Hydrophobic anti-freezing coating material and preparation method of hydrophobic anti-freezing coating
By using hydrophobic nanotitanium dioxide and ethanol combined with epoxy resin or aqueous polyurethane coating materials, the complex and cost-effective preparation of existing pavement hydrophobic anti-coagulation ice coatings is solved, and excellent hydrophobic performance and self-cleaning ability are achieved. Effectively prevent road area from agglomerating and icing, and reduce preparation costs.
Patent Information
- Application Number
- CN202411049437.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing preparation methods for hydrophobic anti-coagulation ice coatings on pavement are complex and costly, limiting their large-scale application on the road.
Hydrophobic nanotitanium dioxide and ethanol are used as the surface layer material, combined with epoxy resin or aqueous polyurethane and ethanol as the base material, and hydrophobic anti-coagulation ice coating is prepared by spraying method, and nanotitanium dioxide is added in the semi-cured state using polymer to avoid agglomeration. , form microstructures to improve hydrophobic properties.
It achieves excellent hydrophobic performance, extremely low wetting performance and self-cleaning ability, effectively preventing moisture from accumulation and icing on asphalt pavement, reducing safety hazards caused by icing on the pavement in winter, and reducing preparation costs.
Smart Images

Figure CN118978844A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of hydrophobic and anti-icing road surface, and in particular to a hydrophobic and anti-icing coating material and a method for preparing the hydrophobic and anti-icing coating. Background Art
[0003] The hydrophobic surface can effectively reduce the adhesion between ice and the substrate surface, reducing snow accumulation and ice formation. The technology was initially applied to the deicing of high-voltage transmission lines, and then gradually expanded to many fields such as building materials, glass surfaces, and ship hulls. In the road field, by applying hydrophobic materials to asphalt pavement, the anti-skid performance of the pavement can be significantly improved, reducing the occurrence of traffic accidents.
[0004] At present, most of the preparation of pavement hydrophobic coatings adopts the sol-gel method. For example, Gao Yingli first hydrothermally reacts the silane coupling agent to obtain a branched chain with a hydrophobic functional group, and then uses nanoparticles to react with it to prepare an emulsion, and then sprays the emulsion on the asphalt mixture by spraying. The material that plays a hydrophobic role is nanoparticles. The main nanoparticles are ZnO, SiO 2 , polytetrafluoroethylene, TiO 2 、Al 2 O 3 (Gao Yingli, Dai Kaiming, Li Xuekun, et al. Anti-icing performance and evaluation of superhydrophobic asphalt concrete [J]. Materials Review, 2017, 31(24): 63-68.).
[0005] The existing preparation methods of hydrophobic anti-icing coatings are relatively complicated and the material costs are high, which limits their large-scale application on roads. Summary of the invention
[0006] The purpose of the present invention is to provide a hydrophobic anti-icing coating material and a method for preparing the hydrophobic anti-icing coating. The hydrophobic anti-icing coating prepared by the present invention exhibits excellent hydrophobicity, extremely low wetting performance and self-cleaning ability, and can effectively prevent the accumulation and freezing of water on the asphalt pavement. The preparation method of the present invention is simple and low-cost.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a hydrophobic anti-icing coating material, comprising a surface layer material and a bottom layer material;
[0009] The surface layer material includes hydrophobic nano-titanium dioxide and a first ethanol; the mass ratio of the hydrophobic nano-titanium dioxide to the first ethanol is 1.5:20;
[0010] The bottom layer material comprises a polymer and a second alcohol; the polymer is an epoxy resin or an aqueous polyurethane; and the mass ratio of the polymer to the second alcohol is 0.8:20.
[0011] Preferably, when the polymer is epoxy resin, the base material further includes a curing agent; the mass ratio of the epoxy resin to the curing agent is 4:1.
[0012] Preferably, the particle size of the hydrophobic nano-titanium dioxide is 25±5nm and the specific surface area is 30±15m 2 / g.
[0013] Preferably, the epoxy resin has an epoxy equivalent of 210 to 244 g / eq, a softening point of 15 to 23° C., a viscosity of 6 to 10 Pa·S, a saponification rate of ≤0.5%, and an inorganic chlorine content of ≤200 ppm.
[0014] Preferably, the waterborne polyurethane has a solid content of 35±5%, a pH value of 6 to 8 at 25° C., and a viscosity of 800 to 1500 MPa·S.
[0015] The present invention provides a method for preparing a hydrophobic anti-icing coating, using the hydrophobic anti-icing coating material described in the above scheme as a raw material, comprising the following steps:
[0016] Firstly coating the bottom layer material onto the surface of the substrate for pre-curing to form an incompletely cured bottom layer;
[0017] The surface layer material is secondly coated onto the surface of the incompletely cured bottom layer and finally cured to obtain the hydrophobic anti-icing coating.
