Polymer waterproof anticorrosive paint and preparation method thereof

By combining polyaniline with tetramethylamine doping treatment with linseed oil-based epoxy polymer, combined with nanofillers to form polymer waterproof and anti-corrosion coatings, the shortcomings of traditional coatings in high temperature and chemical erosion are solved, and the extreme Stability and efficient protection in the environment reduce costs and conform to the principles of sustainable development.

CN118978847AActive Publication Date: 2024-11-19HEBEI YUYANGZELI WATERPROOF MATERIAL
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411339710.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-19
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

Traditional waterproof and anti-corrosion coatings have unstable performance in high temperature environments, are difficult to resist chemical corrosion, and are costly, which cannot meet the strict needs of modern industry and construction industries.

Method used

Polyaniline and tetramethylamine reagent doping treatment are mixed with glycol ether, combined with linseed oil-based epoxy polymer, hardener and nanofiller to form polymer waterproof and anti-corrosion coating, through crosslinking density and three-dimensional network Structure enhances the chemical resistance, temperature resistance and corrosion resistance of coatings.

Benefits of technology

It achieves long-term stability and efficient protection of coatings in extreme environments, significantly improves service life, has excellent physical and chemical stability, reduces costs, and complies with the principle of sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of polymer coatings, and discloses a polymer waterproof anticorrosive coating and a preparation method thereof.The preparation method comprises the steps that polyaniline and a tetramethylamine reagent are mixed, doped and then mixed with glycol ether, and a doped polyaniline solution is obtained after uniform stirring and dispersing; uniformly mixing and stirring the linseed oil-based epoxy polymer and the hardening agent, and then adding the nano filler under a stirring condition to obtain a base material; under a stirring condition, adding the doped polyaniline solution into the base material, and uniformly stirring to obtain the polymer waterproof anticorrosive coating. The excellent performance of doped polyaniline and the unique advantages of the linseed oil-based epoxy polymer are fused, the high-performance coating is successfully developed, the coating shows excellent performance in the aspects of water resistance, corrosion resistance, adhesive force and flexibility, and the overall performance of the coating is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer coatings, and in particular to a polymer waterproof and anticorrosive coating and a preparation method thereof. Background Art

[0002] In today's society, industrial production and construction fields have put forward more stringent and detailed requirements on the waterproof and anti-corrosion properties of materials. With the continuous advancement of technology and the expansion of application fields, traditional waterproof and anti-corrosion coatings can no longer fully meet the needs of modern industry and construction industries. Although there are many traditional waterproof and anti-corrosion coatings on the market, they often expose many shortcomings in practical applications. For example, although some coatings have excellent waterproof performance and can effectively prevent water penetration, they are not satisfactory in terms of high temperature resistance and corrosion resistance. They cannot maintain stable performance in high temperature environments and are difficult to resist the erosion of various chemicals. While other coatings have excellent performance in certain properties, such as high temperature resistance or corrosion resistance, their high cost makes it difficult for these coatings to be used in a wider market, thus limiting their popularization and promotion.

[0003] Therefore, developing an innovative polymer waterproof and anti-corrosion coating has become an urgent need for technological progress. This coating must meet the strict standards of the industrial and construction industries for materials in terms of waterproof and anti-corrosion performance, and should have excellent comprehensive properties such as high temperature resistance and corrosion resistance. Only in this way can it maintain the stability and durability of the material in various extreme environments, thereby improving the efficiency and safety of industrial production and construction. Summary of the invention

[0004] In view of this, the present invention proposes a polymer waterproof and anti-corrosion coating and a preparation method thereof, aiming to provide a polymer waterproof and anti-corrosion coating with excellent comprehensive performance and reasonable cost to meet the waterproof and anti-corrosion needs of materials in the industrial and construction fields.

[0005] The present invention provides a method for preparing a polymer waterproof and anticorrosive coating, comprising: The polyaniline is mixed with a tetramethylamine reagent, and then mixed with ethylene glycol ether after doping treatment, and then stirred and dispersed uniformly to obtain a doped polyaniline solution; After the linseed oil-based epoxy polymer and the hardener are mixed and stirred evenly, the nanofiller is added under stirring to obtain a base material; Under stirring conditions, the doped polyaniline solution is added to the base material, and after stirring evenly, the polymer waterproof and anti-corrosion coating is obtained.

