Low-chroma epoxy resin and production process thereof
By adjusting the dosage of eugenol, isomalon and m-chlorperoxybenzoic acid and introducing silane and hexachlorocyclotriphosphazene, combining titanium-coordinated porphyrin compounds and microcapsules, the high color of epoxy resins and the high color of epoxy resins is solved. The problem of poor flame retardancy has achieved the preparation of epoxy resin with low chromaticity, high flame retardancy and self-healing effect.
Patent Information
- Application Number
- CN202411135167.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-22
AI Technical Summary
Existing epoxy resins have limitations in the preparation of low chromaticity and good flame retardancy, and the chromaticity value of commercially available epoxy resins is generally high, which affects customers' visual perception, and antioxidants are compatible in existing processes. Poor properties and not long-lasting curing effect.
By changing the dosage of eugenol, isomalon and m-chlorperoxybenzoic acid and the ratio of m-chlorperoxybenzoic acid to solvents, silane and hexachlorocyclotriphosphazene are introduced, combining titanium-coordinated porphyrin compounds and Microcapsules, adjust the types and dosage of curing agents and accelerators, and adopt nitrogen protection technology to form low-color epoxy resin.
The vertical combustion grade of low-chromatic epoxy resin is achieved to V0 and V1, the tensile strength and impact strength are significantly improved, and it has good self-repair effect and long-lasting antioxidant properties, and the chromaticity value is reduced to 0.4-4.1.
Smart Images

Figure CN118994849A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of epoxy resin synthesis, in particular to a low-chroma epoxy resin and a production process thereof. Background Art
[0002] Epoxy resins are mainly used in coatings, adhesives, engineering plastics and other fields, with a wide range of applications. Epoxy resins can be synthesized into different epoxy resins according to their sources. The synthesis process generally involves reacting the raw materials with excess epichlorohydrin to form ether bonds and epoxy resins containing epoxy groups under alkaline conditions. Depending on the synthesis principle, unsaturated groups can also be oxidized under the action of an oxidant to obtain epoxy resins. The produced epoxy resins are then subjected to steps such as dissolution, extraction, washing and drying to obtain purified epoxy resins.
[0003] At present, petroleum-based epoxy resin is the most important commercial epoxy resin, among which BPA-type epoxy resin has the highest market share. BPA-type epoxy resin is mainly obtained by reacting epichlorohydrin and bisphenol A in the presence of an alkaline catalyst, but BPA has endocrine activity and as an endocrine disruptor, it affects the environment and human health. Eugenol and magnolia officinalis, as bio-based raw materials, are not environmentally friendly, and the prepared epoxy resins have higher tensile properties and glass transition temperatures. For example, J. Liu, Z. He, G. Wu, et al., Synthesis of a novel nonflammable eugenol-based phosphazene epoxy resin with unique burned intumescent char [J]. Chemical Engineering Journal, 2020, 390: 124620. used eugenol and hexachlorocyclotriphosphazene as raw materials to prepare a hexafunctional epoxy resin with aliphatic diamine D230 as a curing agent. The tensile strength of the epoxy resin was 64.2 MPa and the glass transition temperature was 119 ° C. However, the epoxy equivalent of the epoxy resin prepared by this method was not high.
[0004] Patent CN114410065B discloses "an epoxy resin composition, carbon fiber prepreg, and carbon fiber composite material", which is obtained by combining raw materials of multiple components such as epoxy resin, polyimide resin, toughening agent, nanoparticles, imidazole accelerator and curing agent to obtain a carbon fiber composite material, which has good tensile properties and impact resistance. However, the components are complex, the fusion between the components is reduced, the reaction rate of the imidazole accelerator is fast, the curing effect is uneven, and the mechanical properties of the epoxy resin deteriorate when used alone.
[0005] The chromaticity of epoxy resin directly affects the visual experience of customers. The market demand for some epoxy resins with low chromaticity and transparency is increasing, but the chromaticity values of commercially available epoxy resins are generally high. Patent CN118184959A discloses a "low chromaticity epoxy resin and its production process". In the production process of this patent, antioxidants are always present. The epoxy resin produced by the four-step refining method has low chromaticity and good stability. However, the antioxidant is added to the resin by direct mixing, which has poor compatibility and the anti-oxidation effect of the obtained epoxy resin is not long-lasting.
[0006] Patent CN106008919B discloses "a silane hydrophobically modified phosphorus-containing flame-retardant epoxy resin and its preparation method", which grafts silane and flame-retardant 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide onto epoxy resin by chemical modification, thereby improving the hydrophobicity and flame retardancy of epoxy resin. However, the silane raw material of the invention is a yellow colloid, and the prepared epoxy resin has a high chromaticity.
[0007] Patent CN103881465B discloses "Microcapsules for self-repairing coatings, preparation and application". By preparing microcapsules and water-based fluorocarbon coatings into self-repairing water-based fluorocarbon coatings, when microcracks occur in the coating, the microcapsule cores near the cracks flow out to automatically repair the coating. However, the repair effect of the patent method has "repair errors". When the coating is subjected to pressure, the coating does not crack, but the microcapsules are destroyed under pressure and the cores flow out, resulting in erroneous repair.
[0008] In summary, although many achievements have been made in the production process of epoxy resins, there are still many limitations in preparing epoxy resins with low chroma and good flame retardancy and in expanding the scope of application.
