Super-hydrophobic anti-icing fan blade coating as well as preparation method and application thereof
By using benzyl chloride fluorine-containing acrylic resin and modified nanoparticles in anti-freezing coatings, the problems of insufficient binding force and poor hydrophobic performance of nanoparticles are solved, and efficient anti-junction of fan blades is achieved Ice effect.
Patent Information
- Application Number
- CN202411306455.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-19
AI Technical Summary
In the existing anti-freezing coatings, the nanoparticles and the matrix have weak bonding force, are prone to fall off, and have poor hydrophobic performance, which cannot effectively prevent the fan blades from freezing.
Use benzyl chloride fluorine-containing acrylic resin to bind to modified nanoparticles, and enhance the binding force by forming C-N bonds with the amino group on the nanoparticles, and cross-linking with hydroxyacrylic resin to cure, avoiding the use of additional curing agents to form efficient Superhydrophobic coating.
The adhesion of nanoparticles and the weather resistance of the coating are improved, the adhesion of ice is significantly reduced, and the superhydrophobic and anti-icing performance is improved.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of functional coatings, and in particular to a super-hydrophobic anti-icing fan blade coating, a preparation method and an application thereof. Background Art
[0002] Outdoor equipment in high-altitude and high-latitude areas, such as wind turbines, often face the problem of icing when operating in winter. Blade icing seriously affects the safe operation of wind power equipment. At present, anti-icing technology can be mainly divided into two categories, namely active and passive. Active methods include heating deicing and mechanical deicing. This method requires additional energy input, and has the problems of excessive energy consumption, low efficiency and inconvenient operation. Passive methods use the physical properties of the blade surface to eliminate or prevent icing. For example, using coatings to prevent icing is low-cost, does not require special protection facilities, and the blades are easy to maintain. However, there is a technology that uses nanoparticles to improve the performance of coatings, but in the prior art, the binding force between nanoparticles and the substrate is weak, the nanoparticles are easy to fall off, and their hydrophobic properties are poor.
[0003] For example, the publication number CN102585635A discloses an "anti-icing coating and its preparation method", which includes a hydroxyl-containing main resin, a curing agent, a hydrophobically modified nano-silica sol, a pigment filler, an additive and a solvent. The obtained coating has a low water contact angle and does not have super hydrophobic properties. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a super-hydrophobic anti-icing fan blade coating, a preparation method and an application thereof.
[0005] The technical solution adopted by the present invention is: a super-hydrophobic anti-icing fan blade coating, which comprises, by mass percentage: 30-70% of benzyl chlorinated fluorinated acrylic resin, 5-20% of modified nanoparticles, 20-60% of hydroxy acrylic resin, 1.5-5% of auxiliary agent, and the balance is solvent.
[0006] Furthermore, the nanoparticles are composed of one or two or more of silicon dioxide, titanium dioxide, zinc oxide, and aluminum oxide mixed in any proportion; the modified nanoparticles are nanoparticles with fluorine-containing groups and amino groups grafted on the surface.
[0007] Furthermore, the auxiliary agents are dispersants and defoamers; the contents of the dispersants and defoamers in the coating are 1-3% of the dispersant and 0.5-2% of the defoamer by mass percentage.
[0008] Further, the structure of the benzyl chlorinated fluorinated acrylic resin is as follows:
[0009] Wherein, R1 is one of hydrogen atom, methyl and ethyl, R2 is an alkyl group with less than 18 carbon atoms, R f is a fluorinated alkyl group, and m and n are positive integers.
[0010] Further, the structure of the cyanoacrylic resin is as follows:
[0011] Wherein, m and n are positive integers, R3 is one of a hydrogen atom, a methyl group and an ethyl group, R4 is an alkyl group with less than 18 carbon atoms, and R5 is an alkyl group with less than 6 carbon atoms.
[0012] A method for preparing a super-hydrophobic anti-icing fan blade coating comprises the following steps: Add benzyl chlorinated fluorinated acrylic resin, modified nanoparticles and additives into a solvent; after fully stirring and dispersing, add hydroxy acrylic resin, continue to stir and disperse evenly, and the desired super hydrophobic anti-icing fan blade coating can be obtained.
[0013] Further, the preparation process of the benzyl chlorinated fluorinated acrylic resin is as follows: Add fluorinated acrylic resin, chloromethylation agent and catalyst into solvent, and react at 20-80°C for 1-12 hours; remove the solvent and wash to obtain the desired benzyl chlorinated fluorinated acrylic resin.
