hours to obtain a reaction precursor solution;
[0089] N-bromosuccinimide and the reaction precursor solution were added into the reactor at a ratio of 5 g:40 mL, the temperature of the reactor was raised to 120° C., and the reaction was kept warm for 4 hours to obtain a halogenated precursor solution.
[0090] The halogenated precursor solution, acrylonitrile-ethylene propylene rubber-styrene copolymer ring, anhydrous aluminum chloride and N,N-dimethylformamide were added to the reactor in a dosage ratio of 50mL:200g:20g:1000mL. The temperature of the reactor was raised to 75°C and the reaction was kept warm for 4 hours. After the reaction was completed, the reaction solution was placed in a rotary evaporator, the speed was adjusted to 150rpm, the temperature was set to 40°C, and the system was rotary evaporated to constant weight to obtain a residue. The residue was washed 5 times with deionized water and placed in a drying oven at 80°C for vacuum drying until the residue was constant weight to obtain AES-g-GMA.
[0091] Example 7
[0092] This embodiment provides a method for preparing a high-strength and stable PC / PBT alloy material EPDM-co-SAG, comprising the following steps:
[0093] Styrene, acrylonitrile, glycidyl methacrylate and toluene were added into a reaction kettle in a dosage ratio of 8 g:3 g:5 g:50 mL, and stirred at room temperature for 15 min at a stirring rate of 120 rpm to obtain a reaction solution;
[0094] The reaction solution and benzoyl peroxide were added to the reactor in a dosage ratio of 50 mL: 0.2 g, the temperature of the reactor was raised to 70° C., and the reaction was kept warm for 6 hours. After the reaction was completed, the reaction solution was placed in a rotary evaporator, the speed was adjusted to 100 rpm, the temperature was set to 70° C., and the system was rotary evaporated to a constant weight to obtain a residue, the residue was washed 3 times with deionized water, and then placed in a drying oven at a temperature of 80° C. and vacuum dried until the residue was constant weight, to obtain a styrene-acrylonitrile-GMA ternary random copolymer;
[0095] Styrene-acrylonitrile-glycidyl methacrylate terpolymer, ethylene propylene diene rubber, toluene and benzoyl peroxide were added into the reactor in the amount ratio of 5g:15g:0.2g:50mL, the temperature of the reactor was raised to 150°C, and the reaction was kept warm for 4 hours. After the reaction was completed, the reaction solution was placed in a rotary evaporator, the speed was adjusted to 100rpm, the temperature was set to 70°C, and the system was rotary evaporated to constant weight to obtain a residue. The residue was washed 3 times with deionized water and placed in a drying oven at 80°C for vacuum drying until the residue was constant weight to obtain EPDM-co-SAG.
[0096] Example 8
[0097] This embodiment provides a method for preparing a high-strength and stable PC / PBT alloy material EPDM-co-SAG, comprising the following steps:
[0098] Styrene, acrylonitrile, glycidyl methacrylate and toluene were added into a reaction kettle in a dosage ratio of 10 g:3 g:5 g:50 mL, and stirred at room temperature for 15 min at a stirring rate of 180 rpm to obtain a reaction solution;
[0099] The reaction solution and benzoyl peroxide were added to a reactor in a dosage ratio of 50 mL:0.2 g, the temperature of the reactor was raised to 70° C., and the reaction was kept warm for 9 hours. After the reaction was completed, the reaction solution was placed in a rotary evaporator, the speed was adjusted to 150 rpm, the temperature was set to 80° C., and the system was rotary evaporated to a constant weight to obtain a residue, the residue was washed 5 times with deionized water, and then placed in a drying oven at a temperature of 80° C. and vacuum dried until the residue was constant weight, to obtain a styrene-acrylonitrile-GMA ternary random copolymer;
[0100] Styrene-acrylonitrile-glycidyl methacrylate terpolymer, ethylene propylene rubber, toluene and benzoyl peroxide were added into the reactor in the amount ratio of 6g:10g:0.2g:50mL, the temperature of the reactor was raised to 135°C, and the reaction was kept warm for 5 hours. After the reaction was completed, the reaction solution was placed in a rotary evaporator, the speed was adjusted to 125rpm, the temperature was set to 80°C, and the system was rotary evaporated to constant weight to obtain a residue. The residue was washed with deionized water 5 times and then placed in a drying oven at 80°C for vacuum drying until the residue was constant weight to obtain EPDM-co-SAG.
