High-power PI heating film for high-temperature test of energy storage battery

Through the combination of silicone modified PI film and nanocomposite filler, the thermal conductivity and heat resistance of the PI heating film are improved, and the problem of insufficient thermal conductivity of the PI heating film at high temperatures is solved, and a high-power and environmentally friendly processing process is achieved. .

CN118978807AInactive Publication Date: 2024-11-19WUXI TIANBO ELECTRIC APPLIANCE MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411049796.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The thermal conductivity of PI heating films is insufficient at high temperatures, resulting in more energy loss and difficult processing, especially the thermal imidation temperature of the precursor PAA solution is high, which is not conducive to energy conservation and environmental protection.

Method used

By modifying the molecular chain structure of the PI film by silicone, the thermal imidation temperature is reduced, and nanocomposite fillers with excellent thermal conductivity are filled in the pores of the PI film substrate to improve the thermal conductivity of the PI film.

Benefits of technology

The high-power PI heating film is prepared, with good thermal conductivity, heat resistance and environmentally friendly processing, suitable for high-temperature testing of energy storage batteries, and adapt to higher operating temperature and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974592070000031
    Figure BDA0004974592070000031
  • Figure BDA0004974592070000032
    Figure BDA0004974592070000032
  • Figure BDA0004974592070000041
    Figure BDA0004974592070000041
Patent Text Reader

Abstract

The invention relates to a high-power P I heating film for high-temperature testing of an energy storage battery, and belongs to the technical field of composites.According to the P I heating film, a P I base material is modified through organic silicon, and pores of the base material are filled with nano composite filler; wherein the nano composite filler can be prepared from polytetrafluoroethylene microspheres and any one of nano aluminum nitride, nano boron nitride and carbon nanotubes; the imidization curing temperature of the P I heating film is only 160 DEG C which is far lower than the thermal imidization temperature of a conventional P I film, the P I heating film is energy-saving and environment-friendly and has good toughness and dielectric property, the highest glass-transition temperature can reach 342.2 DEG C, the heat resistance is good, the highest heat conductivity coefficient can reach 2.86 W / (m.K), and the heat conductivity is greatly improved compared with that of the conventional P I heating film. Therefore, the P I heating film with higher power can be prepared, and the P I heating film can be widely applied to the fields of electronic components, displays and semiconductor packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of composite materials, and in particular, relates to a high-power PI heating film for high-temperature testing of energy storage batteries. Background Art

[0002] PI heating film is a heating element made of metal heat sink and polyimide (PI) film. The polyimide film in the raw material of PI heating film is a high-performance engineering plastic. Since its commercialization in the 1950s, it has shown broad application prospects in electronics, chemical industry, new energy, medical and other fields. It has excellent high temperature resistance, low temperature resistance, chemical corrosion resistance, high insulation strength and good mechanical properties.

[0003] The working principle of PI heating film mainly depends on the electrothermal effect of metal heat sink and the thermal conductivity of PI film. When current passes through the metal heat sink, according to Ohm's law, electrical energy will be converted into thermal energy, causing the metal sheet to heat up. Since the metal sheet has good thermal conductivity, the thermal energy will be quickly transferred to the PI film, and further transferred to the heated object through the PI film. At the same time, as an insulating layer, the PI film plays the role of heat insulation and protection of the metal sheet, ensuring the safety and reliability of the heating process. However, the thermal conductivity of the PI film is poor, which will cause the PI heating film to lose more energy during the conduction process. Therefore, in order to increase the power of the heating film, it is necessary to improve the thermal conductivity of the PI film. In addition, the processing of the PI film is difficult, especially the precursor PAA solution usually requires a high temperature of 200-300°C during thermal imidization, which is not conducive to energy saving and environmental protection. Reducing the thermal imidization temperature of the PI film and increasing the thermal conductivity of the PI heating film are the primary problems that need to be solved to improve the PI heating film. Summary of the invention

