Preparation method of cationic UV ink-jet color paste for aluminum coating of lithium battery

By combining UV monomer, dispersant, doped sheet-like talc powder and silane regulator, the problem of insufficient adhesion of UV inkjet color paste for lithium battery outer packaging is solved, and the scratch resistance and temperature resistance are significantly improved. , improves the efficiency of the product.

CN118978831AActive Publication Date: 2024-11-19YINGDE KEDI PIGMENT TECH CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410978511.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-19
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The UV inkjet color paste on the outer packaging of existing lithium batteries has poor adhesion performance, resulting in insufficient scratch resistance and temperature resistance, limiting the efficiency of the product.

Method used

Using a combination of UV monomers, dispersants, pigments, glass fiber agents doped with sheet talc and silane regulators, the adhesion and adhesion properties of the color paste are enhanced and the resistance is improved through ball milling and specific solution treatment. Scratch and temperature resistance.

Benefits of technology

It significantly improves the adhesion and scratch resistance of UV inkjet paste, enhances the temperature resistance of the product, and improves the efficiency of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation method of cationic UV ink-jet color paste for an aluminum coating film of a lithium battery. The preparation method comprises the following steps: weighing the following raw materials in parts by weight: 35-45 parts of a UV monomer, 4-7 parts of a dispersing agent, 3-5 parts of a pigment, 5-9 parts of a glass fiber agent doped with flaky talcum powder and 2-4 parts of a silane conditioning agent; the preparation method comprises the following steps: sequentially adding the raw materials into a stirrer, stirring and fully mixing, then carrying out ball-milling treatment in a ball mill at the ball-milling rotating speed of 300r / min for 1 hour, and obtaining the UV ink-jet color paste after the ball-milling is finished. According to the UV ink-jet color paste disclosed by the invention, the UV monomer is matched with the dispersing agent and the pigment, and the glass fiber agent doped with the flaky talcum powder and the silane conditioning agent are added for mutual regulation and mutual coordination, so that the adhesive force performance of a product is enhanced, and the scratch-resistant stability and the temperature-resistant stability of the product are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inkjet color paste, and in particular to a method for preparing a cationic UV inkjet color paste for lithium battery outer-coated aluminum film. Background Art

[0002] The existing lithium battery outer packaging is mainly made of plastic PET film, which is prepared into a colored film by adding coloring to the glue, and then the battery outer packaging is wrapped. This method uses solvent glue, which not only evaporates a large amount of solvent, but also has a single color for battery packaging, and the color adjustment requires the color of the film; while the inkjet printing method can not only solve the problem of color diversity identification, but also the solvent evaporates. The existing UV inkjet color paste has poor film adhesion performance. In order to improve the adhesion, it is easy to cause the product's poor scratch resistance and poor temperature stability, which limits the product's use efficiency. Summary of the invention

[0003] In view of the defects of the prior art, the purpose of the present invention is to provide a cationic UV inkjet color paste for lithium battery outer aluminum film and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0004] The present invention solves the technical problem by adopting the following technical solution: The present invention provides a method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film, comprising the following steps: Weigh the raw materials according to weight: 35-45 parts of UV monomer, 4-7 parts of dispersant, 3-5 parts of pigment, 5-9 parts of glass fiber agent doped with flaky talc, and 2-4 parts of silane regulator; The raw materials were added into a mixer in sequence and stirred and mixed thoroughly, and then ball-milled in a ball mill at a speed of 300 r / min for 1 h. After the ball milling was completed, a UV inkjet color paste was obtained.

[0005] Preferably, the cationic UV inkjet color paste comprises the following raw materials in parts by weight: 40 parts of UV monomer, 5.5 parts of dispersant, 4 parts of pigment, 7 parts of glass fiber agent doped with flaky talc, and 3 parts of silane regulator.

[0006] Preferably, the UV monomer is 1,6-hexanediol diacrylate; the dispersant is TEGO-675; and the pigment is carbon black.

[0007] Preferably, the preparation method of the glass fiber agent doped with flaky talc is: S01: heat-treating the flaky talc at 210-230°C for 10-15min, cooling it to 50-55°C at a rate of 2-5°C / min, immersing it in a sufficient amount of sodium silicate solution and mixing it thoroughly, then filtering it with suction and drying it to obtain a sodium silicate-modified talc powder; S02: 4-7 parts of glass fiber, 1-3 parts of lanthanum nitrate solution, 1-2 parts of carboxymethyl cellulose and 4-7 parts of sodium lignin sulfonate solution are stirred and mixed thoroughly to obtain a glass fiber solution; S03: ball-milling the glass fiber liquid and the sodium silicate-modified talc powder in a weight ratio of 2:5 at a ball-milling speed of 300-500 r / min for 1-2 h. After the ball-milling is completed, washing and drying are performed to obtain a glass fiber agent doped with flaky talc powder.