[0101] Example 9
[0102] This embodiment provides a method for preparing a high-strength and stable PC / PBT alloy material EPDM-co-SAG, comprising the following steps:
[0103] Styrene, acrylonitrile, glycidyl methacrylate and toluene were added into a reaction kettle at a ratio of 10 g:5 g:5 g:50 mL, and stirred at room temperature for 20 min at a stirring rate of 180 rpm to obtain a reaction solution;
[0104] The reaction solution and benzoyl peroxide were added to the reactor in a dosage ratio of 50 mL: 0.2 g, the temperature of the reactor was raised to 80° C., and the reaction was kept warm for 12 hours. After the reaction was completed, the reaction solution was placed in a rotary evaporator, the speed was adjusted to 150 rpm, the temperature was set to 80° C., and the system was rotary evaporated to a constant weight to obtain a residue, the residue was washed 5 times with deionized water, and then placed in a drying oven at a temperature of 80° C. and vacuum dried until the residue was constant weight, to obtain a styrene-acrylonitrile-GMA ternary random copolymer;
[0105] Styrene-acrylonitrile-glycidyl methacrylate terpolymer, ethylene propylene rubber, toluene and benzoyl peroxide were added into the reactor in the amount ratio of 6g:15g:0.2g:50mL, the temperature of the reactor was raised to 150°C, and the reaction was kept warm for 6 hours. After the reaction was completed, the reaction solution was placed in a rotary evaporator, the speed was adjusted to 150rpm, the temperature was set to 80°C, and the system was rotary evaporated to constant weight to obtain a residue. The residue was washed with deionized water 5 times and then placed in a drying oven at 80°C for vacuum drying until the residue was constant weight to obtain EPDM-co-SAG.
[0106] Preparation of high-strength and stable PC / PBT alloy materials
[0107] Weigh each raw material according to the formula amount described in Table 2 and Table 3 below, put the weighed raw materials into a mixer and mix them evenly to obtain a premix; then put the premix into a twin-screw extruder, and obtain the PC / PBT alloy material described in the present application through melt blending, devolatilization extrusion, cooling and granulation.
[0108] The parameters used for melt extrusion are: the extruder screw aspect ratio is 48:1, a vacuum port is set in the ninth zone and the eleventh zone of the extruder respectively, the feeding section temperature is 200°C, the plasticizing section temperature is 220°C, the homogenizing section temperature is 240°C, and the screw speed is 400rpm.
[0109] Table 2 - Amount of each component in Examples 10-15 (parts by weight)
[0110]
[0111]
[0112] Table 3-Comparative Examples 1-7 Component Amounts (Parts by Weight)
[0113]
[0114] Performance Testing:
[0115] The notched cantilever beam impact strength, tensile strength, flow properties, weather resistance, and hydrolytic stability of the PC / PBT alloy materials prepared in Examples 10-15 and Comparative Examples 1-7 were tested:
[0116] The notched cantilever beam impact strength was tested at room and low temperatures according to ASTM D256-1997 "Standard test method for cantilever beam impact strength of plastics". The test temperatures include: (room temperature) 23±2°C, (low temperature) -40±2°C, and humidity: 50±5%.
[0117] The tensile strength of the prepared specimens was tested for tensile strength according to the standard ASTM D638-2003 "Standard Test Method for Tensile Properties of Plastics", wherein the tensile speed was 50 mm / min, the test temperature was 23±2°C, and the humidity was 50±5%.
[0118] The melt flow rate (MFR) of the prepared particles was tested with reference to the standard ASTM D1238-13 "Test method for measuring the melt flow rate of thermoplastics by extrusion plastometer", the test temperature was 250°C, and the particle mass was 5kg.
[0119] Weathering test: UV / condensation test, UVB-313 light source, deionized water, no relative humidity control, cyclic exposure test conditions are as follows:
[0120] 8h drying: Turn on the UVB-313 light source, and set the irradiance at 310nm to 0.48W·m-2·nm-1, and the black mark temperature to 60±3℃;
[0121] 4h condensation: turn off the light source, the black mark temperature is 50±3℃;
[0122] After 96 hours of UVB aging, the color difference ΔE was tested.
[0123] Hydrolysis stability test: Take the sample particles in the embodiment and the comparative example, place them in a high temperature and high humidity box at a temperature of 100°C and a humidity of 100% RH, keep them for 120h and 240h, take samples and test their MFR respectively, then compare the changes in the flow properties of the materials before and after the accelerated high temperature and high humidity test and calculate the improvement. The MFR improvement rate calculation formula is as follows:
[0124] MFR improvement rate = (MFR after high temperature and high humidity aging - conventional test MFR / conventional test MFR) * 100%
[0125] The various properties of the embodiments and comparative examples were tested according to the above-mentioned methods as shown in Table 4.