[0004] The purpose of the present invention is to provide a high-power PI heating film for high-temperature testing of energy storage batteries. The molecular chain structure of PAA, a precursor for preparing the PI film, is changed by introducing a silicon structure through organic silicon modification. Organic silicon generally has lower surface energy and better flexibility. These characteristics make it easier for the molecular chain of the PAA modified with organic silicon to move and rearrange during heat treatment, thereby reducing the activation energy during imidization, thereby reducing the thermal imidization temperature of PAA; and the thermal conductivity of the PI film is improved by filling the pores of the PI substrate with an inorganic filler having excellent thermal conductivity.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A high-power PI heating film for high-temperature testing of energy storage batteries is prepared by modifying a PI substrate with organic silicon, and filling the pores of the substrate with nanocomposite fillers.

[0007] A high-power PI heating film for high-temperature testing of energy storage batteries, comprising the following raw materials in parts by mass: 165-190 parts of PAA solution, 14-25 parts of nanocomposite filler, 0.8-1.2 parts of adhesive, and 0.05-0.35 parts of dispersant;

[0008] Furthermore, the nanocomposite filler is prepared from polytetrafluoroethylene microspheres and one of nano-aluminum nitride, nano-boron nitride, and carbon nanotubes in a mass ratio of 6-11:7-13;

[0009] Further, the adhesive is polyacrylate;

[0010] Further, the dispersant is ammonium polyacrylate;

[0011] Further, the PAA solution is prepared by the following steps:

[0012] Step 1: Add 2,6-dimethoxynaphthalene, p-fluorobenzoyl chloride, chloroform and ferric chloride into a three-necked flask, start magnetic stirring, and react at room temperature for 24 hours. After the reaction is completed, add hydrochloric acid to the three-necked flask for neutralization, add methanol for precipitation, filter, and recrystallize the solid obtained by filtration to obtain intermediate 1;

[0013] The reaction process is as follows:

[0014]

[0015] Step 2: Add intermediate 1 and chloroform into a three-necked flask, start magnetic stirring, and drop boron tribromide into the flask using a high-pressure dropping pump. After the dropwise addition is completed, react at room temperature for 24 hours. After the reaction is completed, rotary evaporation is performed to obtain intermediate 2;

[0016] The reaction process is as follows:

[0017]

[0018] Step 3: Add intermediate 2, 4-chlorophthalic anhydride, potassium carbonate solution, and dimethylacetamide into a three-necked flask, install a condenser and a thermometer, turn on magnetic stirring, and react at a temperature of 50-60°C for 2h. After the reaction is completed, separate the organic layer with a separatory funnel and rotary evaporate to obtain intermediate 3;

[0019] The reaction process is as follows:

[0020]

[0021] Step 4: Add intermediate 3, 1,3-bis(aminopropyl)tetramethyldisiloxane, sulfone, tetrahydrofuran, and methyl 3-methoxypropionate into a high-pressure reactor, start magnetic stirring, and react at room temperature for 8 hours to obtain a PAA solution that can be used for PI film processing. Heat the PAA solution at 160° C. for imidization for 24 hours to obtain the organosilicon-modified PI film;

[0022] The reaction process is as follows:

[0023]

[0024] Further, the amount ratio of 2,6-dimethoxynaphthalene, p-fluorobenzoyl chloride, chloroform and ferric chloride used in step 1 is 0.1 mol: 0.19-0.2 mol: 180-200 g: 2.4-3 g;

[0025] Furthermore, the usage ratio of the intermediate 1, chloroform and boron tribromide used in step 2 is 0.08 mol:150-180 g:0.32-0.48 mol;

[0026] Furthermore, the potassium carbonate solution in step 3 is a potassium carbonate solution with a mass fraction of 40%, and the amount ratio of the intermediate 2,4-chlorophthalic anhydride, potassium carbonate solution, and dimethylacetamide used in step 3 is 0.05 mol: 0.1-0.11 mol: 80 g: 80-100 g;

[0027] Further, the amount ratio of intermediate 3, 1,3-bis(aminopropyl)tetramethyldisiloxane, dapsone, tetrahydrofuran, and methyl 3-methoxypropionate used in step 4 is 0.04 mol: 0.02-0.04 mol: 0.04-0.06 mol: 80-100 g: 80-100 g, and the sum of the amounts of 1,3-bis(aminopropyl)tetramethyldisiloxane and dapsone is 0.08 mol;