[0018] Preferably, the first coating and the second coating comprise spray coating.
[0019] Preferably, the coating amount of the bottom layer material is 60 to 90 mL / m 2 .
[0020] Preferably, the coating amount of the surface layer material is 100-120 mL / m 2 .
[0021] Preferably, the pre-curing time is 24 hours.
[0022] The present invention provides a hydrophobic anti-icing coating material, comprising a surface layer material and a bottom layer material; the surface layer material comprises hydrophobic nano titanium dioxide and a first ethanol; the mass ratio of the hydrophobic nano titanium dioxide to the first ethanol is 1.5:20; the bottom layer material comprises a polymer and a second ethanol; the polymer is an epoxy resin or an aqueous polyurethane; the mass ratio of the polymer to the second ethanol is 0.8:20.
[0023] The present invention uses polymer as the bottom layer, and in a semi-cured state, hydrophobic nano titanium dioxide is added to partially sink into the resin, and a certain proportion is exposed on the resin surface, thereby avoiding agglomeration and improving its hydrophobic performance.
[0024] After the coating treatment, the surface roughness of the substrate increases, forming numerous micrometer-level papillae and pores, wherein the papillae are formed after the coating reagent, and the pores are caused by the volatilization of the ethanol solvent. The presence of these microstructures has an important influence on the wettability of the coating. When water droplets contact the coating, due to the surface tension of the liquid, it is difficult for the water droplets to penetrate into these tiny pores. Therefore, a certain amount of air is retained inside the pores, which hinders the complete contact between the water droplets and the substrate, thereby forming a gas-liquid-solid three-phase interface. The presence of this three-phase interface significantly reduces the actual contact area between the water droplets and the coating, thereby achieving a hydrophobic effect on the material surface.
[0025] This characteristic of the hydrophobic coating gives it extremely low water droplet adhesion. This hydrophobicity can significantly reduce the wetting degree of water droplets and reduce the effective contact area between dirt and the surface. In addition, when water droplets roll down, their carrying effect can effectively remove most of the pollutants on the surface, thereby significantly improving the self-cleaning ability of the material.
[0026] Furthermore, the hydrophobic coating on the surface of the coated specimen significantly reduced its hydrophilicity, resulting in an unstable ice film structure formed on the surface. Since the bonding strength between the coating and the ice layer is lower than the strength of the ice itself, it becomes difficult for the ice layer to form on the coating surface.
[0027] In summary, the coating of the present invention exhibits excellent hydrophobic properties, extremely low wetting properties and self-cleaning ability, and can effectively prevent the accumulation and freezing of moisture on the asphalt pavement, thereby reducing the safety hazards caused by road icing in winter.
[0028] In addition, the preparation of the hydrophobic anti-icing coating of the present invention requires fewer types of reagents, and the reagents used are cheap and low in cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the schematic diagram of the self-cleaning test flushing;
[0030] Figure 2 Schematic diagram of water residual test. DETAILED DESCRIPTION
[0031] The present invention provides a hydrophobic anti-icing coating material, comprising a surface layer material and a bottom layer material;
[0032] The surface layer material includes hydrophobic nano-titanium dioxide and a first ethanol; the mass ratio of the hydrophobic nano-titanium dioxide to the first ethanol is 1.5:20;
[0033] The bottom layer material comprises a polymer and a second alcohol; the polymer is an epoxy resin or an aqueous polyurethane; and the mass ratio of the polymer to the second alcohol is 0.8:20.
[0034] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0035] The surface layer materials will be described below.
[0036] In the present invention, the surface layer material comprises hydrophobic nano-titanium dioxide and a first ethanol; the mass ratio of the hydrophobic nano-titanium dioxide to the first ethanol is 1.5:20.
[0037] In the present invention, the particle size of the hydrophobic nano-titanium dioxide is preferably 25±5nm, and the specific surface area is preferably 30±15m 2 In the present invention, the first ethanol is preferably anhydrous ethanol.
[0038] The present invention uses hydrophobic nano titanium dioxide as the surface layer material and has good hydrophobic performance.
[0039] The bottom layer material is described below.
[0040] In the present invention, the bottom layer material comprises a polymer and a second alcohol; the polymer is an epoxy resin or an aqueous polyurethane; and the mass ratio of the polymer to the second alcohol is 0.8:20.