[0006] Preferably, the tetramethylamine reagent is tetramethylethylenediamine and / or tetramethylpropylenediamine; The hardener is a phenolic amine hardener; The nano filler is nano silicon dioxide and nano aluminum oxide.

[0007] Preferably, the process of mixing polyaniline with tetramethylamine reagent for doping treatment comprises: Aniline is dissolved in an acidic aqueous solution, and then an oxidant is added to synthesize a hydrochloric acid-doped polyaniline, and after the reaction is completed, the polyaniline powder is obtained by washing and drying. The polyaniline powder is mixed with a tetramethylamine reagent solvent, and then stirred for reaction at room temperature. After the reaction is completed, the mixture is washed and dried to obtain doped polyaniline.

[0008] Preferably, the preparation method of the linseed oil-based epoxy polymer comprises: The linseed oil-based epoxy monomer is prepared by taking linseed oil as a raw material, and then the linseed oil-based epoxy monomer is polymerized into the linseed oil-based epoxy polymer through a ring-opening polymerization reaction.

[0009] Preferably, the process of preparing linseed oil-based epoxy monomer using linseed oil as raw material comprises: After the linseed oil is pre-treated by dehydration, an epoxidant is added dropwise to the linseed oil at 30-50° C., and an epoxidation reaction is carried out with phosphotungstic acid as a catalyst to obtain the linseed oil-based epoxy monomer.

[0010] Preferably, the epoxidizing agent is peracetic acid; The molar ratio of the peracetic acid to the linseed oil is 1.5-2.5:1.

[0011] Preferably, the process of polymerizing the linseed oil-based epoxy monomer to form the linseed oil-based epoxy polymer comprises: The linseed oil-based epoxy monomer and the tertiary amine catalyst are mixed, heated to 50-80° C., and then subjected to polymerization reaction under continuous stirring to obtain the linseed oil-based epoxy polymer.

[0012] Preferably, the tertiary amine catalyst is N,N-dimethylethanolamine.

[0013] The present invention also proposes a polymer waterproof and anti-corrosion coating, which is prepared by the above-mentioned polymer waterproof and anti-corrosion coating preparation method.

[0014] The present invention also provides a protective coating product, which includes the above-mentioned polymer waterproof and anti-corrosion coating.

[0015] From a microscopic perspective, the principle mechanism of the technical solution of the present invention is also reflected in the cross-linking density of the coating. The reaction of linseed oil-based epoxy polymer and hardener generates a highly cross-linked polymer network, which gives the coating excellent chemical resistance and temperature resistance. At the same time, the introduction of doped polyaniline further increases the cross-linking density of the coating, thereby enhancing its overall physical and chemical stability. Specifically: The introduction of doped polyaniline significantly improves the conductivity of the coating, thus giving it excellent anti-corrosion ability. The conjugated structure formed by polyaniline during the doping process gives it good electron transmission ability at the molecular level, which helps the coating form a protective film on the metal surface, effectively blocking the invasion of external corrosive media.

[0016] Linseed oil-based epoxy polymer, as the main component of the base material, provides excellent adhesion and flexibility. Linseed oil is a natural oil, and its unsaturated fatty acid chain forms an epoxy polymer with a three-dimensional network structure after epoxidation. This structure not only gives the coating good mechanical properties, but also improves its chemical resistance and weather resistance.

[0017] The addition of nanofillers further enhances the overall performance of the coating. Nano-silicon dioxide and nano-alumina have extremely small particle sizes and can be evenly dispersed in the base material to form a dense filler network structure. This structure not only improves the mechanical strength and wear resistance of the coating, but also effectively reduces the porosity of the coating, thereby enhancing its waterproof performance.

[0018] Compared with the prior art, the present invention has the following beneficial effects: The present invention proposes a waterproof and anticorrosive coating with excellent durability and long-term stability. This coating is particularly suitable for various harsh environmental conditions, such as oceans, chemical plants, oil platforms and the like. It significantly improves the service life of the coating, making it perform well in these harsh environments. By incorporating doped polyaniline and nanofillers into the coating, the present invention not only maintains the excellent physical properties of the coating, but also exhibits good electrochemical properties. This effectively prevents electrochemical corrosion of metal materials, thereby extending their service life.