[0009] Therefore, a low-chroma epoxy resin and a production process thereof are proposed. Summary of the invention
[0010] The purpose of the present invention is to provide a low-chroma epoxy resin and a production process thereof. By changing the dosage of multiple raw materials such as eugenol, iso-magnolia phenol and meta-chloroperbenzoic acid and the ratio of meta-chloroperbenzoic acid to solvent, the epoxy equivalent of the epoxy resin intermediate is 272-351 g / mol and the viscosity is 1.5-10.9 Pa·s. By introducing silane and hexachlorocyclotriphosphazene into the resin, the vertical combustion grade of the low-chroma epoxy resin is V0 and V1. By synthesizing an accelerator and adjusting the type and dosage of the curing agent, the cured low-chroma epoxy resin has an elongation at break of 7.8%-14.1%, a tensile strength of 28.2-48.6 MPa, and an impact strength of 14.7-26.3 KJ / m 2. By synthesizing titanium-coordinated porphyrin compounds and using them in epoxy resin, the entire production process is filled with nitrogen, and the Gardner chromaticity of the low-color epoxy resin is 0.4-4.1. By introducing two-component microcapsules into the reaction system, the scratch repair test results of the low-color epoxy resin show that it has a good self-repairing effect.
[0011] To achieve the above object, the present invention provides the following technical solutions:
[0012] In one aspect, the present invention provides a production process for a low-chroma epoxy resin, characterized in that it comprises the following steps:
[0013] A hexachlorocyclotriphosphazene solution containing 75-113 parts of hexachlorocyclotriphosphazene is dripped into a mixed solution containing 0-296 parts of eugenol and 0-479 parts of iso-magnoliaol, and 311-622 parts of meta-chloroperbenzoic acid solution are added after stirring and extraction to obtain an epoxy resin intermediate; the ratio of chloroperbenzoic acid to dichloromethane in the meta-chloroperbenzoic acid solution is 1:25-45;
[0014] The structural formula of the epoxy resin intermediate includes the following structure:
[0015]
[0016] The epoxy resin intermediate and silane form epoxy resin in a ratio of 4-189:1-11;
[0017] Dissolving 35 parts of hexachlorocyclotriphosphazene and 114-120 parts of imidazole in tetrahydrofuran to obtain a promoter precursor solution; adding triethylamine to the promoter precursor solution to react to obtain a promoter;
[0018] Adding methanesulfonic acid, the triethylamine and 0-1200 parts of 2-chloroanthraquinone to the reaction solution to obtain an antioxidant precursor; adding 0-65 parts of titanium citrate to the antioxidant precursor, adding a mixed organic solution, heating to 50-60° C., stirring for reaction, and obtaining an antioxidant;
[0019] Adding 38-45 parts of the epoxy resin to the emulsion to obtain core material 1; adding wall liquid to the core material 1 to obtain microcapsule 1; adding a curing agent and the accelerator to 90 parts of the emulsion at a ratio of 10-15:1-2 to obtain core material 2; adding the wall liquid to the core material 2 to obtain microcapsule 2; the microcapsule 1 and the microcapsule 2 form microcapsules at a ratio of 1-20:1-17;
[0020] The epoxy resin is mixed with 167-641 parts of the curing agent, 15-22 parts of the antioxidant, 16.7-64.1 parts of the accelerator and 0-72 parts of the microcapsules, and cured at room temperature for 36 hours, and then cured at 40° C. for 48 hours to obtain a low-color epoxy resin;
[0021] The production process is carried out in a nitrogen atmosphere.
[0022] Preferably, the preparation of the epoxy resin intermediate comprises the following steps:
[0023] The eugenol and the iso-magnolia ol are dissolved in tetrahydrofuran in a reaction kettle to obtain a mixed phenol solution; 100 mL of the triethylamine and potassium carbonate are added to the mixed phenol solution and stirred to obtain a mixed solution; the hexachlorocyclotriphosphazene is dissolved in the tetrahydrofuran to obtain the hexachlorocyclotriphosphazene solution; the mixed solution is heated to 60° C., and nitrogen is introduced into the reaction kettle, and the hexachlorocyclotriphosphazene solution is dripped into the heated mixed solution under stirring, and the dripping is completed within 3.5 hours. After the dripping is completed, the reaction is stirred for 12 hours to obtain a product precursor; the product precursor is extracted with dichloromethane and deionized water and dried, The tetrahydrofuran and the dichloromethane are removed by reduced pressure distillation, and finally vacuum dried for 24 hours to obtain a product intermediate; the product intermediate is dissolved in the dichloromethane to obtain a product intermediate solution; the product intermediate and the dichloromethane in the product intermediate solution have a ratio of 1:25; the m-chloroperbenzoic acid solution is added to the product intermediate solution, and the reaction is stirred at room temperature for 50 hours to obtain an epoxy resin precursor; the epoxy resin precursor is filtered, washed with 15% sodium thiosulfate solution, washed with deionized water, and preliminarily dehydrated with anhydrous magnesium sulfate, and then vacuum dried at 50°C for 48 hours to obtain the epoxy resin intermediate.
[0024] Under the action of potassium carbonate, the hydroxyl groups of eugenol and iso-magnolia phenol react with hexachlorocyclotriphosphazene at the position of the chlorine element to form a structure with hexachlorocyclotriphosphazene as the center and connected by ether bonds, and then triethylamine is added to terminate the reaction. The structural product is dissolved in dichloromethane, extracted with water, separated and dried, and then the olefin bonds in the structure are oxidized into epoxy groups under the action of m-chloroperbenzoic acid to form epoxy resin.
[0025] Preferably, the silane is one of GEOCP-POSS and polydimethylsiloxane.
[0026] The phosphorus and nitrogen elements in hexachlorocyclotriphosphazene play a synergistic flame retardant role in flame retardancy. The phosphorus element forms a stable phosphorus-containing carbon layer in the condensed phase to prevent the combustion reaction process. In addition, PO2· free radicals are generated during the combustion process. This free radical can quench flammable free radicals and terminate the free radical chain reaction of combustion. Under the high temperature conditions of combustion, the nitrogen element generates a flame-retardant gas, which dilutes the concentration of oxygen and combustible mixed gas.
[0027] The Si-O element in GEOCP-POSS is fire-resistant and prevents the combustion process. The cage structure makes the silicon and oxygen elements evenly arranged. The exposed hydroxyl groups of GEOCP-POSS are stably connected with the low-color epoxy resin during the subsequent curing process. The curing agent decomposes under the action of the accelerator, and the carboxyl functional groups formed are stably connected with GEOCP-POSS, which improves the dispersion stability and uniformity of GEOCP-POSS in the system.