[0008] Preferably, the mass fraction of the sodium silicate solution is 10-15%.

[0009] Preferably, the mass fraction of the lanthanum nitrate solution is 2-5%; the mass fraction of the sodium lignin sulfonate solution is 8-12%.

[0010] Preferably, the preparation method of the silane regulator is: S101: chitosan, deionized water and glacial acetic acid are mixed uniformly in a weight ratio of 5:11:1, and then a sodium citrate solution with a content of 5-10% of the total amount of chitosan and titanium oxide with a content of 2-5% of the total amount of chitosan are added and stirred to obtain a chitosan modified solution; S102: Add 2-5 parts of silane coupling agent to 4-7 parts of chitosan modified liquid, stir and mix thoroughly to obtain a silane regulator.

[0011] Preferably, the silane coupling agent is silane coupling agent KH560.

[0012] Preferably, the mass fraction of the sodium citrate solution is 10-15%.

[0013] Compared with the prior art, the present invention has the following beneficial effects: The UV inkjet color paste of the present invention adopts UV monomers, dispersants and pigments, and is mutually adjusted and coordinated by adding a glass fiber agent doped with flaky talc and a silane regulator to enhance the adhesion performance of the product and improve the scratch resistance stability and temperature resistance stability of the product. The flaky talc in the glass fiber agent doped with flaky talc is heat-treated at 210-230° C. for 10-15 min, then cooled to 50-55° C. at a rate of 2-5° C. / min, and then immersed in a sufficient amount of sodium silicate solution to optimize the active efficiency of the talc, and then treated with the sodium silicate solution to optimize the stability of the talc, while the glass fiber, lanthanum nitrate solution and carboxymethyl fiber are The glass fiber liquid adjusted by cellulose and sodium lignin sulfonate solution is improved by sodium silicate-modified talc agent, so as to obtain a glass fiber agent distribution system doped with flaky talc. The flaky talc distribution system enhances the adhesion performance of the product, and the glass fiber is reinforced and adjusted to optimize the temperature resistance and scratch resistance stability of the system. The silane regulator adopts chitosan through the preparation of sodium citrate solution and titanium oxide, and then synergized by a silane coupling agent, so that the silane regulator can enhance the interface of the system raw materials, thereby further enhancing the synergistic effect with the glass fiber agent doped with flaky talc, and further improving the scratch resistance and temperature resistance of the product. DETAILED DESCRIPTION

[0014] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0015] A cationic UV inkjet color paste for lithium battery outer aluminum film of this embodiment includes the following raw materials in parts by weight: 35-45 parts of UV monomer, 4-7 parts of dispersant, 3-5 parts of pigment, 5-9 parts of glass fiber agent doped with flaky talc, and 2-4 parts of silane regulator.

[0016] The cationic UV inkjet color paste of this embodiment includes the following raw materials in parts by weight: 40 parts of UV monomer, 5.5 parts of dispersant, 4 parts of pigment, 7 parts of glass fiber agent doped with flaky talc, and 3 parts of silane regulator.

[0017] The UV monomer in this embodiment is 1,6-hexanediol diacrylate; the dispersant is TEGO-675; and the pigment is carbon black.

[0018] The preparation method of the glass fiber agent doped with flaky talc in this embodiment is as follows: S01: heat-treating the flaky talc at 210-230°C for 10-15min, cooling it to 50-55°C at a rate of 2-5°C / min, immersing it in a sufficient amount of sodium silicate solution and mixing it thoroughly, then filtering it with suction and drying it to obtain a sodium silicate-modified talc powder; S02: 4-7 parts of glass fiber, 1-3 parts of lanthanum nitrate solution, 1-2 parts of carboxymethyl cellulose and 4-7 parts of sodium lignin sulfonate solution are stirred and mixed thoroughly to obtain a glass fiber solution; S03: ball-milling the glass fiber liquid and the sodium silicate-modified talc powder in a weight ratio of 2:5 at a ball-milling speed of 300-500 r / min for 1-2 h. After the ball-milling is completed, washing and drying are performed to obtain a glass fiber agent doped with flaky talc powder.

[0019] The mass fraction of the sodium silicate solution in this embodiment is 10-15%.

[0020] The mass fraction of the lanthanum nitrate solution in this embodiment is 2-5%; the mass fraction of the sodium lignin sulfonate solution is 8-12%.