[0014] Furthermore, the preparation method of the modified nanoparticles is as follows: Adding nanoparticles and fluorosilane coupling agent into the solvent, adjusting pH, and performing ultrasonic dispersion; After reacting at 60°C for 5 to 24 hours, an aminosilane coupling agent is added and reacted at this temperature for 5 to 24 hours; after filtering and drying, the desired modified nanoparticles are obtained.
[0015] Further, the chloromethylation agent is one of trimethylsilyl chloride-paraformaldehyde, hydrogen chloride-triformaldehyde, chloromethyl alkyl ether and chloromethyltrimethylsilane; The catalyst is one or a mixture of two or more of tin tetrachloride, aluminum trichloride and zinc chloride in any proportion; The fluorosilane coupling agent is one or a mixture of two or more of tridecafluorooctyltrimethylsilane, tridecafluorooctyltriethoxysilane, heptadecafluorodecyltrimethoxysilane and heptadecafluorodecyltriethoxysilane in any proportion; The aminosilane coupling agent is one or two or more of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane mixed in any proportion.
[0016] An application of a super-hydrophobic anti-icing fan blade coating, wherein the coating is prepared for use as a super-hydrophobic anti-icing coating for fan blades.
[0017] The beneficial effects of the present invention are: (1) The present invention uses benzyl chlorinated fluorinated acrylic resin. The chlorine atom in the benzyl chlorine group is highly active and undergoes a nucleophilic substitution reaction with the amino group on the modified nanoparticles to generate a CN bond, thereby enhancing the binding force between the nanoparticles and the resin and improving the adhesion of the nanoparticles. (2) The present invention uses benzyl chlorinated fluorinated acrylic resin, in which the chlorine atoms can also react with the hydroxyl groups in the hydroxy acrylic resin to achieve cross-linking and curing, avoiding the use of additional curing agents, thereby reducing the overall cost of the coating; (3) The coating formed by the super-hydrophobic anti-icing fan blade coating obtained by the present invention has a large contact angle, a small rolling angle, and good weather resistance; the fluorine-containing structure greatly reduces the surface energy of the fan blade, and the rough nano-surface structure forms an air cushion, which can inhibit the formation of ice layer and effectively reduce the adhesion of ice layer; (4) The preparation method of the present invention is simple, easy to operate, and is conducive to industrial production. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with specific embodiments.
[0019] A super-hydrophobic anti-icing fan blade coating, comprising, by mass percentage: 30-70% of benzyl chlorinated fluorinated acrylic resin, 5-20% of modified nanoparticles, 20-60% of hydroxy acrylic resin, 1.5-5% of auxiliary agent, and the balance is solvent.
[0020] The nanoparticles are composed of one or two or more of silicon dioxide, titanium dioxide, zinc oxide, and aluminum oxide mixed in any proportion; the modified nanoparticles are nanoparticles with fluorine-containing groups and amino groups grafted on the surface. The additives are dispersants and defoamers; the content of dispersants and defoamers in the coating is 1-3% of dispersants and 0.5-2% of defoamers by mass percentage. Dispersants can be BYK-163, BYK-9076, AG-54 and AG-500. Defoamers can be BYK-A530, BYK-1790, RKZ6001 and RKZ6008.
[0021] The amount of solvent added in the coating is 5 to 20% by mass; the solvent is one or more of ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, ethanol, xylene and cyclohexanone.
[0022] The structure of benzyl chlorinated fluorinated acrylic resin is as follows:
[0023] Wherein, R1 is one of hydrogen atom, methyl and ethyl, R2 is an alkyl group with less than 18 carbon atoms, R f is a fluorinated alkyl group, and m and n are positive integers.
[0024] The structure of cyanoacrylate resin is as follows:
[0025] Wherein, m and n are positive integers, R3 is one of a hydrogen atom, a methyl group and an ethyl group, R4 is an alkyl group with less than 18 carbon atoms, and R5 is an alkyl group with less than 6 carbon atoms.
[0026] A method for preparing a super-hydrophobic anti-icing fan blade coating comprises the following steps: Add benzyl chlorinated fluorinated acrylic resin, modified nanoparticles and additives into a solvent; after fully stirring and dispersing, add hydroxy acrylic resin, continue to stir and disperse evenly, and the desired super hydrophobic anti-icing fan blade coating can be obtained.