[0028] Preferably, the preparation of the antioxidant comprises the following steps:
[0029] The dichloromethane is added to a reactor, and then pyrrole and methyl 4-formylbenzoate are added, and the reaction liquid is obtained by stirring and dissolving; the methylsulfonic acid is added to the reaction liquid, and the triethylamine is added after stirring, and the 2-chloroanthraquinone is added after stirring, and the reaction is continued for 1 hour, and the antioxidant precursor is obtained by separation, elution, and drying; the antioxidant precursor is mixed with the titanium citrate, and the mixed organic solution is added to obtain an antioxidant intermediate reaction liquid; the volume ratio of dichloromethane to methanol in the mixed organic solution is 2:5; the antioxidant intermediate reaction liquid is heated, stirred and reacted for 2 hours, and then the methanol and the dichloromethane are evaporated to remove, filtered, washed with saturated sodium chloride, and then washed with deionized water, and the dichloromethane is added again to dissolve, and n-hexane is added to precipitate and dry to obtain the antioxidant.
[0030] The structural formula of the antioxidant is as follows:
[0031]
[0032] Pyrrole and methyl 4-formylbenzoate are used as raw materials to synthesize tetrakis(p-methoxycarbonylphenyl)N-displaced porphyrin under acidic conditions, and then triethylamine is added to terminate the reaction. Tetrakis(p-methoxycarbonylphenyl)N-displaced porphyrin has high reactivity. In order to achieve its antioxidant effect in epoxy resin, 2-chloroanthraquinone is added as a protective agent to prevent it from being oxidized, and then it forms a titanium-containing porphyrin complex with titanium citrate. After the obtained antioxidant is added to the epoxy resin and cured, the NH bond on the N-displaced porphyrin is connected with the acidic substance after the decomposition of the curing agent, which improves the compatibility of the antioxidant with the epoxy resin system on the one hand, and on the other hand, the NH bond on the N-displaced porphyrin has active chemical properties, and its activity is reduced after being connected with the curing agent, and the durability of the antioxidant is increased.
[0033] Preferably, the 2-chloroanthraquinone is 880-1200 parts.
[0034] Preferably, the titanium citrate is 60-65 parts.
[0035] Preferably, the preparation of the microcapsules comprises the following steps:
[0036] The ammonium chloride, Tween 80 and resorcinol are mixed evenly, deionized water is added, and the mixture is heated and stirred to obtain the emulsion; 38-45 parts of the epoxy resin are added to the emulsion and stirred for 2 hours to obtain the core material 1; urea and formaldehyde are added to the deionized water to dissolve, and then the triethylamine is added to make the pH value 9 to obtain the shell liquid; the core material 1 is heated to 60° C., the shell liquid is added thereto under stirring, the pH value of the system is adjusted to 4, the reaction is stirred for 5 hours, and the microcapsule 1 is obtained by washing, filtering and drying; the solidified The curing agent and the accelerator are added to 90 parts of the emulsion in a ratio of 10-15:1-2 to obtain core material 2; the total amount of the curing agent and the benzyl dimethylamine accelerator is 55 parts; the core material 2 is heated to 60°C, the shell liquid is added thereto under stirring, the pH of the system is adjusted to 4, the reaction is stirred for 5 hours, and the microcapsule 2 is washed, filtered and dried; the microcapsule 1 and the microcapsule 2 are mixed to obtain the microcapsule; the ratio of the microcapsule 1 to the microcapsule 2 in the microcapsule is 1-20:1-17.
[0037] Urea and formaldehyde are used as raw materials to form the wall shell material of the microcapsule. The core material one and the core material two are wrapped by dripping to form microcapsules. The main components of profile one and profile two are curing agent and accelerator, which are consistent with the components of epoxy resin in the main resin, improving the consistency and compatibility of the microcapsules in the main resin. However, excessive addition of microcapsules is not conducive to the repair process. Excessive addition of microcapsules will introduce a large amount of wall shell materials that are inconsistent with the main resin. When the low-chroma epoxy resin is damaged by the outside world, the wrapped materials of microcapsules one and microcapsule two leak out, and the leaked two components of raw materials are cured after contact, thereby achieving a slow curing effect. If the two core material components of capsule one and microcapsule two are wrapped in the same wall shell material, the microcapsules will be cured during the curing process of the epoxy resin, and the self-repair effect after damage cannot be achieved.
[0038] Preferably, the curing agent is one of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, dodecenylsuccinic anhydride, dodecahydro-9,10-phenanthrene dicarboxylic anhydride, 4-cyclohexene-1,2-dicarboxylic acid dialkyl ester and pentaerythritol tetra(ethylhexanoate).
[0039] After the epoxy resin is mixed with the curing agent and the accelerator, the anhydride curing agent opens with the epoxy group in the epoxy resin to form a hydroxyl group for curing under room temperature curing and heating conditions. The curing reaction process is accelerated under the action of the accelerator. Imidazole has high reactivity. After adding it to the reaction system, the catalytic rate is fast, which will lead to inconsistent curing speeds and uneven curing of various parts of the epoxy resin, and ultimately lead to incomplete curing, which ultimately affects the mechanical properties of the low-chroma epoxy resin. The nitrogen position of imidazole No. 1 is capped and connected with hexachlorocyclotriphosphazene to avoid the problem of excessive catalytic activity of active hydrogen at the nitrogen position No. 1. Under the conditions of accelerator and heating, the ester curing agent promotes the breakage of the ester curing agent, and the formed carboxylic acid compound reacts with the epoxy resin to cure.
[0040] Preferably, the amount of the microcapsules is 26-72 parts.
