Building fireproof coating and preparation method thereof
By introducing two flame retardants of DOPO and pentaerythritol phosphate into polyurethane, the problem of insufficient flame retardant performance of water-based polyurethane coatings is solved, and the fire resistance and mechanical properties are significantly improved, forming building fire-retardant coatings with excellent fire resistance.
Patent Information
- Application Number
- CN202411143753.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-19
AI Technical Summary
The flame retardant properties of existing water-based polyurethane coatings are insufficient. When a single inorganic or organic flame retardant is introduced, it is easy to affect the fire resistance and mechanical properties of the coating, and it is poorly miscible with water-based polyurethane.
By introducing two different P-containing flame retardants, DOPO and pentaerythritol phosphate, into the hard and soft segments of polyurethane, modified polyether polyols and ring-opening compounds are prepared through esterification reaction and ring-opening addition reaction, and the modified aqueous properties are synthesized Polyurethane and mixed with fillers and additives to prepare building fire-retardant coatings with excellent fire resistance.
It significantly improves the fire resistance of the paint, including improving performance indicators such as fire resistance, tensile strength, adhesion and backfire time.
Smart Images

Figure BDA0005001654580000031 
Figure BDA0005001654580000032 
Figure BDA0005001654580000033
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fire retardant coatings, and in particular to a building fire retardant coating and a preparation method thereof. Background Art
[0002] Fire retardant coating is a functional coating that reduces or prevents the flammability of the coated materials and reduces fire losses. It is widely used in construction industries such as steel structures. Waterborne polyurethane (WPU) is a polymer material with water as the medium. It has the characteristics of low odor, non-toxicity, and non-pollution. Therefore, it is widely used. The limiting oxygen index (LOI) of ordinary polyurethane is only about 18%, and it is easily ignited. Strengthening its flame retardant properties can protect the substrate, reduce the burning rate on the surface of the material, promote self-extinguishing of combustion, prevent further expansion of the fire, improve fire safety, and provide certain protection for personnel life safety. Therefore, flame retardant treated WPU is the direction of WPU functionalization, and it is also the trend of future polymer materials integrating multiple functions.
[0003] Improving the fire retardant performance of coatings is inseparable from flame retardants. Usually flame retardants include inorganic and organic flame retardants. If a large amount of inorganic flame retardant is introduced alone, not only will the dispersion be poor, but the resistance to cracking through curing film will be even worse. Among organic flame retardants, environmentally friendly intumescent flame retardants have stable chemical properties, high nitrogen content, and good fire retardant performance; but they have poor miscibility with water-based polyurethane, which affects the fire retardant and mechanical properties of the coating.
[0004] To this end, the present invention provides a building fire retardant coating and a preparation method thereof. Summary of the invention
[0005] 1. Technical problems to be solved:
[0006] In view of the above technical problems, the present invention provides a building fire retardant coating and a preparation method thereof.
[0007] 2. Technical solution:
[0008] A fireproof building coating, comprising the following components by mass: 30-40 parts of modified waterborne polyurethane, 20-30 parts of filler, 3-6 parts of additives and 15-30 parts of water;
[0009] The modified waterborne polyurethane comprises the following components by mass: 15-35 parts of isophorone diisocyanate, 25-45 parts of modified polyether polyol, 5-10 parts of ring-opening compound, 2-6 parts of dimethylol propionic acid, 0.05-0.1 parts of dibutyltin dilaurate and 80-150 parts of deionized water;
[0010] The modified polyether polyol is obtained by esterification reaction of 10-20 parts by mass of polyether polyol and 2-5 parts by mass of DOPO;
[0011] The ring-opening compound is obtained by a ring-opening addition reaction between ethylene glycol diglycidyl ether and pentaerythritol phosphate, and the molar ratio of ethylene glycol diglycidyl ether to pentaerythritol phosphate is 1:2.
[0012] Furthermore, the filler includes one or more of zinc oxide, titanium oxide, zinc borate, expanded vermiculite, and sepiolite.
[0013] Furthermore, the auxiliary agent includes 0.2 to 0.4 parts of a defoaming agent, 0.5 to 1.0 parts of a dispersant and 2 to 5 parts of a film-forming auxiliary agent.
[0014] Defoaming agent: CF246; Dispersant: 5040; Film-forming aid: Alcohol ester 12.