[0019] Among the components of the coating, the use of linseed oil-based epoxy polymer makes the coating of the present invention have excellent biodegradability. This property makes the coating harmless to the environment, conforms to the principle of sustainable development, and also meets environmental protection requirements. During the construction process, the coating of the present invention exhibits good leveling and adhesion, and can form a uniform and smooth coating. This not only improves the aesthetics of the coating, but also enhances its practicality, so that it can perform well in various applications.

[0020] In addition, the coating of the present invention also has excellent temperature resistance and can operate stably in a wide temperature range of -40°C to 150°C. This feature enables the coating to meet application requirements in different environments, and its performance can be kept stable regardless of extreme cold or high temperature conditions. In summary, the polymer waterproof and anti-corrosion coating of the present invention and its preparation method have shown significant technical innovation. It has brought significant economic and social benefits in practical applications, and provides a new type of efficient, environmentally friendly and economical material for related fields, which has broad application prospects and market potential. DETAILED DESCRIPTION

[0021] The exemplary embodiments of the present disclosure will be described in more detail below. Although the exemplary embodiments of the present disclosure are shown below, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present disclosure and to be able to fully convey the scope of the present disclosure to those skilled in the art. It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments. Example 1

[0022] This embodiment prepares a polymer waterproof and anti-corrosion coating, and the specific steps are as follows: 1. Dissolve 100 g of aniline in 1000 ml of hydrochloric acid solution, then add 110 g of ammonium persulfate as an oxidant under stirring. After reacting at room temperature for 2 hours, wash and dry the resulting polyaniline hydrochloric acid doped body to obtain polyaniline powder.

[0023] 2. The obtained polyaniline powder was mixed with 200 ml of tetramethylethylenediamine and stirred for reaction at room temperature for 4 hours. After the reaction was completed, it was washed and dried again to obtain doped polyaniline.

[0024] 3. Using linseed oil as raw material, first perform dehydration pretreatment, then add peracetic acid at a molar ratio of 2:1 to the linseed oil at 40°C, and perform epoxidation reaction using phosphotungstic acid as a catalyst to obtain a linseed oil-based epoxy monomer.

[0025] 4. The obtained linseed oil-based epoxy monomer is mixed with N,N-dimethylethanolamine catalyst, and the temperature is raised to 60° C., and a polymerization reaction is carried out under continuous stirring to obtain a linseed oil-based epoxy polymer.

[0026] 5. 100 g of linseed oil-based epoxy polymer and 50 g of phenolic amine hardener were mixed and stirred evenly, and then 50 g of nano-silicon dioxide and 50 g of nano-aluminum oxide were added under stirring to obtain a base material.

[0027] 6. Under stirring conditions, add 200 ml of doped polyaniline solution to the above base material, and stir evenly to obtain a polymer waterproof and anti-corrosion coating. Example 2

[0028] This embodiment partially adjusts the steps in Example 1 to optimize the performance of the coating: 1. Dissolve 120 g of aniline in 1200 ml of hydrochloric acid solution, then add 130 g of potassium persulfate as an oxidant under stirring. After reacting at room temperature for 2.5 hours, wash and dry the resulting polyaniline hydrochloric acid-doped body to obtain polyaniline powder.

[0029] 2. The obtained polyaniline powder was mixed with 250 ml of tetramethylpropylenediamine and stirred at room temperature for 4.5 hours. After the reaction was completed, it was washed and dried again to obtain doped polyaniline.

[0030] 3. Using linseed oil as raw material, first perform dehydration pretreatment, then add peracetic acid at a molar ratio of 2.2:1 to the linseed oil at 45°C, and perform epoxidation reaction using phosphotungstic acid as a catalyst to obtain a linseed oil-based epoxy monomer.

[0031] 4. The obtained linseed oil-based epoxy monomer was mixed with N,N-dimethylethanolamine catalyst, and the temperature was raised to 70° C., and a polymerization reaction was carried out under continuous stirring to obtain a linseed oil-based epoxy polymer.