[0041] On the other hand, the present invention provides a low-chroma epoxy resin, characterized in that: the low-chroma epoxy resin comprises an epoxy resin, a curing agent, an accelerator, an antioxidant and microcapsules; the low-chroma epoxy resin is prepared by the production process of the low-chroma epoxy resin as described in any one of the above items; the epoxy equivalent of the epoxy resin intermediate is 272-351 g / mol, and the viscosity of the epoxy resin intermediate is 1.5-10.9 Pa·s; the vertical burning grade of the low-chroma epoxy resin is V0 and V1; the elongation at break of the low-chroma epoxy resin is 7.8%-14.1%, the tensile strength is 28.2-48.6 MPa, and the impact strength is 14.7-26.3 KJ / m 2 ; The Gardner chromaticity of the low-chroma epoxy resin is 0.4-4.1; The scratch repair test results of the low-chroma epoxy resin are -, ++ and +++.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] 1. By using hexachlorocyclotriphosphazene, eugenol and iso-magnolia ol as raw materials, changing the dosage of eugenol, iso-magnolia ol and meta-chloroperbenzoic acid and the ratio of meta-chloroperbenzoic acid to solvent, the relative content of olefinic bonds in the product changes, and the olefinic bonds are oxidized to form epoxy groups under the action of meta-chloroperbenzoic acid. Changing the above conditions makes the epoxy resin intermediate have moderate epoxy equivalent and viscosity, and stable basic physical properties.
[0044] 2. By introducing silane into the epoxy resin intermediate, the GEOCP-POSS in the silane is stably connected to the resin through chemical bonds during the subsequent curing process of the resin. The phosphorus and nitrogen elements in hexachlorocyclotriphosphazene can play an effective flame retardant role. The low-color epoxy resin obtained by using silane and hexachlorocyclotriphosphazene together has a good vertical combustion rating.
[0045] 3. By adding different types of curing agents to the epoxy resin and changing the production process of the synthesized accelerator, the low-color epoxy resin obtained has good mechanical properties. By changing the type and amount of the curing agent, changing the amount of imidazole in the synthetic accelerator and controlling the amount of the accelerator, the curing agent reacts with the open-ring epoxy group, and the accelerator promotes the curing process, the cured low-color epoxy resin has good tensile properties.
[0046] 4. Metal-coordinated porphyrin compounds are prepared by using pyrrole, methyl 4-formylbenzoate and titanium citrate. Porphyrin compounds have a structure of 18π conjugated electrons, high stability and aromaticity, and therefore have good antioxidant effects. They can be used in epoxy resins to prepare low-chroma epoxy resins. Nitrogen runs through the entire production process, which greatly avoids the oxidation of various components in the epoxy resin, thereby reducing the chromaticity value.
[0047] 5. By adding microcapsules, low-color epoxy resin has a good self-repairing effect. Epoxy resin, curing agent and accelerator are made into different microcapsules respectively. The composition of the microcapsules is the same as the main component of the epoxy resin. The fusion degree of the microcapsules and the epoxy resin is better. In addition, the self-repairing function of the low-color epoxy resin is realized. Compared with the formation of new chemical bonds after the chemical bonds are broken, the repair effect is more stable. The functional group repair effect of chemical bonds such as unsaturated carbon-carbon double bonds, carbon-carbon triple bonds and disulfide bonds is poor. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is a graph showing the viscosity changes with temperature in Example 4;
[0049] Figure 2 This is a SEM electron microscope image of the low-chroma epoxy resin repair effect of Example 49 of the present invention. DETAILED DESCRIPTION
[0050] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] See also Figure 1 to Figure 2 The present invention provides a low-chroma epoxy resin and a production process thereof, and the technical scheme is as follows:
[0052] Glycidyl ether oxypropyl caged polysilsesquioxane-POSS (GEOCP-POSS) was purchased from Xi'an Qiyue Biotechnology Co., Ltd.; the basic properties of the material are as follows:
[0053] Appearance Colorless transparent viscous liquid Viscosity 4800cps density 1.25g / mL Molecular weight 1337.88 Epoxy equivalent 167 Refractive Index 1.51 Resin solubility Soluble in epoxy resin, polyurethane resin, acrylic resin
[0054] Methyltetrahydrophthalic anhydride, CAS: 11070-44-3; Methylhexahydrophthalic anhydride, CAS: 34090-76-1; Dodecenylsuccinic anhydride, CAS: 19780-11-1; Dodecahydro-9,10-phenanthrene dicarboxylic anhydride, CAS: 51037-16-2; 4-cyclohexene-1,2-dicarboxylic acid dialkyl esters, CAS: 7042-40-2; Pentaerythritol tetra(ethylhexanoate), CAS: 7299-99-2; 2-Chloroanthraquinone, CAS: 131-09-9; Benzyldimethylamine, CAS: 103-83-3.
[0055] Examples 1-11
[0056] Dissolve 0-296 parts of eugenol and 0-479 parts of iso-magnolia ol in 1.5L of tetrahydrofuran in a reactor to obtain a mixed phenol solution; add 100mL of triethylamine and 274 parts of potassium carbonate to the mixed phenol solution and stir evenly to obtain a mixed solution; dissolve 104 parts of hexachlorocyclotriphosphazene in 1L of tetrahydrofuran to obtain a hexachlorocyclotriphosphazene solution; heat the mixed solution to 60°C, introduce nitrogen into the reactor, drop the hexachlorocyclotriphosphazene solution into the heated mixed solution under stirring, control the dropwise addition to be completed within 3.5 hours, stir the reaction for 12 hours after the dropwise addition is completed to obtain a product precursor; extract the product precursor with dichloromethane and deionized water and dry it, and remove tetrahydrofuran and dichloromethane by reduced pressure distillation, Finally, vacuum drying for 24 hours obtains the product intermediate; the product intermediate is dissolved in dichloromethane to obtain a product intermediate solution; the ratio of the product intermediate to dichloromethane in the product intermediate solution is 1:25; m-chloroperbenzoic acid solution is added to the product intermediate solution, and the reaction is stirred at room temperature for 50 hours to obtain an epoxy resin precursor; the ratio of chloroperbenzoic acid to dichloromethane in the m-chloroperbenzoic acid solution is 1:25-45; the total amount of m-chloroperbenzoic acid is 311-622 parts; the epoxy resin precursor is filtered, washed with 15% sodium thiosulfate solution, washed with deionized water, and preliminarily dehydrated with anhydrous magnesium sulfate, and then vacuum dried at 50°C for 48 hours to obtain an epoxy resin intermediate.