[0028] Furthermore, a method for preparing a high-power PI heating film for high-temperature testing of an energy storage battery comprises the following steps:

[0029] Step 1: Prepare various raw materials according to mass proportions, mix the nanocomposite filler, dispersant, binder and water, and stir at high speed to emulsify to form a water-based mixed suspension;

[0030] Step 2: Evenly mix the water-based mixed suspension and the PAA solution, degas and cast into a film;

[0031] Step 3: heating the film for imidization to obtain the PI heating film;

[0032] Furthermore, in the second step, the stirring speed range is 7500-8500 r / min, and the stirring time condition is 30-45 min;

[0033] Furthermore, the imidization condition in the third step is heating at a temperature of 160° C. for 24 h.

[0034] Beneficial effects of the present invention:

[0035] 1) The present invention uses silicone-modified PI as a substrate, and fills nano-composite fillers in the pores of the substrate to prepare a high-power PI heating film for high-temperature testing of energy storage batteries. The PI heating film of the present invention can be adapted to a variety of inorganic fillers, has excellent thermal conductivity, and is simple to process. The thermal imidization temperature is low, and it is energy-saving and environmentally friendly.

[0036] 2) The present invention uses 2,6-dimethoxynaphthalene and p-fluorobenzoyl chloride as raw materials and ferric chloride as a catalyst to undergo an electrophilic substitution reaction to obtain an intermediate 1, uses boron tribromide to remove the methyl group of the intermediate 1 to obtain an intermediate 2 having two hydroxy groups, and then uses the Williamson synthesis method to cause a nucleophilic substitution reaction between the intermediate 2 and 4-chlorophthalic anhydride to obtain an intermediate 3, and finally copolymerizes the intermediate 3, 1,3-bis(aminopropyl)tetramethyldisiloxane, and aminophenylsulfone in a mixed solvent of tetrahydrofuran and 3-methoxymethylpropionate to obtain a processable PAA solution, and the PAA solution can obtain the organosilicon-modified PI after thermal imidization; organosilicon generally has lower surface energy and better flexibility, and the present invention introduces 1,3-bis(aminopropyl)tetramethyldisiloxane into the organosilicon structure to modify the PI film, so that the PAA molecular chain is more likely to move and rearrange, thereby reducing the activation energy in the PAA thermal imidization process, thereby reducing The temperature required for the low-heat imidization process, not only that, the silicone structure also has good inorganic affinity, so it can be more fully combined with inorganic fillers during the preparation of the PI heating film; the flexible groups (ether bonds) in the silicone-modified PI molecules can also reduce the internal stress of the molecules, and can also play a role in reducing the imidization temperature. Not only that, the introduction of flexible groups can also make the cured PI film have better toughness; the fluorine atoms introduced by p-fluorobenzoyl chloride can effectively improve the dielectric properties of the PI film after curing. Lower dielectric properties mean that the degree of polarization of the material in the electric field is lower, so energy loss can be reduced, thereby improving heating efficiency; the silicone-modified PI molecules of the present invention have a higher content of rigid groups (naphthalene rings, benzene), and these rigid groups can effectively increase the glass transition temperature of the PI film and improve the thermal stability of the PI film, so that the final PI film can withstand higher temperatures, thereby increasing the power consumption of the PI heating film.

[0037] 3) The PI heating film of the present invention has good heat resistance and can adapt to higher operating temperatures. The low dielectric properties and good thermal conductivity can reduce the loss of the PI heating film during heat conduction. The processing method is simple, and the thermal imidization temperature is low, which is energy-saving and environmentally friendly. Not only that, it also has good toughness and can be widely used in electronic components, displays, and semiconductor packaging fields. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] A PAA solution is prepared by the following steps:

[0041] Step 1: 0.1 mol 2,6-dimethoxynaphthalene, 0.19 mol p-fluorobenzoyl chloride, 180 g chloroform and 2.4 g ferric chloride were added into a container and reacted at room temperature for 24 h. After the reaction was completed, hydrochloric acid was added into the container for neutralization, methanol was added for precipitation, and the solid obtained by filtration was recrystallized to obtain intermediate 1;

[0042] Step 2: 0.08 mol of intermediate 1 and 150 g of chloroform were added into a container, and 0.32 mol of boron tribromide was added dropwise thereto. After the addition was completed, the reaction was carried out at room temperature for 24 hours. After the reaction was completed, the intermediate 2 was obtained by rotary evaporation;

[0043] Step 3: 0.05 mol of intermediate 2, 0.1 mol of 4-chlorophthalic anhydride, 80 g of 40% potassium carbonate solution, and 80 g of dimethylacetamide were added into a container, and reacted at 50°C for 2 h. After the reaction, the organic layer was separated by a separatory funnel, and the intermediate 3 was obtained by rotary evaporation;

[0044] Step 4: 0.04 mol of intermediate 3, 0.04 mol of 1,3-bis(aminopropyl)tetramethyldisiloxane, 0.04 mol of sulfone, 80 g of tetrahydrofuran, and 80 g of methyl 3-methoxypropionate were added into a container and reacted at room temperature for 8 h to obtain a PAA solution that can be used for processing.

[0045] Example 2

[0046] A PAA solution is prepared by the following steps:

[0047] Step 1: 0.1 mol 2,6-dimethoxynaphthalene, 0.195 mol p-fluorobenzoyl chloride, 190 g chloroform and 2.7 g ferric chloride were added into a container and reacted at room temperature for 24 hours. After the reaction was completed, hydrochloric acid was added into the container for neutralization, methanol was added for precipitation, and the solid obtained by filtration was recrystallized to obtain intermediate 1;

[0048] Step 2: 0.08 mol of intermediate 1 and 165 g of chloroform were added into a container, and 0.4 mol of boron tribromide was added dropwise thereto. After the addition was completed, the mixture was reacted at room temperature for 24 h. After the reaction was completed, intermediate 2 was obtained by rotary evaporation;

[0049] Step 3: 0.05 mol of intermediate 2, 0.105 mol of 4-chlorophthalic anhydride, 80 g of 40% potassium carbonate solution, and 90 g of dimethylacetamide were added into a container, and reacted at 55°C for 2 h. After the reaction, the organic layer was separated by a separatory funnel, and the intermediate 3 was obtained by rotary evaporation;

[0050] Step 4: 0.04 mol of intermediate 3, 0.03 mol of 1,3-bis(aminopropyl)tetramethyldisiloxane, 0.05 mol of sulfone, 90 g of tetrahydrofuran, and 90 g of methyl 3-methoxypropionate were added to a container and reacted at room temperature for 8 h to obtain a PAA solution that can be used for processing.

[0051] Example 3

[0052] A PAA solution is prepared by the following steps:

[0053] Step 1: 0.1 mol 2,6-dimethoxynaphthalene, 0.2 mol p-fluorobenzoyl chloride, 200 g chloroform and 3 g ferric chloride are added into a container and reacted at room temperature for 24 hours. After the reaction is completed, hydrochloric acid is added into the container for neutralization, methanol is added for precipitation, and the solid obtained by filtration is recrystallized to obtain intermediate 1;

[0054] Step 2: 0.08 mol of intermediate 1 and 180 g of chloroform were added into a container, and 0.48 mol of boron tribromide was added dropwise thereto. After the addition was completed, the mixture was reacted at room temperature for 24 h. After the reaction was completed, intermediate 2 was obtained by rotary evaporation;

[0055] Step 3: 0.05 mol of intermediate 2, 0.11 mol of 4-chlorophthalic anhydride, 80 g of 40% potassium carbonate solution, and 100 g of dimethylacetamide were added into a container, and reacted at 60° C. for 2 h. After the reaction was completed, the organic layer was separated with a separatory funnel, and the intermediate 3 was obtained by rotary evaporation;

[0056] Step 4: 0.04 mol of intermediate 3, 0.02 mol of 1,3-bis(aminopropyl)tetramethyldisiloxane, 0.06 mol of sulfone, 100 g of tetrahydrofuran, and 100 g of methyl 3-methoxypropionate were added to a container, and reacted at room temperature for 8 hours to obtain a PAA solution that can be used for processing.