[0021] The preparation method of the silane regulator of this embodiment is: S101: chitosan, deionized water and glacial acetic acid are mixed uniformly in a weight ratio of 5:11:1, and then a sodium citrate solution with a content of 5-10% of the total amount of chitosan and titanium oxide with a content of 2-5% of the total amount of chitosan are added and stirred to obtain a chitosan modified solution; S102: Add 2-5 parts of silane coupling agent to 4-7 parts of chitosan modified liquid, stir and mix thoroughly to obtain a silane regulator.

[0022] The silane coupling agent of this embodiment is silane coupling agent KH560.

[0023] The mass fraction of the sodium citrate solution of the present embodiment is 10-15%.

[0024] A method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film of this embodiment comprises the following steps: The raw materials were added into a mixer in sequence and stirred and mixed thoroughly, and then ball-milled in a ball mill at a speed of 300 r / min for 1 h. After the ball milling was completed, a UV inkjet color paste was obtained.

[0025] Example 1. A cationic UV inkjet color paste for lithium battery outer aluminum film of this embodiment includes the following raw materials in parts by weight: 35 parts of UV monomer, 4 parts of dispersant, 3 parts of pigment, 5 parts of glass fiber agent doped with flaky talc, and 2 parts of silane regulator.

[0026] The UV monomer in this embodiment is 1,6-hexanediol diacrylate; the dispersant is TEGO-675; and the pigment is carbon black.

[0027] The preparation method of the glass fiber agent doped with flaky talc in this embodiment is as follows: S01: The flaky talc powder is first heat-treated at 210°C for 10 minutes, then cooled to 50°C at a rate of 2°C / min, and then immersed in a sufficient amount of sodium silicate solution and mixed thoroughly, followed by suction filtration and drying to obtain a sodium silicate-modified talc powder; S02: 4 parts of glass fiber, 1 part of lanthanum nitrate solution, 1 part of carboxymethyl cellulose and 4 parts of sodium lignin sulfonate solution are stirred and mixed thoroughly to obtain a glass fiber solution; S03: ball-milling the glass fiber liquid and the sodium silicate-modified talc powder in a weight ratio of 2:5 at a ball-milling speed of 300 r / min for 1 h. After the ball-milling is completed, washing and drying are performed to obtain a glass fiber agent doped with flaky talc powder.

[0028] The mass fraction of the sodium silicate solution in this embodiment is 10%.

[0029] The mass fraction of the lanthanum nitrate solution in this embodiment is 2%; the mass fraction of the sodium lignin sulfonate solution is 8%.

[0030] The preparation method of the silane regulator of this embodiment is: S101: chitosan, deionized water and glacial acetic acid are mixed uniformly in a weight ratio of 5:11:1, and then a sodium citrate solution with a total amount of 5% of the total amount of chitosan and a titanium oxide with a total amount of 2% of the total amount of chitosan are added and stirred to obtain a chitosan modified solution; S102: Add 2 parts of silane coupling agent into 4 parts of chitosan modified liquid and stir to mix thoroughly to obtain a silane regulator.

[0031] The silane coupling agent of this embodiment is silane coupling agent KH560.

[0032] The mass fraction of the sodium citrate solution in this embodiment is 10%.

[0033] A method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film of this embodiment comprises the following steps: The raw materials were added into a mixer in sequence and stirred and mixed thoroughly, and then ball-milled in a ball mill at a speed of 300 r / min for 1 h. After the ball milling was completed, a UV inkjet color paste was obtained.

[0034] Example 2. A cationic UV inkjet color paste for lithium battery outer aluminum film of this embodiment includes the following raw materials in parts by weight: 45 parts of UV monomer, 7 parts of dispersant, 5 parts of pigment, 9 parts of glass fiber agent doped with flaky talc, and 4 parts of silane regulator.

[0035] The UV monomer in this embodiment is 1,6-hexanediol diacrylate; the dispersant is TEGO-675; and the pigment is carbon black.

[0036] The preparation method of the glass fiber agent doped with flaky talc in this embodiment is as follows: S01: The flaky talc powder is first heat-treated at 230°C for 15 minutes, then cooled to 55°C at a rate of 5°C / min, and then immersed in a sufficient amount of sodium silicate solution and mixed thoroughly, followed by suction filtration and drying to obtain a sodium silicate-modified talc powder; S02: 7 parts of glass fiber, 3 parts of lanthanum nitrate solution, 2 parts of carboxymethyl cellulose and 7 parts of sodium lignin sulfonate solution are stirred and mixed thoroughly to obtain a glass fiber solution; S03: ball-milling the glass fiber liquid and the sodium silicate-modified talc powder in a weight ratio of 2:5 at a ball-milling speed of 500 r / min for 2 h. After the ball-milling is completed, washing and drying are performed to obtain a glass fiber agent doped with flaky talc powder.