[0057] The detailed information of the production process of epoxy resin intermediates is shown in Table 1.
[0058] Table 1 Production process conditions of epoxy resin intermediates
[0059]
[0060] Example 12
[0061] The epoxy equivalent and viscosity of the epoxy resin intermediate prepared in Examples 1-11 were measured. The test method for epoxy equivalent is as follows: the epoxy equivalent of the epoxy resin intermediate is determined by direct titration with quaternary ammonium bromide salt, 1.0 part of the epoxy resin intermediate of the example is placed in a beaker, and dissolved with 30 mL of chloroform, then tetraethylammonium bromide reagent and crystal violet indicator are added, and perchloric acid-glacial acetic acid standard solution is used to titrate until the system turns green, which is the titration end point. The viscosity of the epoxy resin intermediate is analyzed by a rotor rheometer instrument, using a rotor with a diameter of 25 mm, controlling the test temperature to 20-60°C, and testing at a heating rate of 3°C / min, where the results of viscosity changes with temperature in Example 4 are shown as follows. Figure 1 The viscosity test results of the epoxy resin of the embodiment at 35° C. are shown in Table 2.
[0062] Table 2 Performance test results of epoxy resin intermediates
[0063]
[0064]
[0065] like Figure 1 As shown, with the increase of the test temperature, the viscosity shows a trend of gradually decreasing, and the increase of temperature reduces the connection strength between the epoxy resin intermediate molecules and reduces the internal friction. As shown in Table 2, by reasonably proportioning the contents of eugenol and iso-magnolia phenol, and connecting with hexachlorocyclotriphosphazene to form epoxy resin intermediates with different epoxy equivalents, the epoxy resin intermediates obtained in the embodiment have an epoxy equivalent of 272-351g / mol, indicating that each epoxy group has a high resin amount and the average molecular weight of the resin is high; the epoxy resin intermediate viscosity of Examples 1-11 is 1.5-10.9Pa·s. Among them, only iso-magnolia phenol is added in Example 1, and the content of the epoxy resin intermediate obtained is the highest, and the viscosity is also the highest, which is not conducive to the subsequent production process and the actual work use. When the dosage of embodiment 6 eugenol and iso-magnolia phenol is 247 parts and 80 parts respectively, the epoxy equivalent is the lowest and the viscosity is also the smallest. The results of embodiments 4, 8-11 show that adjusting the ratio of the number of meta-chloroperbenzoic acid and methylene chloride and the dosage of meta-chloroperbenzoic acid has a greater impact on the epoxy equivalent and viscosity. The epoxy equivalent and viscosity of the epoxy resin intermediate obtained in embodiment 4 are moderate. The epoxy equivalent increases linearly with the content of olefinic bonds in the product intermediate, that is, the higher the relative content of olefinic bonds, the higher the epoxy equivalent. The molecular weight is positively correlated with the viscosity. The more completely the meta-chloroperbenzoic acid is oxidized, the higher the viscosity.
[0066] Examples 13-21
[0067] Comparative Examples 1 and 2
[0068] The difference from Example 4 is that the amount of hexachlorocyclotriphosphazene is changed, and the other production processes for preparing the epoxy resin intermediate remain unchanged. The epoxy resin intermediate is mixed with GEOCP-POSS in a ratio of 4-189:1-11, and stirred to obtain epoxy resin. The specific production process is shown in Table 3.
[0069] The epoxy resin was mixed with 635 parts of pentaerythritol tetra(ethylhexanoate) curing agent, 15 parts of antioxidant, 63.5 parts of accelerator and 26 parts of microcapsules, and cured at room temperature for 36 hours, and then cured at 40° C. for 48 hours to obtain a low-color epoxy resin;
[0070] The preparation method of the accelerator is as follows: 35 parts of hexachlorocyclotriphosphazene and 118 parts of 6,7-dimethyl-1H-naphtho[2,3-d]imidazole are dissolved in 2L of tetrahydrofuran to obtain an accelerator precursor solution; then 50mL of triethylamine is added to the accelerator precursor solution, and the temperature is increased to 60°C, and after stirring for 24 hours, the accelerator is filtered and evaporated to remove the organic reagent and unreacted raw materials, and finally the accelerator is washed and vacuum dried to obtain the accelerator;
[0071] The preparation method of the antioxidant is as follows: 800 mL of dichloromethane is added to a reactor, and then 335 parts of pyrrole and 820 parts of methyl 4-formylbenzoate are added, and the reaction liquid is obtained by stirring and dissolving; 335 parts of methylsulfonic acid are added to the reaction liquid, and 3.2 mL of triethylamine is added after stirring for 60 minutes, and 1135 parts of 2-chloroanthraquinone are added after stirring for 2 minutes, and the reaction is continued for 1 hour, and the antioxidant precursor is obtained by separation, elution, and drying; 10 parts of the antioxidant precursor are mixed with 60 parts of titanium citrate, and 800 mL of a mixed organic solution is added to obtain an antioxidant intermediate reaction liquid; the volume ratio of dichloromethane to methanol in the mixed organic solution is 2:5; the antioxidant intermediate reaction liquid is heated to 50°C, stirred for reaction for 2 hours, and then methanol and dichloromethane are evaporated to remove, filtered, washed with saturated sodium chloride, and then washed with deionized water, and dichloromethane is added again to dissolve, and n-hexane is added to precipitate and dried to obtain an antioxidant;
[0072] The preparation method of the microcapsule is as follows: 0.5 parts of ammonium chloride, 0.5 parts of Tween 80 and 0.5 parts of resorcinol are mixed evenly, 80 mL of deionized water is added thereto and mixed evenly, and heated and stirred to obtain an emulsion; 40 parts of epoxy resin are added to the emulsion and stirred for 2 hours to obtain a core material 1; 15 parts of urea and 30 parts of formaldehyde are added to 150 mL of deionized water to dissolve, and then triethylamine is added to make the pH value 9 to obtain a shell liquid; the core material 1 is heated to 60°C, the shell liquid is added thereto under stirring, the pH value of the system is adjusted to 4, and the reaction is stirred. The reaction mixture was stirred for 5 hours, and then washed, filtered, and dried to obtain microcapsule 1; the curing agent and the accelerator were added to 90 parts of the emulsion in a ratio of 15:2 to obtain core material 2; the total amount of curing agent pentaerythritol tetra(ethylhexanoate) ester and accelerator benzyldimethylamine was 55 parts; the core material 2 was heated to 60°C, and the shell liquid was added thereto under stirring, the pH of the system was adjusted to 4, the reaction was stirred for 5 hours, and the reaction was washed, filtered, and dried to obtain microcapsule 2; microcapsule 1 and microcapsule 2 constituted a microcapsule; the ratio of microcapsule 1 to microcapsule 2 in the microcapsule was 1:1.