[0032] 5. 110 g of linseed oil-based epoxy polymer and 60 g of phenolic amine hardener were mixed and stirred evenly, and then 60 g of nano-silicon dioxide and 60 g of nano-aluminum oxide were added under stirring to obtain a base material.

[0033] 6. Under stirring conditions, add 250 ml of the doped polyaniline solution to the above base material, and stir evenly to obtain a polymer waterproof and anti-corrosion coating. Example 3

[0034] In this example, we further optimized the formula in Example 2 to improve the weather resistance and adhesion of the coating: 1. Dissolve 150 g of aniline in 1500 ml of hydrochloric acid solution, then add 150 g of sodium persulfate as an oxidant under stirring. After reacting at room temperature for 3 hours, wash and dry the resulting polyaniline hydrochloric acid-doped body to obtain polyaniline powder.

[0035] 2. The obtained polyaniline powder was mixed with 300 ml of a mixed solvent of tetramethylethylenediamine and tetramethylpropylenediamine (in a ratio of 1:1), and stirred at room temperature for 5 hours. After the reaction was completed, it was washed and dried again to obtain doped polyaniline.

[0036] 3. Using linseed oil as raw material, first perform dehydration pretreatment, then add peracetic acid at a molar ratio of 2.5:1 to the linseed oil at 50°C, and perform epoxidation reaction using phosphotungstic acid as a catalyst to obtain a linseed oil-based epoxy monomer.

[0037] 4. The obtained linseed oil-based epoxy monomer is mixed with N,N-dimethylethanolamine catalyst, and the temperature is raised to 80° C., and a polymerization reaction is carried out under continuous stirring to obtain a linseed oil-based epoxy polymer.

[0038] 5. 120 g of linseed oil-based epoxy polymer and 70 g of phenolic amine hardener were mixed and stirred evenly, and then 70 g of nano-silicon dioxide and 70 g of nano-alumina were added under stirring to obtain a base material.

[0039] 6. Under stirring conditions, add 300 ml of the doped polyaniline solution to the above base material, and stir evenly to obtain a polymer waterproof and anti-corrosion coating.

[0040] The above three embodiments all demonstrate the preparation method of the polymer waterproof and anti-corrosion coating of the present invention. By optimizing the raw material ratio and reaction conditions, a coating product with excellent performance can be prepared.

[0041] The following comparative examples are provided to further illustrate the superiority of the preparation method of the present invention.

[0042] Comparative Example 1 This comparative example does not use linseed oil-based epoxy monomers, but uses traditional petroleum-based epoxy monomers to prepare polymer waterproof and anticorrosive coatings. The specific steps are as follows: 1. Dissolve 100 g of aniline in 1000 ml of hydrochloric acid solution, then add 110 g of ammonium persulfate as an oxidant under stirring. After reacting at room temperature for 2 hours, wash and dry the resulting polyaniline hydrochloric acid doped body to obtain polyaniline powder.

[0043] 2. The obtained polyaniline powder was mixed with 200 ml of tetramethylethylenediamine and stirred for reaction at room temperature for 4 hours. After the reaction was completed, it was washed and dried again to obtain doped polyaniline.

[0044] 3. Using petroleum-based epoxy monomer as raw material, the petroleum-based epoxy monomer is mixed with N,N-dimethylethanolamine catalyst, and then the temperature is raised to 60°C, and a polymerization reaction is carried out under continuous stirring conditions to obtain a petroleum-based epoxy polymer.

[0045] 4. 100 g of petroleum-based epoxy polymer and 50 g of phenolic amine hardener were mixed and stirred evenly, and then 50 g of nano-silicon dioxide and 50 g of nano-alumina were added under stirring to obtain a base material.

[0046] 5. Under stirring conditions, add 200 ml of the doped polyaniline solution to the above base material, and stir evenly to obtain a polymer waterproof and anti-corrosion coating.

[0047] Comparative Example 2 In this comparative example, doped polyaniline is not used, but polyaniline powder is directly mixed with a base material to prepare a polymer waterproof and anticorrosive coating. The specific steps are as follows: 1. Dissolve 100 g of aniline in 1000 ml of hydrochloric acid solution, then add 110 g of ammonium persulfate as an oxidant under stirring. After reacting at room temperature for 2 hours, wash and dry the resulting polyaniline hydrochloric acid doped body to obtain polyaniline powder.