[0015] Furthermore, the preparation method of the building fire retardant coating comprises the following steps:
[0016] S1: Preparation of modified waterborne polyurethane: Add isophorone diisocyanate, modified polyether polyol and ring-opening compound to acetone, add catalyst dibutyltin dilaurate, react with stirring at 50-55°C under nitrogen atmosphere, cool to room temperature, add dimethylolpropionic acid, continue to react with stirring at 50-55°C, add triethylamine after the reaction is completed, add deionized water, evaporate the acetone to obtain an emulsion.
[0017] S2: preparing a fire retardant coating: mixing waterborne polyurethane, filler, additives and water to obtain a fire retardant coating.
[0018] Furthermore, the modified polyether polyol is prepared by the following steps:
[0019] Weigh 10-20 parts by mass of polyether polyol and add it into a three-necked flask, then add 2-5 parts of DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide), 3-6 parts of triethylamine and 10-30 parts of dichloromethane, add 5-10 parts of carbon tetrachloride dropwise under ice bath, stir and react at room temperature, dilute with 50-100 parts of water after the reaction is completed, extract with ethyl acetate, dry with Na2SO4, and spin dry to obtain modified polyether polyol.
[0020] Furthermore, the ring-opening compound is prepared by the following steps:
[0021] 1 mol of ethylene glycol diglycidyl ether and 2 mol of pentaerythritol phosphate are added into a three-necked flask, and 1% of HZSM-5 molecular sieve is added as a catalyst. The mixture is reacted at 80-90° C. for 5-6 hours, and the catalyst is removed by filtration to obtain a ring-opening compound.
[0022] 3. Beneficial effects:
[0023] The invention introduces two different P-containing flame retardants, DOPO and pentaerythritol phosphate, into the hard and soft segments of polyurethane respectively, thereby modifying the polyurethane chain segments, increasing the fireproof performance of the polyurethane, and obtaining a building fireproof coating with excellent fireproof performance. DETAILED DESCRIPTION
[0024] The present invention is described in detail below.
[0025] Embodiment 1:
[0026] A fireproof building coating, comprising the following components by weight: 35 parts of modified waterborne polyurethane, 25 parts of zinc oxide, 5 parts of additives and 20 parts of water; the additives include 0.3 parts of defoamer CF246, 0.8 parts of dispersant 5040 and 3 parts of film-forming additive alcohol ester 12, all of which are purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0027] The modified waterborne polyurethane comprises the following components by mass: 25 parts of isophorone diisocyanate, 30 parts of modified polyether polyol, 6 parts of ring-opening compound, 4 parts of dimethylol propionic acid, 0.08 parts of dibutyltin dilaurate and 100 parts of water;
[0028] The modified polyether polyol is obtained by esterification reaction of 15 parts by weight of polyether polyol and 3 parts by weight of DOPO;
[0029] The ring-opening compound is obtained by a ring-opening addition reaction between ethylene glycol diglycidyl ether and pentaerythritol phosphate, wherein the molar ratio of ethylene glycol diglycidyl ether to pentaerythritol phosphate is 1:2.
[0030] Wherein, the polyether polyol is polyether polyol N210, MW.1000, hydroxyl value: 107-117 mg KOH / g.
[0031] The structural formula of DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide) is as follows:
[0032]
[0033] The structure of ethylene glycol diglycidyl ether is as follows:
[0034]
[0035] The structure of pentaerythritol phosphate is as follows:
[0036]
[0037] The preparation method of building fire retardant coating comprises the following steps:
[0038] S1: Preparation of modified waterborne polyurethane: Add isophorone diisocyanate, modified polyether polyol and ring-opening compound to acetone according to the above ratio, add dibutyltin dilaurate as a catalyst, stir and react at 55°C under nitrogen atmosphere, cool to room temperature, add dimethylolpropionic acid, continue to stir and react at 55°C, add triethylamine after the reaction is completed, add deionized water, and evaporate the acetone to obtain an emulsion.
[0039] S2: preparing a fire retardant coating: mixing waterborne polyurethane, filler, additives and water to obtain a fire retardant coating.