[0057] Example 4

[0058] A high-power PI heating film for high-temperature testing of an energy storage battery comprises the following raw materials in parts by mass: 165 parts of the PAA solution obtained in Example 1, 14 parts of a nano-composite filler, 0.8 parts of polyacrylate, and 0.05 parts of ammonium polyacrylate, wherein the nano-composite filler is prepared from polytetrafluoroethylene microspheres and nano-aluminum nitride in a mass ratio of 6:13.

[0059] A method for preparing a high-power PI heating film for high-temperature testing of an energy storage battery comprises the following steps:

[0060] Step 1: Prepare the raw materials according to the mass fraction, mix the nanocomposite filler, dispersant, binder and water, and stir at a high speed of 7500r / min for 30min to emulsify to form a water-based mixed suspension;

[0061] Step 2: Evenly mix the water-based mixed suspension and the PAA solution, degas and cast into a film;

[0062] Step 3: Heat the film at 160° C. for 24 hours for imidization to obtain the PI heating film.

[0063] Example 5

[0064] A high-power PI heating film for high-temperature testing of an energy storage battery comprises the following raw materials in parts by mass: 190 parts of the PAA solution obtained in Example 2, 14 parts of a nano-composite filler, 1 part of a polyacrylate, and 0.25 parts of ammonium polyacrylate, wherein the nano-composite filler is prepared from polytetrafluoroethylene microspheres and nano-boron nitride in a mass ratio of 8:7.

[0065] A method for preparing a high-power PI heating film for high-temperature testing of an energy storage battery comprises the following steps:

[0066] Step 1: Prepare the raw materials according to the mass fraction, mix the nanocomposite filler, dispersant, binder and water, and emulsify the mixture at a high speed of 8000 r / min for 37.5 min to form a water-based mixed suspension;

[0067] Step 2: Evenly mix the water-based mixed suspension and the PAA solution, degas and cast into a film;

[0068] Step 3: Heat the film at 160° C. for 24 hours for imidization to obtain the PI heating film.

[0069] Example 6

[0070] A high-power PI heating film for high-temperature testing of an energy storage battery comprises the following raw materials in parts by mass: 165 parts of the PAA solution obtained in Example 3, 25 parts of a nanocomposite filler, 1.2 parts of polyacrylate, and 0.35 parts of ammonium polyacrylate, wherein the nanocomposite filler is prepared from polytetrafluoroethylene microspheres and carbon nanotubes in a mass ratio of 11:7.

[0071] A method for preparing a high-power PI heating film for high-temperature testing of an energy storage battery comprises the following steps:

[0072] Step 1: Prepare the raw materials according to the mass fraction, mix the nanocomposite filler, dispersant, binder and water, and emulsify at 8500r / min for 45min to form a water-based mixed suspension;

[0073] Step 2: Evenly mix the water-based mixed suspension and the PAA solution, degas and cast into a film;

[0074] Step 3: Heat the film at 160° C. for 24 hours for imidization to obtain the PI heating film.

[0075] Comparative Example 1

[0076] This comparative example is the PI heating film sold by Shenzhen Fulianda New Materials Co., Ltd.

[0077] The PI heating films obtained in Examples 4-6 and the PI heating films sold by Shenzhen Fulianda New Materials Co., Ltd. were subjected to performance tests.

[0078] Dielectric performance test: Dielectric constant test was performed using a dielectric constant tester at a temperature of 25°C.

[0079] Tensile performance test: The test was carried out using Shenzhen Sansi Zongheng electronic tensile testing machine with a test speed of 20mm / min.