[0027] The preparation process of benzyl chlorinated fluorinated acrylic resin is as follows: Add fluorinated acrylic resin, chloromethylation agent and catalyst into solvent, react at 20-80°C for 1-12 hours, remove the solvent and wash, and the desired benzyl chlorinated fluorinated acrylic resin can be obtained. The amount of chloromethylation agent and catalyst added depends on the actual situation.
[0028] The preparation method of modified nanoparticles is as follows: Add nanoparticles and fluorosilane coupling agent into solvent, add acetic acid to adjust pH to 4-5, and disperse by ultrasonication; After reacting at 60°C for 5 to 24 hours, add the aminosilane coupling agent and react at this temperature for 5 to 24 hours; after filtering and drying, the desired modified nanoparticles can be obtained. The amount of fluorosilane coupling agent and aminosilane coupling agent added depends on the actual situation.
[0029] The chloromethylation agent is one of trimethylsilyl chloride-paraformaldehyde, hydrogen chloride-triformaldehyde, chloromethyl alkyl ether and chloromethyltrimethylsilane; The catalyst is one or a mixture of two or more of tin tetrachloride, aluminum trichloride and zinc chloride in any proportion; The fluorosilane coupling agent is one or a mixture of two or more of tridecafluorooctyltrimethylsilane, tridecafluorooctyltriethoxysilane, heptadecafluorodecyltrimethoxysilane and heptadecafluorodecyltriethoxysilane in any proportion; The aminosilane coupling agent is one or a mixture of two or more of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane in any proportion.
[0030] Example 1 A method for preparing a super-hydrophobic anti-icing fan blade coating comprises the following steps: First, prepare the benzyl chlorinated fluorinated acrylic resin: Add 50 g of fluorinated acrylic resin (Anhui Zhongen Chemical Co., Ltd.), 21.7 g of trimethylsilyl chloride, 6 g of paraformaldehyde, 13.1 g of tin tetrachloride, and 200 mL of chloroform solvent into a round-bottom flask and stir evenly; The reaction was stirred at 50 °C for 6 hours. After the reaction was completed, chloroform was evaporated under reduced pressure using a rotary evaporator. The obtained product was washed three times with 20 mL of the solution to obtain a benzyl chlorinated fluorinated acrylic resin.
[0031] Preparation of modified nanoparticles: Add 60 g of nano-silica with an average particle size of 200 nm, 11.3 g of heptadecafluorodecyltrimethoxysilane and 500 mL of 90% ethanol aqueous solution into a round-bottom flask. Add acetic acid to adjust the solution pH to 4, ultrasonically disperse for 20 minutes, and stir at 60 °C for 6 hours. Then add 11.1 g of 3-aminopropyltriethoxysilane, continue to stir at 60 °C for 12 hours, filter the product and vacuum dry it at 80 °C for 3 hours to obtain modified nanoparticles.
[0032] Weigh the raw materials according to the following mass percentages: Benzyl chlorinated fluorinated acrylic resin 46%, modified nanoparticles 9%, dispersant BYK-163 1.2%, defoamer BYK-A530 0.8%, mixed solvent 15%. The mixed solvent is composed of butyl acetate, ethanol and xylene.
[0033] After mixing the above components, stir and disperse them for 2 hours, add 28% of hydroxyl acrylic resin (Chenyou Paint Co., Ltd.), and continue to stir and disperse for 3 hours to obtain a super hydrophobic anti-icing fan blade coating.
[0034] Example 2 A method for preparing a super-hydrophobic anti-icing fan blade coating comprises the following steps: First, prepare the benzyl chlorinated fluorinated acrylic resin: Add 50 g of fluorinated acrylic resin (Anhui Zhongen Chemical Co., Ltd.), 24.5 g of chloromethyltrimethylsilane, 13.1 g of tin tetrachloride, and 200 mL of chloroform solvent into a round-bottom flask and stir evenly; The reaction was stirred at 80 °C for 1 hour. After the reaction was completed, chloroform was evaporated under reduced pressure using a rotary evaporator. The obtained product was washed three times with 20 mL of the solution to obtain a benzyl chlorinated fluorinated acrylic resin.
[0035] Preparation of modified nanoparticles: Add 60 g of nano-silica with an average particle size of 200 nm, 11.3 g of heptadecafluorodecyltrimethoxysilane and 500 mL of 90% ethanol aqueous solution into a round-bottom flask. Add acetic acid to adjust the solution pH to 4, ultrasonically disperse for 20 minutes, and stir at 60 °C for 5 hours. Then add 11.1 g of 3-aminopropyltriethoxysilane, continue to stir at 60 °C for 24 hours, filter the product and vacuum dry it at 80 °C for 3 hours to obtain modified nanoparticles.