[0040] in:
[0041] The modified polyether polyol and the ring-opening compound are prepared by the following steps:
[0042] (1) The modified polyether polyol is prepared by the following steps:
[0043] Weigh 15 parts of polyether polyol by mass and add them into a three-necked flask, then add 3 parts of DOPO, 5 parts of triethylamine and 20 parts of dichloromethane, add 8 parts of carbon tetrachloride dropwise under an ice bath, stir and react at room temperature, dilute with 80 parts of water after the reaction, extract with ethyl acetate, dry with Na2SO4, and spin dry to obtain modified polyether polyol.
[0044] (2) The ring-opening compound is prepared by the following steps:
[0045] 1 mol of ethylene glycol diglycidyl ether and 2 mol of pentaerythritol phosphate were added into a three-necked flask, and 1% HZSM-5 molecular sieve was added as a catalyst. The mixture was reacted at 85° C. for 6 h, and the catalyst was removed by filtration to obtain a ring-opened compound.
[0046] Embodiment 2:
[0047] A fireproof building coating, comprising the following components by weight: 30 parts of modified waterborne polyurethane, 20 parts of expanded vermiculite, 4 parts of additives and 15 parts of water; the additives include 0.3 parts of defoamer CF246, 0.8 parts of dispersant 5040 and 3 parts of film-forming additive alcohol ester 12, all of which are purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0048] The modified waterborne polyurethane comprises the following components by mass: 30 parts of isophorone diisocyanate, 40 parts of modified polyether polyol, 8 parts of ring-opening compound, 5 parts of dimethylol propionic acid, 0.08 parts of dibutyltin dilaurate and 100 parts of water;
[0049] The modified polyether polyol is obtained by esterification reaction of 20 parts by weight of polyether polyol and 5 parts by weight of DOPO;
[0050] The ring-opening compound is obtained by a ring-opening addition reaction between ethylene glycol diglycidyl ether and pentaerythritol phosphate, wherein the molar ratio of ethylene glycol diglycidyl ether to pentaerythritol phosphate is 1:2.
[0051] Wherein, the polyether polyol is polyether polyol N210, MW.1000, hydroxyl value: 107-117 mg KOH / g.
[0052] The preparation method is the same as that of Example 1, except that the amounts of the components are different.
[0053] Embodiment 3:
[0054] A fireproof building coating, comprising the following components by weight: 40 parts of modified waterborne polyurethane, 30 parts of titanium oxide, 4 parts of additives and 25 parts of water; the additives include 0.3 parts of defoamer CF246, 0.8 parts of dispersant 5040 and 3 parts of film-forming additive alcohol ester 12, all of which are purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0055] The modified waterborne polyurethane comprises the following components by mass: 35 parts of isophorone diisocyanate, 35 parts of modified polyether polyol, 6 parts of ring-opening compound, 5 parts of dimethylol propionic acid, 0.08 parts of dibutyltin dilaurate and 100 parts of water;
[0056] The modified polyether polyol is obtained by esterification reaction of 18 parts by weight of polyether polyol and 3 parts by weight of DOPO;
[0057] The ring-opening compound is obtained by a ring-opening addition reaction between ethylene glycol diglycidyl ether and pentaerythritol phosphate, wherein the molar ratio of ethylene glycol diglycidyl ether to pentaerythritol phosphate is 1:2.
[0058] Wherein, the polyether polyol is polyether polyol N210, MW.1000, hydroxyl value: 107-117 mg KOH / g.
[0059] The preparation method is the same as that of Example 1, except that the amounts of the components are different.
[0060] Comparative Example 1:
[0061] A fireproof building coating, comprising the following components by weight: 35 parts of waterborne polyurethane, 25 parts of zinc oxide, 5 parts of additives and 20 parts of water; the additives include 0.3 parts of defoamer CF246, 0.8 parts of dispersant 5040 and 3 parts of film-forming additive alcohol ester 12, all of which are purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0062] The waterborne polyurethane comprises the following components by mass: 25 parts of isophorone diisocyanate, 30 parts of polyether polyol, 6 parts of glyceryl monostearate and 4 parts of dimethylol propionic acid, 0.08 parts of dibutyltin dilaurate and 100 parts of water;
[0063] Wherein, the polyether polyol is polyether polyol N210, MW.1000, hydroxyl value: 107-117 mg KOH / g.