[0037] The mass fraction of the sodium silicate solution in this embodiment is 15%.

[0038] The mass fraction of the lanthanum nitrate solution in this embodiment is 5%; the mass fraction of the sodium lignin sulfonate solution is 12%.

[0039] The preparation method of the silane regulator of this embodiment is: S101: chitosan, deionized water and glacial acetic acid are mixed uniformly in a weight ratio of 5:11:1, and then a sodium citrate solution containing 10% of the total amount of chitosan and titanium oxide containing 5% of the total amount of chitosan are added and stirred to obtain a chitosan modified solution; S102: Add 5 parts of silane coupling agent into 7 parts of chitosan modified liquid and stir to mix thoroughly to obtain a silane regulator.

[0040] The silane coupling agent of this embodiment is silane coupling agent KH560.

[0041] The mass fraction of the sodium citrate solution in this embodiment is 15%.

[0042] A method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film of this embodiment comprises the following steps: The raw materials were added into a mixer in sequence and stirred and mixed thoroughly, and then ball-milled in a ball mill at a speed of 300 r / min for 1 h. After the ball milling was completed, a UV inkjet color paste was obtained.

[0043] Example 3. A cationic UV inkjet color paste for lithium battery outer aluminum film of this embodiment includes the following raw materials in parts by weight: 40 parts of UV monomer, 5.5 parts of dispersant, 4 parts of pigment, 7 parts of glass fiber agent doped with flaky talc, and 3 parts of silane regulator.

[0044] The UV monomer in this embodiment is 1,6-hexanediol diacrylate; the dispersant is TEGO-675; and the pigment is carbon black.

[0045] The preparation method of the glass fiber agent doped with flaky talc in this embodiment is as follows: S01: The flaky talc powder is first heat-treated at 220°C for 12 minutes, then cooled to 52°C at a rate of 3.5°C / min, then immersed in a sufficient amount of sodium silicate solution and mixed thoroughly, then filtered and dried to obtain a sodium silicate-modified talc powder; S02: 5.5 parts of glass fiber, 2 parts of lanthanum nitrate solution, 1.5 parts of carboxymethyl cellulose and 5.5 parts of sodium lignin sulfonate solution are stirred and mixed thoroughly to obtain a glass fiber solution; S03: ball-milling the glass fiber liquid and the sodium silicate-modified talc powder in a weight ratio of 2:5 at a ball-milling speed of 400 r / min for 1.5 h. After the ball-milling is completed, washing and drying are performed to obtain a glass fiber agent doped with flaky talc powder.

[0046] The mass fraction of the sodium silicate solution in this embodiment is 12.5%.

[0047] The mass fraction of the lanthanum nitrate solution in this embodiment is 3.5%; the mass fraction of the sodium lignin sulfonate solution is 10%.

[0048] The preparation method of the silane regulator of this embodiment is: S101: chitosan, deionized water and glacial acetic acid are mixed uniformly in a weight ratio of 5:11:1, and then a sodium citrate solution containing 7.5% of the total amount of chitosan and titanium oxide containing 3.5% of the total amount of chitosan are added and stirred to obtain a chitosan modified solution; S102: Add 3 parts of silane coupling agent into 5 parts of chitosan modified liquid and stir to mix thoroughly to obtain a silane regulator.

[0049] The silane coupling agent of this embodiment is silane coupling agent KH560.

[0050] The mass fraction of the sodium citrate solution in this embodiment is 12.5%.

[0051] A method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film of this embodiment comprises the following steps: The raw materials were added into a mixer in sequence and stirred and mixed thoroughly, and then ball-milled in a ball mill at a speed of 300 r / min for 1 h. After the ball milling was completed, a UV inkjet color paste was obtained.

[0052] Comparative Example 1. The difference from Example 3 is that no glass fiber agent doped with flaky talc is added.

[0053] Comparative Example 2. The difference from Example 3 is that S01 treatment was not used in the preparation of the glass fiber agent doped with flaky talc.

[0054] Comparative Example 3. The difference from Example 3 is that glass fiber liquid treatment is not used in the preparation of the glass fiber agent doped with flaky talc.

[0055] Comparative Example 4. The difference from Example 3 is that the glass fiber liquid preparation method is different: no lanthanum nitrate solution and carboxymethyl cellulose are added.