[0073] All production processes are carried out under the condition of nitrogen as protective gas.
[0074] Table 3 Changes in the dosage of hexachlorocyclotriphosphazene and GEOCP-POSS in the production process of epoxy resin intermediates
[0075]
[0076]
[0077] Comparative Example 3
[0078] The difference from Example 4 is that GEOCP-POSS is replaced by an equal amount of polydimethylsiloxane.
[0079] Embodiment 22
[0080] The low-chroma epoxy resins prepared in Examples 13-21 and Comparative Examples 1-3 were subjected to flame retardant performance tests. According to UL94 "Test Method for Combustion Performance of Plastic Materials", a vertical combustion test was performed using a TTech-GBT2408UL94 horizontal vertical combustion tester at 25°C and 52% humidity. The test results were expressed as V0, V1, and V2, where V0 means that it can quickly self-extinguish and there is no melt dripping, and the flame retardant effect is the best, followed by V1, and V2 has the worst flame retardant effect. The flame retardant test results are shown in Table 3.
[0081] The result of table 3 shows that the low chroma epoxy resin prepared by embodiment 13-21 of the present invention has a vertical combustion grade of V0 and V1, and has a good flame retardant effect.Comparative Example 1, compared with the embodiment, improves the consumption of GEOCP-POSS, and the vertical combustion grade is V0, but excessive GEOCP-POSS is not completely fused in the low chroma epoxy resin, and the uniformity of the low chroma epoxy resin is the worst.Comparative Example 2 reduces the consumption of hexachlorocyclotriphosphazene, and the flame retardant grade is V2, and the reduction in the consumption of hexachlorocyclotriphosphazene also makes it incomplete to react with eugenol and iso-magnolia phenol, and the low chroma epoxy resin cannot be fully formed.Comparative Example 3 replaces the silane species with polydimethylsiloxane, and the flame retardant performance is slightly poor, but the low chroma epoxy resin of comparative example 3 is visible to the naked eye after curing.Uniform degradation.In summary, hexachlorocyclotriphosphazene and GEOCP-POSS synergize to jointly improve the flame retardant effect of low chroma epoxy resin.
[0082] Examples 23-32
[0083] According to the production process of Example 16, epoxy resin, antioxidant and microcapsules were prepared.
[0084] The production process conditions and dosage of the accelerator were changed, and the type and dosage of the curing agent were also changed, as shown in Table 4. The epoxy resin and the curing agent, 15 parts of antioxidant, the accelerator and 26 parts of microcapsules were mixed, cured at room temperature for 36 hours, and then cured at 40°C for 48 hours to obtain a low-color epoxy resin.
[0085] Table 4 Accelerator production process, dosage and curing agent change conditions
[0086]
[0087]
[0088] Comparative Example 4
[0089] Different from Example 23, hexachlorocyclotriphosphazene was not added, the amount of imidazole remained unchanged, and the accelerator was produced, and the amount of the accelerator remained unchanged.
[0090] Embodiment 33
[0091] The low-color epoxy resin obtained by curing was subjected to mechanical property tests. The tensile strength, elongation at break and impact strength of the low-color epoxy resin were tested. The tensile properties were measured according to GB / T 1040-2006 "Determination of tensile properties of plastics"; the impact strength was measured according to GB / T2571-1995 "Impact test method for resin castings". The final results are shown in Table 5.
[0092] Table 5 Mechanical properties test results of low chroma epoxy resin
[0093]
[0094]
[0095] As shown in Table 5, the elongation at break of the low-chroma epoxy resins of the embodiments and comparative examples is 7.8%-14.1%, the tensile strength is 28.2-48.6 MPa, and the impact strength is 14.7-26.3 KJ / m 2 . By using two types of curing agents, including anhydride and ester curing agents, changing the dosage of curing agent and accelerator, and changing the dosage of imidazole in the process of synthesizing the accelerator, the low-color epoxy resin is completely cured and has good tensile properties and impact resistance. Example 31 uses pentaerythritol tetra(ethylhexanoate) ester as a curing agent, 120 parts of imidazole, and the dosages of curing agent and accelerator are 641 and 64.1 parts respectively, that is, the dosage ratio of curing agent to accelerator is 10:1. The obtained low-color epoxy resin has the highest elongation at break and tensile strength, but the impact strength is reduced to only 15.0KJ / m 2 The low-color epoxy resin prepared in Example 26 has the highest impact strength. In Comparative Example 4, hexachlorocyclotriphosphazene is not added, and imidazole is directly used as an accelerator. The tensile strength of the low-color epoxy resin is poor and the impact resistance effect is average.