[0041] In the present invention, the epoxy equivalent of the epoxy resin is preferably 210-244 g / eq, the softening point is preferably 15-23° C., the viscosity is preferably 6-10 Pa·S, the saponification rate is preferably ≤0.5%, and the inorganic chlorine is preferably ≤200 ppm; the solid content of the aqueous polyurethane is preferably 35±5%, the pH value at 25° C. is preferably 6-8, and the viscosity is preferably 800-1500 Mpa·S.
[0042] In the present invention, when the polymer is an epoxy resin, the base material preferably further comprises a curing agent; the mass ratio of the epoxy resin to the curing agent is preferably 4: 1. In the present invention, the epoxy resin curing agent is preferably a curing agent (T-31), with a viscosity of 2000 to 4000 Mpa·S and an amine value of 400 to 550 mgKOH / g.
[0043] In the present invention, the second ethanol is preferably anhydrous ethanol.
[0044] The present invention provides a method for preparing a hydrophobic anti-icing coating, using the hydrophobic anti-icing coating material described in the above scheme as a raw material, comprising the following steps:
[0045] Firstly coating the bottom layer material onto the surface of the substrate for pre-curing to form an incompletely cured bottom layer;
[0046] The surface layer material is secondly coated onto the surface of the incompletely cured bottom layer and finally cured to obtain the hydrophobic anti-icing coating.
[0047] The present invention first coats the bottom layer material onto the surface of the substrate for pre-curing to form an incompletely cured bottom layer.
[0048] In the present invention, the substrate is preferably an asphalt pavement. In the embodiment of the present invention, a glass slide is used as the substrate to facilitate performance testing.
[0049] The present invention preferably disperses the polymer (when the polymer is an epoxy resin, it also includes a curing agent) into the second ethanol to obtain the bottom material. The present invention has no special requirements for the dispersion method, as long as it can be evenly dispersed. In an embodiment of the present invention, specifically, the polymer (when the polymer is an epoxy resin, it also includes a curing agent) is dispersed into anhydrous ethanol and stirred for 1 hour to obtain the bottom material.
[0050] The present invention has no special requirements for the first coating method, and a coating method well known in the art can be used. When the substrate is an asphalt pavement, the first coating is preferably brushed first and then sprayed. Since there are pores in the asphalt pavement, the present invention first brushes and then sprays to ensure that the asphalt pavement is evenly attached to the underlying material. In an embodiment of the present invention, when the substrate is a glass slide, the first coating is sprayed.
[0051] In the present invention, the coating amount of the base material is preferably 60 to 90 mL / m 2 , more preferably 70 to 80 mL / m 2 In the embodiment of the present invention, the specific value is 75 mL / m 2 .
[0052] In the present invention, the pre-curing is preferably carried out at room temperature; the pre-curing time is preferably 24 hours.
[0053] After forming the incompletely cured bottom layer, the present invention applies the surface layer material to the surface of the incompletely cured bottom layer for a second time, and performs final curing to obtain the hydrophobic anti-icing coating.
[0054] The present invention preferably disperses the hydrophobic nano titanium dioxide into the first ethanol to obtain the surface layer material. The present invention has no special requirements for the dispersion method, as long as it can be evenly dispersed. In an embodiment of the present invention, the hydrophobic nano titanium dioxide is dispersed into anhydrous ethanol, first magnetically stirred for 30 minutes, and then ultrasonically dispersed for 30 minutes to obtain the surface layer material.
[0055] The present invention has no special requirements for the second coating method, and any coating method known in the art can be used. When the substrate is an asphalt pavement, the second coating is preferably first brushed and then sprayed. In an embodiment of the present invention, when the substrate is a glass slide, the second coating is sprayed.
[0056] In the present invention, the coating amount of the surface layer material is preferably 100 to 120 mL / m 2 , more preferably 110 to 115 mL / m 2 In the embodiment of the present invention, it is specifically 112.5 mL / m 2 .
[0057] In the present invention, the final curing is preferably carried out at room temperature, and the final curing time is preferably 24 hours.
[0058] The present invention uses a polymer as a bottom layer, and in a semi-cured state, hydrophobic nano titanium dioxide is added to partially sink into the resin, and a certain proportion is exposed on the resin surface to avoid agglomeration and improve its hydrophobicity. At the same time, the roughness of the coating surface can be increased to form numerous micron-level papillae, and the volatilization of ethanol forms a large number of pores. The presence of numerous papillae and pores significantly reduces the wetting degree of water droplets, so that the coating exhibits excellent hydrophobicity, extremely low wetting performance and self-cleaning ability, and can effectively prevent the accumulation and freezing of water on the asphalt pavement, thereby reducing the safety hazards caused by road icing in winter.