[0056] Comparative Example 5. The difference from Example 3 is that no silane regulator is added.

[0057] The products of Examples 1-3 and Comparative Examples 1-5 were subjected to performance tests; The products of Examples 1-3 and Comparative Examples 1-5 were scratched 50 times and placed at 65°C for 12 hours to test the scratch resistance and temperature stability of the products. The test performance is as follows:

[0058] It can be seen from Comparative Examples 1-5 and Examples 1-3 that; The product of Example 3 still has excellent bonding strength performance under scratching and temperature resistance conditions. At the same time, no glass fiber agent doped with flaky talc and no silane regulator are added to the product, and the performance of the product deteriorates significantly. In addition, the glass fiber agent doped with flaky talc is not treated with S01, no glass fiber liquid treatment, and no lanthanum nitrate solution and carboxymethyl cellulose are added in the preparation of the glass fiber agent doped with flaky talc, and the performance of the product tends to deteriorate. Only the glass fiber agent doped with flaky talc prepared by the method of the present invention has the most significant product performance effect.

[0059] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0060] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing cationic UV inkjet color paste for lithium battery outer aluminum film, characterized in that: The following steps are involved: Weigh the raw materials according to weight: 35-45 parts of UV monomer, 4-7 parts of dispersant, 3-5 parts of pigment, 5-9 parts of glass fiber agent doped with flaky talc, and 2-4 parts of silane regulator; The raw materials were added into a mixer in sequence and stirred and mixed thoroughly, and then ball-milled in a ball mill at a speed of 300 r / min for 1 h. After the ball milling was completed, a UV inkjet color paste was obtained.

2. The method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film according to claim 1, characterized in that: 40 parts of UV monomer, 5.5 parts of dispersant, 4 parts of pigment, 7 parts of glass fiber agent doped with flaky talc, and 3 parts of silane regulator.

3. The method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film according to claim 1, characterized in that: The UV monomer is 1,6-hexanediol diacrylate; the dispersant is TEGO-675; and the pigment is carbon black.

4. The method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film according to claim 1, characterized in that: The preparation method of the glass fiber agent doped with flaky talc is as follows: S01: heat-treating the flaky talc at 210-230°C for 10-15min, cooling it to 50-55°C at a rate of 2-5°C / min, immersing it in a sufficient amount of sodium silicate solution and mixing it thoroughly, then filtering it with suction and drying it to obtain a sodium silicate-modified talc powder; S02: 4-7 parts of glass fiber, 1-3 parts of lanthanum nitrate solution, 1-2 parts of carboxymethyl cellulose and 4-7 parts of sodium lignin sulfonate solution are stirred and mixed thoroughly to obtain a glass fiber solution; S03: ball-milling the glass fiber liquid and the sodium silicate-modified talc powder in a weight ratio of 2:5 at a ball-milling speed of 300-500 r / min for 1-2 h. After the ball-milling is completed, washing and drying are performed to obtain a glass fiber agent doped with flaky talc powder.

5. The method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film according to claim 4, characterized in that: The mass fraction of the sodium silicate solution is 10-15%.

6. The method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film according to claim 4, characterized in that: The mass fraction of the lanthanum nitrate solution is 2-5%; the mass fraction of the sodium lignin sulfonate solution is 8-12%.

7. The method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film according to claim 1, characterized in that: The preparation method of the silane regulator is: S101: chitosan, deionized water and glacial acetic acid are mixed uniformly in a weight ratio of 5:11:1, and then a sodium citrate solution with a content of 5-10% of the total amount of chitosan and titanium oxide with a content of 2-5% of the total amount of chitosan are added and stirred to obtain a chitosan modified solution; S102: Add 2-5 parts of silane coupling agent to 4-7 parts of chitosan modified liquid, stir and mix thoroughly to obtain a silane regulator.

8. The method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film according to claim 7, characterized in that: The silane coupling agent is silane coupling agent KH560.

9. The method for preparing a cationic UV inkjet color paste for lithium battery outer aluminum film according to claim 7, characterized in that: The mass fraction of the sodium citrate solution is 10-15%.

Citation Information

Patent Citations

  • Preparation method of chitosan / titanium dioxide sol antibacterialpackaging film

    CN104479155A

  • Porous adsorption film and preparation method thereof

    CN104549176A

  • UV inkjet color paste and preparation method and application thereof

    CN107151486A

  • Ultraviolet (UV) inkjet ink pigment paste and preparation method thereof

    CN109401439A

  • Nano color paste for ultraviolet curing ink jet and preparation method of nano color paste

    CN113563761A