[0036] Weigh the raw materials according to the following mass percentages: Benzyl chlorinated fluorinated acrylic resin 46%, modified nanoparticles 9%, dispersant BYK-163 1.2%, defoamer BYK-A530 0.8%, mixed solvent 15%. The mixed solvent is composed of butyl acetate, ethanol and xylene.
[0037] After mixing the above components, stir and disperse them for 2 hours, add 28% of hydroxyl acrylic resin (Chenyou Paint Co., Ltd.), and continue to stir and disperse for 3 hours to obtain a super hydrophobic anti-icing fan blade coating.
[0038] Example 3 A method for preparing a super-hydrophobic anti-icing fan blade coating comprises the following steps: First, prepare the benzyl chlorinated fluorinated acrylic resin: Add 50 g of fluorinated acrylic resin (Anhui Zhongen Chemical Co., Ltd.), 24.5 g of chloromethyltrimethylsilane, 13.1 g of tin tetrachloride, and 200 mL of chloroform solvent into a round-bottom flask and stir evenly; The reaction was stirred at 20°C for 12 hours. After the reaction was completed, chloroform was evaporated under reduced pressure using a rotary evaporator. The obtained product was washed three times with 20 mL of the solution to obtain a benzyl chlorinated fluorinated acrylic resin.
[0039] Preparation of modified nanoparticles: 79.8 g of nano-silica with an average particle size of 100 nm, 11.3 g of heptadecafluorodecyltrimethoxysilane and 500 mL of 90% ethanol aqueous solution were added to a round-bottom flask. Acetic acid was added dropwise to adjust the solution pH to 4, ultrasonic dispersion was performed for 20 minutes, and the mixture was stirred and reacted at 60 °C for 24 hours. Then 11.1 g of 3-aminopropyltriethoxysilane was added, and the mixture was stirred and reacted at 60 °C for 5 hours. The product was filtered and vacuum dried at 80 °C for 3 hours to obtain modified nanoparticles.
[0040] Weigh the raw materials according to the following mass percentages: Benzyl chlorinated fluorinated acrylic resin 46%, modified nanoparticles 9%, dispersant BYK-163 1.2%, defoamer BYK-A530 0.8%, mixed solvent 15%. The mixed solvent is composed of butyl acetate, ethanol and xylene.
[0041] After mixing the above components, stir and disperse them for 2 hours, add 28% of hydroxyl acrylic resin (Chenyou Paint Co., Ltd.), and continue to stir and disperse for 3 hours to obtain a super hydrophobic anti-icing fan blade coating.
[0042] Example 4 A method for preparing a super-hydrophobic anti-icing fan blade coating comprises the following steps: The preparation method of benzyl chlorinated fluorinated acrylic resin is as shown in Example 1 Preparation of modified nanoparticles: Add 60 g of nano-silica with an average particle size of 200 nm, 9.4 g of tridecafluorooctyl trimethoxysilane and 500 mL of 90% ethanol aqueous solution into a round-bottom flask. Add acetic acid to adjust the solution pH to 4, ultrasonically disperse for 20 minutes, and stir at 60 °C for 6 hours. Then add 11.1 g of 3-aminopropyl triethoxysilane, continue to stir at 60 °C for 12 hours, filter the product and vacuum dry it at 80 °C for 3 hours to obtain modified nanoparticles.
[0043] Weigh the raw materials according to the following mass percentages: Benzyl chlorinated fluorinated acrylic resin 46%, modified nanoparticles 9%, dispersant BYK-163 1.2%, defoamer BYK-A530 0.8%, mixed solvent 15%. The mixed solvent is composed of butyl acetate, ethanol and xylene.
[0044] After mixing the above components, stir and disperse them for 2 hours, add 28% of hydroxyl acrylic resin (Chenyou Paint Co., Ltd.), and continue to stir and disperse for 3 hours to obtain a super hydrophobic anti-icing fan blade coating.
[0045] Example 5 A method for preparing a super-hydrophobic anti-icing fan blade coating comprises the following steps: The preparation method of benzyl chlorinated fluorinated acrylic resin is as shown in Example 1 Preparation of modified nanoparticles: Add 60 g of nano-silica with an average particle size of 200 nm, 11.3 g of heptadecafluorodecyltrimethoxysilane and 500 mL of 90% ethanol aqueous solution into a round-bottom flask. Add acetic acid to adjust the solution pH to 4, ultrasonically disperse for 20 minutes, and stir at 60 °C for 6 hours. Then add 11.1 g of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, continue to stir at 60 °C for 12 hours, filter the product and vacuum dry it at 80 °C for 3 hours to obtain modified nanoparticles.