[0126] Table 4 - Performance test results of various embodiments and comparative examples
[0127]
[0128]
[0129] Data Analysis:
[0130] It can be seen from Examples 10-15 that the PC / PBT alloy material prepared according to the method and process of the present invention has excellent impact strength, especially excellent low-temperature impact resistance at -40°C, and excellent weather resistance and hydrolysis resistance. After the UVB accelerated aging test, the ΔE value of the material is ≤2.0; after the high temperature and high humidity accelerated aging test at 100°C and 100% RH, the flowability of the material is not improved much, indicating that the molecular chain of the material is rarely broken under severe high temperature and high humidity conditions, and has stable hydrolysis resistance, which is specifically manifested in that after 120h of accelerated aging, the MFR increase rate of the material is ≤17%, and after 240h of accelerated aging, the MFR increase rate of the material is ≤37%.
[0131] It can be seen from the test results of Comparative Examples 1 and 2 that after adding equal parts of POE-g-GMA or EMA-co-GMA, the impact resistance at room temperature is acceptable, but not as good as the weather-resistant toughening compatibilizer used in the present invention, and its weather resistance and hydrolysis resistance are even worse than Examples 1 and 2 of the present invention; especially after a large amount of EMA-co-GMA is used in Comparative Example 2, the flowability of the material decreases significantly, inhibiting the high flowability that the alloy material should have.
[0132] In Comparative Examples 3 and 4, silicon-containing polycarbonate was not used, and only conventional MBS toughening agents and acrylate toughening agents were used. The materials had good impact properties, but insufficient cold resistance, and poor performance in weather resistance and hydrolysis stability, and could not meet the requirements for use under harsh conditions.
[0133] Comparative Example 5 only uses unfunctionalized AES, and no other polyester toughening agents or compatibilizers are added. The compatibility of polycarbonate and polybutylene terephthalate in the alloy system is limited, making the impact performance of the alloy material very poor, and the cold resistance and weather resistance are not improved, and the hydrolysis stability is poor; in Comparative Example 6, a small amount of acrylate toughening agent and AES are used in combination. Since the acrylate toughening agent contains GMA functional groups, it can be capped with polycarbonate or polybutylene terephthalate in the alloy system, which can improve the compatibility and impact toughness of the alloy material, but the improvement in weather resistance is limited, which may be related to the type of compatibilizer or toughening agent. Even if the siloxane copolymer polycarbonate and AES are more, the advantages of good weather resistance of the two are not brought into play. In Comparative Example 7, without adding silicon-containing polycarbonate, the cold resistance cannot show advantages, and the weather resistance and hydrolysis stability cannot meet the use under harsh outdoor conditions.
[0134] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0135] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0136] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A high-strength and stable PC / PBT alloy material, It is characterized in that The invention comprises the following raw material components in parts by weight:
2. A high-strength and stable PC / PBT alloy material according to claim 1, It is characterized in that The polycarbonate is one or more of bisphenol A polycarbonate, tetrabromobisphenol A polycarbonate, tetrafluorobisphenol A polycarbonate, bisphenol S polycarbonate and bisphenol AP polycarbonate.
3. A high-strength and stable PC / PBT alloy material according to claim 1, It is characterized in that The preparation method of the silicon-containing polycarbonate comprises the following steps: A1. Put bisphenol A and N,N-dimethylformamide into a reaction kettle and stir at room temperature for 10-15 minutes. After stirring, raise the temperature of the reaction kettle to 50-100°C, slowly introduce phosgene into the reaction kettle, and keep the temperature for reaction for 2-4 hours to obtain a reaction precursor solution. A2. Add the reaction precursor liquid, hydroxy silicone oil with a molecular weight of 1200-3600 and sodium carbonate into the reactor, increase the temperature of the reactor to 100-150° C., keep the temperature for 2-4 hours, and post-treat to obtain silicon-containing polycarbonate.