[0080] Heat resistance test: refer to ISO11357-2:2002 (DSC) for glass transition temperature test; the test results are shown in Table 1:

[0081] Table 1

[0082]

[0083] It can be seen from Table 1 that the PI heating films obtained by Examples 4-6 have higher thermal conductivity and lower dielectric constant than the PI heating film of Comparative Example 1. High thermal conductivity means high thermal conduction efficiency, and lower dielectric properties mean that the degree of polarization of the material in the electric field is lower, which can also reduce energy loss and improve heating efficiency. The PI heating films obtained by Examples 4-6 can withstand higher tensile strength and have a higher glass transition temperature than the PI heating film of Comparative Example 1, indicating that the PI heating film of the present invention also has better heat resistance and mechanical properties, and can therefore be widely used in electronic components, displays, and semiconductor packaging fields.

[0084] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A high-power PI heating film for high-temperature testing of energy storage batteries, comprising the following raw materials in parts by weight: 165-190 parts of PAA solution, 14-25 parts of nanocomposite filler, 0.8-1.2 parts of adhesive, and 0.05-0.35 parts of dispersant; in, The PAA solution is prepared by the following steps: Step 1, adding 2,6-dimethoxynaphthalene, p-fluorobenzoyl chloride, chloroform and ferric chloride into a container, and reacting at room temperature for 24 hours to obtain intermediate 1; Step 2: Add intermediate 1 and chloroform to chloroform, mix well, add boron tribromide, and react at room temperature for 24 hours to obtain intermediate 2; Step 3: Add intermediate 2, 4-chlorophthalic anhydride, potassium carbonate solution and dimethylacetamide into a container, and react at 50-60° C. for 2 h to obtain intermediate 3; Step 4: Add intermediate 3, 1,3-bis(aminopropyl)tetramethyldisiloxane, sulfone, tetrahydrofuran, and methyl 3-methoxypropionate into a container, and react at room temperature for 8 hours to obtain the PAA solution.

2. The high-power PI heating film for high-temperature testing of energy storage batteries according to claim 1, characterized in that: The amount ratio of 2,6-dimethoxynaphthalene, p-fluorobenzoyl chloride, chloroform and ferric chloride used in step 1 is 0.1 mol: 0.19-0.2 mol: 180-200 g: 2.4-3 g.

3. The high-power PI heating film for high-temperature testing of energy storage batteries according to claim 1, characterized in that: The usage ratio of intermediate 1, chloroform and boron tribromide used in step 2 is 0.08 mol:150-180 g:0.32-0.48 mol.

4. The high-power PI heating film for high-temperature testing of energy storage batteries according to claim 1, characterized in that: The potassium carbonate solution in step 3 is a potassium carbonate solution with a mass fraction of 40%, and the amount ratio of the intermediate 2,4-chlorophthalic anhydride, potassium carbonate solution and dimethylacetamide used in step 3 is 0.05 mol: 0.1-0.11 mol: 80 g: 80-100 g.

5. The high-power PI heating film for high-temperature testing of energy storage batteries according to claim 1, characterized in that: The amount ratio of intermediate 3, 1,3-bis(aminopropyl)tetramethyldisiloxane, sulfone, tetrahydrofuran, and methyl 3-methoxypropionate used in step 4 is 0.04 mol: 0.02-0.04 mol: 0.04-0.06 mol: 80-100 g: 80-100 g.

6. The high-power PI heating film for high-temperature testing of energy storage batteries according to claim 1, characterized in that: The total amount of 1,3-bis(aminopropyl)tetramethyldisiloxane and dapsone used in step 3 is 0.08 mol.

7. The high-power PI heating film for high-temperature testing of energy storage batteries according to claim 1, characterized in that: The nano composite filler is prepared from polytetrafluoroethylene microspheres and one of nano aluminum nitride, nano boron nitride and carbon nano tubes in a mass ratio of 6-11:7-13.

8. The high-power PI heating film for high-temperature testing of energy storage batteries according to claim 1, characterized in that: The adhesive is polyacrylate.

9. The high-power PI heating film for high-temperature testing of energy storage batteries according to claim 1, characterized in that: The dispersant is ammonium polyacrylate.

10. The high-power PI heating film for high-temperature testing of energy storage batteries according to claim 1, characterized in that: The thermal imidization temperature of the PAA solution was 160°C and the time was 24 h.