[0046] Weigh the raw materials according to the following mass percentages: Benzyl chlorinated fluorinated acrylic resin 46%, modified nanoparticles 9%, dispersant BYK-163 1.2%, defoamer BYK-A530 0.8%, mixed solvent 15%. The mixed solvent is composed of butyl acetate, ethanol and xylene.
[0047] After mixing the above components, stir and disperse them for 2 hours, add 28% of hydroxyl acrylic resin (Chenyou Paint Co., Ltd.), and continue to stir and disperse for 3 hours to obtain a super hydrophobic anti-icing fan blade coating.
[0048] Example 6 A method for preparing a super-hydrophobic anti-icing fan blade coating comprises the following steps: The preparation method of benzyl chlorinated fluorinated acrylic resin is as shown in Example 1 The preparation method of modified nanoparticles is as in Example 1 Weigh the raw materials according to the following mass percentages: Benzyl chlorinated fluorinated acrylic resin 65%, modified nanoparticles 5%, dispersant BYK-9076 1.0%, defoamer BYK-1790 0.5%, solvent 8.5%. The solvent is propylene glycol methyl ether acetate.
[0049] After the above components are mixed, they are stirred and dispersed for 2 hours, 20% of hydroxyl acrylic resin (Chenyou Paint Co., Ltd.) is added, and stirring and dispersion is continued for 3 hours to obtain a super hydrophobic anti-icing fan blade coating.
[0050] Example 7 A method for preparing a super-hydrophobic anti-icing fan blade coating comprises the following steps: The preparation method of benzyl chlorinated fluorinated acrylic resin is as shown in Example 1 The preparation method of modified nanoparticles is as in Example 1 Weigh the raw materials according to the following mass percentages: Benzyl chlorinated fluorinated acrylic resin 30%, modified nanoparticles 20%, dispersant BYK-9076 2.0%, defoamer BYK-1790 3.0%, solvent 10%. The solvent is ethanol.
[0051] After mixing the above components, stir and disperse for 2 hours, add 35% of hydroxyl acrylic resin (Chenyou Paint Co., Ltd.), and continue to stir and disperse for 3 hours to obtain a super hydrophobic anti-icing fan blade coating.
[0052] Example 8 A method for preparing a super-hydrophobic anti-icing fan blade coating comprises the following steps: The preparation method of benzyl chlorinated fluorinated acrylic resin is as shown in Example 1 The preparation method of modified nanoparticles is as in Example 1 Weigh the raw materials according to the following mass percentages: Benzyl chlorinated fluorinated acrylic resin 30%, modified nanoparticles 5%, dispersant BYK-9076 0.5%, defoamer BYK-1790 1.0%, solvent 8.5%. The solvent is cyclohexanone.
[0053] After mixing the above components, stir and disperse them for 2 hours, add 55% of hydroxyl acrylic resin (Chenyou Paint Co., Ltd.), and continue to stir and disperse for 3 hours to obtain a super hydrophobic anti-icing fan blade coating.
[0054] The coatings obtained in Examples 1 to 8 were sprayed on epoxy resin substrates, and after curing at room temperature, performance tests were performed. The results obtained are shown in Table 1.
[0055] Table 1. Test results of coating samples
[0056] It can be seen from Table 1 that the samples obtained in the examples can all achieve a super-hydrophobic effect, wherein the coatings prepared from the samples obtained in Examples 1 and 4 can obtain a water contact angle higher than 160 degrees, have very low ice adhesion, and have more excellent super-hydrophobic and anti-icing properties.
[0057] The coating obtained by the present invention can enhance the binding force and adhesion of nanoparticles through chemical bond connection. The method of directly preparing benzyl-chlorinated fluorinated acrylic resin by chloromethylation reaction, the chlorine atom in the introduced benzyl chloride group has high activity, can react with the amino group on the modified nanoparticle to generate a CN bond by nucleophilic substitution reaction, enhance the binding force of the nanoparticle and the resin, and improve the adhesion of the nanoparticle. The chlorine atom in the introduced benzyl chloride group can also react with the hydroxyl group in the hydroxy acrylic resin to achieve cross-linking and curing, avoiding the use of an additional curing agent. The obtained coating has a large contact angle, a small rolling angle, and good weather resistance, can effectively reduce the adhesion of ice layers, and has a good anti-icing effect.