[0059] The hydrophobic anti-icing coating material and the preparation method of the hydrophobic anti-icing coating provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be understood as limiting the protection scope of the present invention.
[0060] The technical specifications of the raw materials used in the following examples are shown in Table 1.
[0061] Table 1 Technical indicators of raw materials
[0062]
[0063]
[0064] Embodiment 1-2
[0065] According to the formula in Table 2, the hydrophobic nano-titanium dioxide was dispersed in anhydrous ethanol, magnetically stirred for 30 minutes, and ultrasonically dispersed for 30 minutes to obtain a uniform dispersion as the surface layer material; then the polymer was dispersed in anhydrous ethanol (when epoxy resin is used, a curing agent is needed and added together), magnetically stirred for 1 hour, and a uniform dispersion was obtained as the bottom layer material. The bottom layer material containing the polymer was sprayed on a glass slide (20×20cm), and after the bottom layer material was cured for 24 hours, the top layer coating was sprayed on the uncured bottom layer, and cured at room temperature for 24 hours to obtain a hydrophobic coating. The spraying was carried out using a pump spray pen, and the bottom layer was sprayed 1.5mL each time, and sprayed twice, while the surface layer was sprayed 1.5mL each time, and sprayed 3 times.
[0066] Table 2 Materials and dosages of the examples
[0067]
[0068] Comparative Example
[0069] Untreated slide surface.
[0070] Performance Testing
[0071] 1. Contact angle test
[0072] In this experiment, the contact angle of the sample was measured using a contact angle meter DSA100 (KRUSS, Germany). The surface free energy was calculated by measuring the contact angles of distilled water, glycerol and formamide on the sample. The surface free energy of the solid was calculated using the Young equation based on the contact angle measurement using the Owens three-liquid method. The test results are shown in Table 3.
[0073] Table 3 Contact angle and surface free energy
[0074]
[0075]
[0076] As shown in Table 3, the contact angles of Examples 1 and 2 are 135° and 122.75°, and the surface free energy is 9.90 mJ / m 2 and 18.15mJ / m 2 , which are significantly higher than the untreated comparative examples, and have good hydrophobic and anti-wetting properties.
[0077] 2. Self-cleaning test
[0078] The hydrophobic coating was prepared by spraying on a 20×20 cm glass sheet, and the specimen was sealed with transparent tape to prevent sewage from seeping in. After the solidification was complete, the pollutants (prepared according to the proportions shown in Table 4) were evenly covered on the coating surface, with a total of 100 mL of sewage. The specimen containing sewage was placed in an oven and dried for 4 h. After the drying was completed, the tapes were removed and the specimen and pollutant were weighed. 1 Place the specimen on Figure 1 The specimen is placed in a tank with an inclination of 10°. 1000 mL of tap water is added to the spray gun spray pot to flush the specimen at a flow rate of 8 mL / s. The flushed specimen is placed in an oven to dry for 4 h, and the mass after drying is weighed. 2 , take photos, observe the pollutant washout, and conduct three parallel tests. Figure 1 As shown; by calculating the amount of dirt loss d 1 =m 1 -m 2 , d 1 The larger the value, the stronger the self-cleaning ability of the coating. The test results are shown in Table 5.
[0079] Table 4 Road surface pollutants
[0080]
[0081] Table 5 Scouring results
[0082] formula <![CDATA[d 1 (g)]]> Example 1 6.77 Example 2 6.3 Comparative Example 5.4
[0083] It can be seen from Table 5 that the self-cleaning performance of the test pieces of the embodiments is improved to a certain extent, while the self-cleaning performance of the comparative examples is relatively weak.
[0084] 3. Water Residue Test
[0085] The substrate is a frosted glass plate. Several 20×20 cm coating specimens are prepared and their mass m is weighed. 3 ; Place the specimens on a tripod with an inclination angle of 5°; prepare 250mL of tap water and put it into a spray pot, and adjust the flow rate of the spray gun to 8mL / s; fix the spray gun on a 30cm high load platform and spray the specimens. During the spraying process, observe the residual water flow. Figure 2 As shown; 1 minute after the spraying ends, weigh the mass m of the specimen 4 , and calculate the residual water flow d 2 =m 4 -m 3 . Water flow residual d 2 It reflects the ability of the coating surface to repel water droplets, d 2 The smaller the value, the more hydrophobic the coating surface is. The test results are shown in Table 6.
[0086] Table 6 Water flow residual
[0087] formula <![CDATA[d 2 (g)]]> Example 1 5.07 Example 2 4.93 Comparative Example 6.87
[0088] It can be seen from Table 6 that the embodiments can significantly reduce the residual amount of water flow compared with the comparative examples, among which the hydrophobicity of Example 2 is the best.