[0096] Examples 34-42
[0097] Comparative Examples 5-7
[0098] Different from Example 16, the following production process is changed, as shown in Table 6.
[0099] Comparative Example 7
[0100] The production process conditions are consistent with those of Example 34, but nitrogen is not introduced in all production processes.
[0101] Embodiment 43
[0102] The chromaticity values of the low-chromaticity epoxy resins of Examples 34-42 and Comparative Examples 5-7 were tested. The specific testing method is as follows: the low-chromaticity epoxy resin was mixed and dissolved with dichloromethane, and then the chromaticity value was tested, the number of parts and mL volume ratio of the epoxy resin to the dichloromethane was 1:5, and the test was performed according to GB / T 22295-2008 "Method for determination of color of transparent liquids (Gardner colorimetric)", and the test results are shown in Table 6.
[0103] As shown in Table 6, the low chromaticity epoxy resin Gardner chromaticity of the embodiment and the comparative example is 0.4-4.1. The smaller the Gardner chromaticity, the smaller the chromaticity value of the epoxy resin, and the higher the purity of the epoxy resin. The Gardner chromaticity of Examples 34-42 is 0.5-1.7, and the chromaticity of the epoxy resin prepared by the comparative example is 2.0-4.1, and the chromaticity value is significantly improved compared with the embodiment. Comparative Examples 5 and 6 do not add antioxidant protective agent and titanium citrate, respectively, and the Gardner chromaticity is improved. Comparative Example 7 does not pass nitrogen, and the chromaticity value is significantly improved. The results show that the porphyrin complex containing titanium is prepared with pyrrole, methyl 4-formylbenzoate and titanium citrate as raw materials, and the amount of each component, the temperature of the reaction and the amount of the porphyrin complex containing titanium in the resin are controlled, and the epoxy resin obtained has a lower chromaticity.
[0104] Table 6 Production process conditions of antioxidants and dosage of antioxidants
[0105]
[0106]
[0107] Examples 44-53
[0108] The difference from Example 16 is that the promoter benzyldimethylamine is replaced with an equal amount of the promoter obtained by the process of Example 29, and the preparation conditions of the microcapsules in the production process are changed, as shown in Table 7.
[0109] Table 7 Changes in the production process of microcapsules and their dosage in the resin
[0110]
[0111] Comparative Example 8
[0112] The difference from Example 16 is that the amount of microcapsules used is 0 parts.
[0113] Embodiment 54
[0114] The low-chroma epoxy resin prepared in Examples 44-53 and Comparative Example 8 was subjected to a scratch repair test. The low-chroma epoxy resin was placed at room temperature for 24 hours, and then its surface was scratched with a scalpel, and the length of the scratch was controlled to be 1.5 cm and the depth of the scratch was 5 mm. The scratched low-chroma epoxy resin was then placed at room temperature for 50 hours, and then the surface repair of the low-chroma epoxy resin was observed under a microscope, and the final repair results were recorded in Table 8. The state of the surface of the low-chroma epoxy resin before scratching was used as a reference index, and the results were recorded as ++++, +++ indicating that the repair effect was good, ++ indicating that the repair effect was reduced, and - indicating that there was no obvious change in the resin scratch, that is, the resin had no repair effect.
[0115] Table 8 Low chroma epoxy resin scratch test test results
[0116]
[0117] The scratch test repair test results are shown in Table 8. In Examples 44-53, by controlling the amount of epoxy resin in core material one, the ratio of the number of curing agent and the accelerator in core material two, the ratio of the number of microcapsules one to microcapsules two, and the amount of microcapsules are reasonably adjusted, the low-chroma epoxy resin obtained has a good self-repairing effect. Compared with Example 52, Example 53 increases the amount of microcapsules and decreases the repair effect. Comparative Example 8 does not add microcapsules, so the low-chroma epoxy resin does not have a self-repairing effect. In summary, the low-chroma epoxy resin prepared by the present invention has been verified by the scratch test and has a good self-repairing effect.
[0118] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production process for low-chroma epoxy resin, Features: The following steps are involved: A hexachlorocyclotriphosphazene solution containing 75-113 parts of hexachlorocyclotriphosphazene is dripped into a mixed solution containing 0-296 parts of eugenol and 0-479 parts of iso-magnoliaol, and 311-622 parts of meta-chloroperbenzoic acid solution are added after stirring and extraction to obtain an epoxy resin intermediate; the ratio of chloroperbenzoic acid to dichloromethane in the meta-chloroperbenzoic acid solution is 1:25-45; The epoxy resin intermediate and silane form epoxy resin in a ratio of 4-189:1-11; Dissolving 35 parts of hexachlorocyclotriphosphazene and 114-120 parts of imidazole in tetrahydrofuran to obtain a promoter precursor solution; adding triethylamine to the promoter precursor solution to react to obtain a promoter; Adding methanesulfonic acid, the triethylamine and 0-1200 parts of 2-chloroanthraquinone to the reaction solution to obtain an antioxidant precursor; adding 0-65 parts of titanium citrate to the antioxidant precursor, adding a mixed organic solution, heating to 50-60° C., stirring for reaction, and obtaining an antioxidant; Adding 38-45 parts of the epoxy resin to the emulsion to obtain core material 1; adding wall liquid to the core material 1 to obtain microcapsule 1; adding a curing agent and the accelerator to 90 parts of the emulsion at a ratio of 10-15:1-2 to obtain core material 2; adding the wall liquid to the core material 2 to obtain microcapsule 2; the microcapsule 1 and the microcapsule 2 form microcapsules at a ratio of 1-20:1-17; The epoxy resin is mixed with 167-641 parts of the curing agent, 15-22 parts of the antioxidant, 16.7-64.1 parts of the accelerator and 0-72 parts of the microcapsules, and cured at room temperature for 36 hours, and then cured at 40° C. for 48 hours to obtain a low-color epoxy resin; The production process is carried out in a nitrogen atmosphere.