4. A high-strength and stable PC / PBT alloy material according to claim 3, It is characterized in that In step A1, the dosage ratio of bisphenol A, phosgene and dichloromethane is 12-15g:8-9g:80-100mL, and the stirring rate is 120-180rpm; in step A2, the dosage ratio of hydroxy silicone oil with a molecular weight of 1200-3600, sodium carbonate and reaction precursor liquid is 6-8g:2-3g:18-20mL, and the stirring rate is 120-180rpm. Post-treatment includes: pouring the reaction solution into deionized water to form a polycarbonate precipitate, collecting the filter cake by suction filtration, washing the filter cake with dichloromethane, placing the filter cake in a drying furnace at a temperature of 80°C and vacuum drying until the filter cake has a constant weight, to obtain silicon-containing polycarbonate.
5. A high-strength and stable PC / PBT alloy material according to claim 1, It is characterized in that The weather-resistant toughening and compatibility modifier is one or both of AES-g-GMA and EPDM-co-SAG.
6. A high-strength and stable PC / PBT alloy material according to claim 5, It is characterized in that The preparation method of the AES-g-GMA comprises the following steps: B1, adding azobisisobutyronitrile, glycidyl methacrylate and N,N-dimethylformamide into a reactor, raising the temperature of the reactor to 80-120° C., and keeping the temperature for 2-4 hours to obtain a reaction precursor solution; B2. Add N-bromosuccinimide and the reaction precursor solution into the reaction kettle, increase the temperature of the reaction kettle to 80-120° C., keep the temperature for 2-4 hours, and post-treat to obtain the halogenated precursor solution. B3. Add the halogenated precursor solution, acrylonitrile-ethylene propylene diene monomer rubber-styrene copolymer ring, anhydrous aluminum chloride and N,N-dimethylformamide into the reactor, increase the temperature of the reactor to 50-100°C, keep the reaction temperature for 2-4 hours, and obtain AES-g-GMA after post-treatment.
7. A high-strength and stable PC / PBT alloy material according to claim 5, It is characterized in that The preparation method of the EPDM-co-SAG comprises the following steps: C1. Add styrene, acrylonitrile, glycidyl methacrylate and toluene into a reaction kettle, and stir for 15-20 minutes at room temperature to obtain a reaction solution; C2, adding the reaction solution and benzoyl peroxide into a reactor, raising the temperature of the reactor to 70-80°C, keeping the temperature for reaction for 6-12h, and post-treating to obtain a styrene-acrylonitrile-glycidyl methacrylate ternary random copolymer; C3. Add styrene-acrylonitrile-glycidyl methacrylate terpolymer, ethylene propylene diene rubber, toluene and benzoyl peroxide into a reactor, increase the temperature of the reactor to 120-150° C., keep the reaction warm for 4-6 hours, and obtain EPDM-co-SAG by post-treatment.
8. A high-strength and stable PC / PBT alloy material according to claim 1, It is characterized in that The hydrolysis stabilizer is one or more of an epoxy chain extender and a carbodiimide, and the epoxy chain extender is one or more of styrene-acrylic acid-glycidyl methacrylate, styrene-acrylate-glycidyl methacrylate, acrylate-glycidyl methacrylate, styrene-acrylonitrile-glycidyl methacrylate, and styrene-glycidyl methacrylate copolymer, and has an average molecular weight of 5000-100000 and an epoxy equivalent of 200-500 g / mol.
9. A method for preparing a high-strength and stable PC / PBT alloy material, applicable to a high-strength and stable PC / PBT alloy material as claimed in any one of claims 1 to 8, It is characterized in that The following steps are involved: S1, polycarbonate, silicon-containing polycarbonate, polybutylene terephthalate, weather-resistant toughening compatibility modifier, hydrolysis stabilizer, transesterification inhibitor, light stabilizer, antioxidant and lubricant are mixed uniformly in proportion to obtain a premix; S2. The premix is fed into the main feed port of a twin-screw extruder, and the modified alloy material is obtained through melt blending, devolatilization extrusion, cooling and granulation.
10. A method for preparing a high-strength and stable PC / PBT alloy material according to claim 9, It is characterized in that The melt blending process parameters are: the feeding section temperature is 180-220°C, the plasticizing section temperature is 200-240°C, the homogenizing section temperature is 220-260°C, the screw speed is 300-600rpm, the extruder aspect ratio is 36:1-60:1, and at least one vacuum devolatilization port is set at the end of the extruder.
Citation Information
Patent Citations
Toughening modified PC and preparation method thereof
CN104672835A
Toughened PC / SI-PC / PBT alloy material and preparation method thereof
CN110760175A
Cited By
Hydrolysis-resistant flame-retardant PBT / PC alloy material and preparation method thereof
CN120775353A