[0048] 2. The obtained polyaniline powder was mixed with 200 ml of tetramethylethylenediamine and stirred for reaction at room temperature for 4 hours. After the reaction was completed, it was washed and dried again to obtain doped polyaniline.

[0049] 3. Using linseed oil as raw material, first perform dehydration pretreatment, then add peracetic acid at a molar ratio of 2:1 to the linseed oil at 40°C, and perform epoxidation reaction using phosphotungstic acid as a catalyst to obtain a linseed oil-based epoxy monomer.

[0050] 4. The obtained linseed oil-based epoxy monomer is mixed with N,N-dimethylethanolamine catalyst, and the temperature is raised to 60° C., and a polymerization reaction is carried out under continuous stirring to obtain a linseed oil-based epoxy polymer.

[0051] 5. 100 g of linseed oil-based epoxy polymer and 50 g of phenolic amine hardener were mixed and stirred evenly, and then 50 g of nano-silicon dioxide and 50 g of nano-aluminum oxide were added under stirring to obtain a base material.

[0052] 6. Add 100 grams of polyaniline powder directly into the above base material, stir evenly to obtain a polymer waterproof and anti-corrosion coating.

[0053] Comparative Example 3 This comparative example does not use nano silicon dioxide and nano aluminum oxide, but only uses linseed oil-based epoxy polymer and doped polyaniline to prepare a polymer waterproof anticorrosive coating, and the specific steps are as follows: 1. Dissolve 100 g of aniline in 1000 ml of hydrochloric acid solution, then add 110 g of ammonium persulfate as an oxidant under stirring. After reacting at room temperature for 2 hours, wash and dry the resulting polyaniline hydrochloric acid doped body to obtain polyaniline powder.

[0054] 2. The obtained polyaniline powder was mixed with 200 ml of tetramethylethylenediamine and stirred for reaction at room temperature for 4 hours. After the reaction was completed, it was washed and dried again to obtain doped polyaniline.

[0055] 3. Using linseed oil as raw material, first perform dehydration pretreatment, then add peracetic acid at a molar ratio of 2:1 to the linseed oil at 40°C, and perform epoxidation reaction using phosphotungstic acid as a catalyst to obtain a linseed oil-based epoxy monomer.

[0056] 4. The obtained linseed oil-based epoxy monomer is mixed with N,N-dimethylethanolamine catalyst, and the temperature is raised to 60° C., and a polymerization reaction is carried out under continuous stirring to obtain a linseed oil-based epoxy polymer.

[0057] 5. Mix 100 g of linseed oil-based epoxy polymer and 50 g of phenolic amine hardener and stir evenly to obtain a base material.

[0058] 6. Under stirring conditions, add 200 ml of doped polyaniline solution to the above base material, and stir evenly to obtain a polymer waterproof and anti-corrosion coating.

[0059] Test Example 1 The coatings prepared in Examples 1-3 of the present invention and Comparative Examples 1-3 were subjected to performance testing, including testing of indicators such as water resistance, corrosion resistance, adhesion and flexibility.

[0060] The judging criteria and testing methods include: 1. Water resistance 1. Test methods Immersion test: Soak the paint sample in water for a certain period of time (24 hours) and observe whether there is peeling, blistering or other changes on the surface.

[0061] Wet heat test: Place the coating sample in a high humidity and high temperature environment (85% humidity, 60°C) to test the stability and water resistance of the coating.

[0062] 2. Evaluation Criteria Excellent: The coating shows no noticeable changes when immersed in water or exposed to high humidity, with no blistering, peeling or other damage on the surface, and is effectively resistant to water penetration.

[0063] Good: The coating has slight changes in water immersion or high humidity environment, but it does not affect the main performance.

[0064] General: Coating shows visible damage or penetration from water immersion or high humidity environments, affecting coating functionality.

[0065] 2. Corrosion resistance 1. Test methods Salt spray test: Place the coating sample in a salt spray test chamber (5% sodium chloride solution, 35°C) and check the corrosion of the coating regularly.