2. A process for producing a low-chroma epoxy resin according to claim 1, Features: The preparation of the epoxy resin intermediate comprises the following steps: The eugenol and the iso-magnolia ol are dissolved in tetrahydrofuran in a reaction kettle to obtain a mixed phenol solution; 100 mL of the triethylamine and potassium carbonate are added to the mixed phenol solution and stirred to obtain a mixed solution; the hexachlorocyclotriphosphazene is dissolved in the tetrahydrofuran to obtain the hexachlorocyclotriphosphazene solution; the mixed solution is heated to 60° C., and nitrogen is introduced into the reaction kettle, and the hexachlorocyclotriphosphazene solution is dripped into the heated mixed solution under stirring, and the dripping is completed within 3.5 hours. After the dripping is completed, the reaction is stirred for 12 hours to obtain a product precursor; the product precursor is extracted with dichloromethane and deionized water and dried, The tetrahydrofuran and the dichloromethane are removed by reduced pressure distillation, and finally vacuum dried for 24 hours to obtain a product intermediate; the product intermediate is dissolved in the dichloromethane to obtain a product intermediate solution; the product intermediate and the dichloromethane in the product intermediate solution have a ratio of 1:25; the m-chloroperbenzoic acid solution is added to the product intermediate solution, and the reaction is stirred at room temperature for 50 hours to obtain an epoxy resin precursor; the epoxy resin precursor is filtered, washed with 15% sodium thiosulfate solution, washed with deionized water, and preliminarily dehydrated with anhydrous magnesium sulfate, and then vacuum dried at 50°C for 48 hours to obtain the epoxy resin intermediate.
3. A production process for a low-chroma epoxy resin according to claim 1, Features: The silane is one of GEOCP-POSS and polydimethylsiloxane.
4. A process for producing a low-chroma epoxy resin according to claim 1, Features: The preparation of the antioxidant comprises the following steps: The dichloromethane is added to a reactor, and then pyrrole and methyl 4-formylbenzoate are added, and the reaction liquid is obtained by stirring and dissolving; the methylsulfonic acid is added to the reaction liquid, and the triethylamine is added after stirring, and the 2-chloroanthraquinone is added after stirring, and the reaction is continued for 1 hour, and the antioxidant precursor is obtained by separation, elution, and drying; the antioxidant precursor is mixed with the titanium citrate, and the mixed organic solution is added to obtain an antioxidant intermediate reaction liquid; the volume ratio of dichloromethane to methanol in the mixed organic solution is 2:5; the antioxidant intermediate reaction liquid is heated, stirred and reacted for 2 hours, and then the methanol and the dichloromethane are evaporated to remove, filtered, washed with saturated sodium chloride, and then washed with deionized water, and the dichloromethane is added again to dissolve, and n-hexane is added to precipitate and dry to obtain the antioxidant.
5. The production process of a low-chroma epoxy resin according to claim 1, Features: The 2-chloroanthraquinone is 880-1200 parts.
6. The production process of a low-chroma epoxy resin according to claim 1, Features: The titanium citrate is 60-65 parts.
7. The production process of a low-chroma epoxy resin according to claim 1, Features: The preparation of the microcapsules comprises the following steps: The ammonium chloride, Tween 80 and resorcinol are mixed evenly, deionized water is added, and the mixture is heated and stirred to obtain the emulsion; 38-45 parts of the epoxy resin are added to the emulsion and stirred for 2 hours to obtain the core material 1; urea and formaldehyde are added to the deionized water to dissolve, and then the triethylamine is added to make the pH value 9 to obtain the shell liquid; the core material 1 is heated to 60° C., the shell liquid is added thereto under stirring, the pH value of the system is adjusted to 4, the reaction is stirred for 5 hours, and the microcapsule 1 is obtained by washing, filtering and drying; the solidified The curing agent and the accelerator are added to 90 parts of the emulsion in a ratio of 10-15:1-2 to obtain core material 2; the total amount of the curing agent and the benzyl dimethylamine accelerator is 55 parts; the core material 2 is heated to 60°C, the shell liquid is added thereto under stirring, the pH of the system is adjusted to 4, the reaction is stirred for 5 hours, and the microcapsule 2 is washed, filtered and dried; the microcapsule 1 and the microcapsule 2 are mixed to obtain the microcapsule; the ratio of the microcapsule 1 to the microcapsule 2 in the microcapsule is 1-20:1-17.
8. The production process of a low-chroma epoxy resin according to claim 1, Features: The curing agent is one of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, dodecenylsuccinic anhydride, dodecahydro-9,10-phenanthrene dicarboxylic anhydride, 4-cyclohexene-1,2-dicarboxylic acid dialkyl ester and pentaerythritol tetra(ethylhexanoate).
9. The production process of a low-chroma epoxy resin according to claim 1, Features: The amount of the microcapsules is 26-72 parts.
10. A low-color epoxy resin, Features: The low-color epoxy resin comprises epoxy resin, curing agent, accelerator, antioxidant and microcapsule; the low-color epoxy resin is prepared by the production process of the low-color epoxy resin according to any one of claims 1 to 9; the epoxy equivalent of the epoxy resin intermediate is 272-351 g / mol, and the viscosity of the epoxy resin intermediate is 1.5-10.9 Pa·s; the vertical combustion grade of the low-color epoxy resin is V0 and V1; the elongation at break of the low-color epoxy resin is 7.8%-14.1%, the tensile strength is 28.2-48.6 MPa, and the impact strength is 14.7-26.3 KJ / m 2 ; The Gardner chromaticity of the low-chroma epoxy resin is 0.4-4.1; The scratch repair test results of the low-chroma epoxy resin are -, ++ and +++.