Claims
1. A super-hydrophobic anti-icing fan blade coating, It is characterized in that Included by mass percentage: 30-70% of benzyl chlorinated fluorinated acrylic resin, 5-20% of modified nanoparticles, 20-60% of hydroxy acrylic resin, 1.5-5% of auxiliary agent, and the balance is solvent.
2. A super hydrophobic anti-icing fan blade coating according to claim 1, It is characterized in that The nanoparticles are composed of one or two or more of silicon dioxide, titanium dioxide, zinc oxide and aluminum oxide mixed in any proportion; the modified nanoparticles are nanoparticles with fluorine-containing groups and amino groups grafted on the surface.
3. A super hydrophobic anti-icing fan blade coating according to claim 1, It is characterized in that The auxiliary agents are dispersants and defoamers; the contents of the dispersants and defoamers in the coating are 1-3% of the dispersant and 0.5-2% of the defoamer by mass percentage.
4. A super hydrophobic anti-icing fan blade coating according to claim 1, It is characterized in that The structure of the benzyl chlorinated fluorinated acrylic resin is as follows: Among them, R 1 is one of a hydrogen atom, a methyl group and an ethyl group, R 2 is an alkyl group with less than 18 carbon atoms, R f is a fluorinated alkyl group, and m and n are positive integers.
5. A super hydrophobic anti-icing fan blade coating according to claim 1, It is characterized in that The structure of the cyanoacrylate resin is as follows: Where m, n are positive integers, R 3 is one of a hydrogen atom, a methyl group and an ethyl group, R 4 is an alkyl group with less than 18 carbon atoms, R 5 It is an alkyl group having less than 6 carbon atoms.
6. A method for preparing a super-hydrophobic anti-icing fan blade coating according to any one of claims 1 to 5, It is characterized in that The following steps are involved: Adding benzyl chlorinated fluorinated acrylic resin, modified nanoparticles and additives into a solvent; After sufficient stirring and dispersion, add hydroxy acrylic resin and continue to stir and disperse evenly to obtain the desired super hydrophobic anti-icing fan blade coating.
7. A method for preparing a super-hydrophobic anti-icing fan blade coating according to claim 6, It is characterized in that The preparation process of the benzyl chlorinated fluorinated acrylic resin is as follows: Add fluorinated acrylic resin, chloromethylation agent and catalyst into solvent, and react at 20-80°C for 1-12 hours; remove the solvent and wash to obtain the desired benzyl chlorinated fluorinated acrylic resin.
8. A method for preparing a super-hydrophobic anti-icing fan blade coating according to claim 7, It is characterized in that The preparation method of the modified nanoparticles is as follows: Adding nanoparticles and fluorosilane coupling agent into the solvent, adjusting pH, and performing ultrasonic dispersion; After reacting at 60°C for 5 to 24 hours, an aminosilane coupling agent is added and reacted at this temperature for 5 to 24 hours; after filtering and drying, the desired modified nanoparticles are obtained.
9. A method for preparing a super-hydrophobic anti-icing fan blade coating according to claim 8, It is characterized in that The chloromethylation agent is one of trimethylsilyl chloride-paraformaldehyde, hydrogen chloride-triformaldehyde, chloromethyl alkyl ether and chloromethyltrimethylsilane; The catalyst is one or a mixture of two or more of tin tetrachloride, aluminum trichloride and zinc chloride in any proportion; The fluorosilane coupling agent is one or a mixture of two or more of tridecafluorooctyltrimethylsilane, tridecafluorooctyltriethoxysilane, heptadecafluorodecyltrimethoxysilane and heptadecafluorodecyltriethoxysilane in any proportion; The aminosilane coupling agent is one or two or more of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane mixed in any proportion.
10. Application of the super hydrophobic anti-icing fan blade coating according to any one of claims 1 to 5, It is characterized in that The coating is prepared for use as a super-hydrophobic anti-icing coating for fan blades.
Citation Information
Patent Citations
Super-hydrophobic acrylic polyurethane coating and preparation method thereof
CN104910779A
Wear-resistant super-hydrophobic coating compound
CN106634064A
Concrete super-hydrophobic self-repairing protective coating and preparation method thereof
CN113444438A
Superhydrophobic coating composition and coated articles obtained therefrom
US20080015298A1