[0089] 4. De-icing test
[0090] Two groups of Marshall specimens with similar surface conditions and consistent gradation were selected. One group of specimens was cleaned and dried, and the hydrophobic coating material was first brushed and then sprayed as the experimental group (the total coating amount of the bottom material was 75 mL / m 2 The coating amount of the surface material is 112.5mL / m 2 ), and the other group was untreated as the control group; the samples were sealed and wrapped with waterproof tape and sealing glue to form a bowl-shaped structure with a height of 10mm to prevent water loss; 40g of water was evenly sprinkled on the surface of each sample, and the whole was placed in a refrigerator at -4℃ for 4h to form an ice layer on the surface of the sample; after the surface of the sample was completely frozen, the tape of all samples in the refrigerator was removed, and the samples were taken out one by one and the mass was quickly measured and recorded as m 5 Then place the sample, release a 419.2g solid steel ball from 50cm above and let it fall freely to the top of the sample, repeat 10 times, the process should be done quickly to prevent the ice layer from melting, and observe the cracks of the ice layer on the surface of the sample, remove the broken ice on the surface of the sample, and measure the mass and record it as m 6 Then clean up all the ice remaining on the surface and measure the mass again, record it as m 7 . The ice breakage rate is calculated based on the quality data and the de-icing effect is analyzed.
[0091] De-icing level is assessed according to the degree of ice cracking, and the ice damage rate is calculated As shown in Table 7.
[0092] Table 7 Ice damage rate
[0093]
[0094]
[0095] It can be seen from Table 7 that the deicing performance of the embodiments is better than that of the comparative examples, among which the deicing performance of embodiment 3 is the best.
[0096] It can be seen from the above examples that the present invention provides a method for preparing a hydrophobic anti-icing coating. The hydrophobic anti-icing coating prepared by the present invention exhibits excellent hydrophobicity, extremely low wetting performance and self-cleaning ability, and can effectively prevent water accumulation and icing on asphalt pavement.
[0097] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A hydrophobic anti-icing coating material, characterized in that: Including surface material and base material; The surface layer material includes hydrophobic nano-titanium dioxide and a first ethanol; the mass ratio of the hydrophobic nano-titanium dioxide to the first ethanol is 1.5:20; The bottom layer material comprises a polymer and a second alcohol; the polymer is an epoxy resin or an aqueous polyurethane; and the mass ratio of the polymer to the second alcohol is 0.8:
20.
2. The hydrophobic anti-icing coating material according to claim 1, characterized in that: When the polymer is epoxy resin, the base material further includes a curing agent; the mass ratio of the epoxy resin to the curing agent is 4:
1.
3. The road surface hydrophobic anti-icing coating material according to claim 1, characterized in that: The particle size of the hydrophobic nano titanium dioxide is 25±5nm and the specific surface area is 30±15m 2 / g.
4. The road surface hydrophobic anti-icing coating material according to claim 1 or 2, characterized in that: The epoxy resin has an epoxy equivalent of 210 to 244 g / eq, a softening point of 15 to 23° C., a viscosity of 6 to 10 Pa·S, an easy saponification rate of ≤0.5%, and inorganic chlorine ≤200 ppm.
5. The road surface hydrophobic anti-icing coating material according to claim 1, characterized in that: The waterborne polyurethane has a solid content of 35±5%, a pH value of 6-8 at 25° C., and a viscosity of 800-1500 Mpa·S.
6. A method for preparing a hydrophobic anti-icing coating, using the hydrophobic anti-icing coating material according to any one of claims 1 to 5 as a raw material, comprising the following steps: Firstly coating the bottom layer material onto the surface of the substrate for pre-curing to form an incompletely cured bottom layer; The surface layer material is secondly coated onto the surface of the incompletely cured bottom layer and finally cured to obtain the hydrophobic anti-icing coating.
7. The preparation method according to claim 6, characterized in that: The first coating and the second coating include spraying.
8. The preparation method according to claim 6, characterized in that: The coating amount of the bottom layer material is 60 to 90 mL / m 2 .
9. The preparation method according to claim 6, characterized in that: The coating amount of the surface layer material is 100-120 mL / m 2 .
10. The preparation method according to claim 6, characterized in that: The pre-curing time is 24 hours.
Citation Information
Patent Citations
Method for preparing durable super-amphiphobic coatings capable of being sprayed
CN106893454A
Super-hydrophobic paint for preventing road surface from being frozen and preparation method and construction method of super-hydrophobic paint
CN108047776A
Super-hydrophobic coating for asphalt pavement and preparation method thereof
CN113265193A