[0066] Acid and alkali corrosion test: Expose the coating sample to an acidic or alkaline solution (sulfuric acid, sodium hydroxide) to observe its corrosion resistance.

[0067] 2. Evaluation Criteria Excellent: The coating has no obvious corrosion phenomenon when exposed to corrosive media (salt spray, acid and alkali solutions), and the coating remains intact.

[0068] Good: The paint has slight corrosion in corrosive media, but it does not affect the main performance.

[0069] General: The coating shows obvious corrosion, peeling or damage in the corrosive media, which reduces the protective ability of the coating.

[0070] 3. Adhesion 1. Test methods Cross-hatch test: Scratch a grid on the paint surface (using a knife), then apply tape and quickly remove it to check if the coating has fallen off.

[0071] Pull-off test: Use a pull-off instrument to pull the paint off and measure the adhesion of the paint.

[0072] 2. Evaluation Criteria Excellent: The adhesion between the paint and the substrate is strong and not easy to peel or fall off.

[0073] Good: The paint has good adhesion and may peel slightly, but it does not affect the main performance.

[0074] General: The paint has poor adhesion and is easy to peel or fall off, affecting the effectiveness of the coating.

[0075] 4. Flexibility 1. Test methods Bend test: Bend the coating sample to a certain angle (180 degrees) and observe whether there is cracking, peeling or other damage.

[0076] Impact test: The coating samples are subjected to impact test to evaluate their flexibility and impact resistance under stress conditions.

[0077] 2. Evaluation Criteria Excellent: The coating has good flexibility and will not crack or peel during bending or deformation.

[0078] Good: The coating has a certain degree of flexibility and may have slight cracks during bending or deformation, but it does not affect the main performance.

[0079] General: The coating has poor flexibility and is prone to cracking or peeling during bending or deformation, affecting the integrity of the coating.

[0080] The test results are shown in Table 1: Table 1

[0081] According to the data in Table 1, we can observe that the coatings of Examples 1-3 all exhibit excellent performance in terms of water resistance, corrosion resistance, adhesion and flexibility, and all meet or exceed the excellent standards. In contrast, the coatings of Control Examples 1-3 have mixed performances in these performance indicators. Specifically, the water resistance and corrosion resistance of Control Example 1 meet good standards, but its adhesion and flexibility are only average; Control Example 2 is average in all these performance indicators; and although Control Example 3 meets excellent standards in water resistance and corrosion resistance, its adhesion and flexibility are still average. These results show that the embodiments of the present invention are superior to the Control Examples in various performance indicators, showing superior comprehensive performance.

[0082] From a microscopic perspective, the excellent performance of the polymer waterproof and anticorrosive coating of the present invention is mainly due to its unique formula and preparation process. The introduction of doped polyaniline significantly improves the corrosion resistance and adhesion of the coating. As a conductive polymer, polyaniline in its doped form can effectively shield and resist the invasion of corrosive media, thereby protecting the substrate under the coating from corrosion. In addition, the addition of doped polyaniline also enhances the bonding force between the coating and the substrate, making the coating more firmly attached to the surface of the substrate.

[0083] The use of linseed oil-based epoxy polymer gives the coating excellent flexibility and water resistance. Linseed oil itself has good flexibility and water resistance. After the epoxidation reaction, epoxy groups are introduced into its molecular structure, which further improves its compatibility with doped polyaniline, making the final coating have better comprehensive performance. The presence of epoxy groups not only enhances the cross-linking density of the coating, but also improves the mechanical strength and chemical resistance of the coating.

[0084] During the preparation process, the uniform mixing and full reaction of linseed oil-based epoxy monomer and doped polyaniline were ensured by controlling the reaction conditions and the use of catalysts, thus obtaining a high-molecular waterproof and anti-corrosion coating with excellent performance. In addition, the added N,N-dimethylethanolamine catalyst played a key role in the polymerization reaction, which not only promoted the polymerization of epoxy monomers, but also increased the molecular weight of the polymer, thereby enhancing the comprehensive performance of the coating.

[0085] In summary, the polymer waterproof and anticorrosive coating of the present invention successfully combines the advantages of doped polyaniline and linseed oil-based epoxy polymer through a unique formula and preparation process to prepare a high-performance coating that performs well in water resistance, corrosion resistance, adhesion and flexibility. This coating is not only suitable for various industrial and civil fields, but also has the advantages of environmental protection, economy and easy construction, and has broad market application prospects.

[0086] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a polymer waterproof and anticorrosive coating, characterized in that: include: The polyaniline is mixed with a tetramethylamine reagent, and then mixed with ethylene glycol ether after doping treatment, and then stirred and dispersed uniformly to obtain a doped polyaniline solution; After the linseed oil-based epoxy polymer and the hardener are mixed and stirred evenly, the nanofiller is added under stirring to obtain a base material; Under stirring conditions, the doped polyaniline solution is added to the base material, and after stirring evenly, the polymer waterproof and anti-corrosion coating is obtained.

2. The method for preparing a polymer waterproof and anticorrosive coating according to claim 1, characterized in that: The tetramethylamine reagent is tetramethylethylenediamine and / or tetramethylpropylenediamine; The hardener is a phenolic amine hardener; The nano fillers are nano silicon dioxide and nano aluminum oxide.

3. The method for preparing a polymer waterproof and anticorrosive coating according to claim 1, characterized in that: The process of mixing polyaniline with tetramethylamine reagents for doping includes: Aniline is dissolved in an acidic aqueous solution, and then an oxidant is added to synthesize a hydrochloric acid-doped polyaniline, and after the reaction is completed, the polyaniline powder is obtained by washing and drying. The polyaniline powder is mixed with a tetramethylamine reagent solvent, and then stirred for reaction at room temperature. After the reaction is completed, the mixture is washed and dried to obtain doped polyaniline.

4. The method for preparing a polymer waterproof and anticorrosive coating according to claim 1, characterized in that: The preparation method of the linseed oil-based epoxy polymer comprises: The linseed oil-based epoxy monomer is prepared by taking linseed oil as a raw material, and then the linseed oil-based epoxy monomer is polymerized into the linseed oil-based epoxy polymer through a ring-opening polymerization reaction.

5. The method for preparing a polymer waterproof and anticorrosive coating according to claim 4, characterized in that: The process of preparing linseed oil-based epoxy monomer using linseed oil as raw material includes: After the linseed oil is pre-treated by dehydration, an epoxidant is added dropwise to the linseed oil at 30-50° C., and an epoxidation reaction is carried out with phosphotungstic acid as a catalyst to obtain the linseed oil-based epoxy monomer.

6. The method for preparing a polymer waterproof and anticorrosive coating according to claim 5, characterized in that: The epoxidizing agent is peracetic acid; The molar ratio of the peracetic acid to the linseed oil is 1.5-2.5:

1.

7. The method for preparing a polymer waterproof and anticorrosive coating according to claim 4, characterized in that: The process of polymerizing the linseed oil-based epoxy monomer to form the linseed oil-based epoxy polymer comprises: The linseed oil-based epoxy monomer and the tertiary amine catalyst are mixed, heated to 50-80° C., and then subjected to polymerization reaction under continuous stirring to obtain the linseed oil-based epoxy polymer.

8. The method for preparing a polymer waterproof and anticorrosive coating according to claim 7, characterized in that: The tertiary amine catalyst is N,N-dimethylethanolamine.

9. A polymer waterproof and anti-corrosion coating, characterized in that: The polymer waterproof and anti-corrosion coating is prepared by the preparation method of the polymer waterproof and anti-corrosion coating according to any one of claims 1-8.

10. A protective coating product, characterized in that: The protective coating product includes the polymer waterproof and anti-corrosion coating as described in claim 9.

Citation Information

Patent Citations

  • Method for preparing epoxidized oil under ultrasound condition

    CN101613639A

  • Preparation technique of improved epoxy flaxseed oil plasticizer

    CN106316989A

  • Catalyst and method for preparing epoxidized linseed oil through same

    CN107930660A

  • Modified polyaniline / epoxy resin composite anticorrosive paint and preparation method thereof

    CN111892855A

  • New doping macromonomer agent, for the preparation of conductive polyaniline, useful in e.g. conductive coatings and films and for the manufacture of glues, hairsprays and inks or paints applicable as absorbent of electromagnetic waves

    FR2880350A1