[0064] Comparative Example 2:
[0065] A fireproof building coating, comprising the following components by weight: 35 parts of modified waterborne polyurethane, 6 parts of pentaerythritol phosphate, 25 parts of zinc oxide, 5 parts of additives and 20 parts of water; the additives include 0.3 parts of defoamer CF246, 0.8 parts of dispersant 5040 and 3 parts of film-forming additive alcohol ester 12, all of which are purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0066] The modified waterborne polyurethane comprises the following components by mass: 25 parts of isophorone diisocyanate, 30 parts of modified polyether polyol, 6 parts of glyceryl monostearate and 4 parts of dimethylol propionic acid, 0.08 parts of dibutyltin dilaurate and 100 parts of water;
[0067] The modified polyether polyol is obtained by esterification reaction of 15 parts by weight of polyether polyol and 3 parts by weight of DOPO;
[0068] Wherein, the polyether polyol is polyether polyol N210, MW.1000, hydroxyl value: 107-117 mg KOH / g.
[0069] Comparative Example 3:
[0070] A fire retardant coating for buildings, comprising the following components by mass: 35 parts of modified waterborne polyurethane, 6 parts of DOPO, 25 parts of zinc oxide, 5 parts of additives and 20 parts of water; the additives include 0.3 parts of defoamer CF246, 0.8 parts of dispersant 5040 and 3 parts of film-forming additive alcohol ester 12, all of which are purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0071] The modified waterborne polyurethane comprises the following components by mass: 25 parts of isophorone diisocyanate, 30 parts of polyether polyol, 6 parts of ring-opening compound, 4 parts of dimethylol propionic acid, 0.08 parts of dibutyltin dilaurate and 100 parts of water;
[0072] The ring-opening compound is obtained by a ring-opening addition reaction between ethylene glycol diglycidyl ether and pentaerythritol phosphate, wherein the molar ratio of ethylene glycol diglycidyl ether to pentaerythritol phosphate is 1:2.
[0073] Wherein, the polyether polyol is polyether polyol N210, MW.1000, hydroxyl value: 107-117 mg KOH / g.
[0074] Test example:
[0075] Experiment: Take the fire retardant coating obtained in Example 1-3 and Comparative Example 1-3, apply it to the surface of the steel plate, the coating thickness is 1mm, stand at room temperature 25℃ for 48h, vacuum dry at 60℃ for 24h, stand at 25℃, 65RH% for 7d to form a coating, prepare the sample, test its performance respectively and record the test results:
[0076] Mechanical properties test: The tensile properties of the coating samples were tested using a universal tensile machine with a tensile rate of 100 mm / min;
[0077] Adhesion test: Using GB / T9286 as the reference standard, use a paint film cross cutter to cross the surface of the coating sample, and use a pressure-sensitive tape to perform an adhesion pull test to determine the adhesion level (1-5);
[0078] Fire performance test: The small chamber combustion method in GB12441 is used as the reference method. A digital thermometer is used to record the temperature of the back-fired surface of the sample. The time when the back temperature reaches 220°C (back-fire time) is used as the performance index.
[0079] Carbon layer strength test: using RS300 stress rheometer, the distance between the flat plates is 10 cm, the compression time is 60 s, and the compression is to 1 mm; carbon layer formation conditions: nitrogen conditions, formation temperature 50-800 ° C, heating rate 20 ° C / min.
[0080]
[0081]
[0082] According to the data in the above table, compared with Comparative Example 1, Example 1-2 introduces two different P-containing flame retardants, DOPO and pentaerythritol phosphate, into the soft segment and hard segment of the polyurethane, respectively, which can significantly improve the fire retardant performance of the coating. Compared with Comparative Examples 2 and 3, in which two different P-containing flame retardants, DOPO and pentaerythritol phosphate, are added separately to the coating, the fire retardant performance is also significantly improved, and various properties such as tensile strength, adhesion level, back-fire time, and carbon layer strength are significantly improved.
[0083] Although the present invention has been disclosed as above in terms of preferred embodiments, they are not intended to limit the present invention. Anyone skilled in the art can make various changes or modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection defined by the claims of this application.
Claims
1. A fire retardant coating for buildings, characterized in that: The composition comprises the following components by weight: 30-40 parts of modified waterborne polyurethane, 20-30 parts of filler, 3-6 parts of additives and 15-30 parts of water; The modified waterborne polyurethane comprises the following components by mass: 15-35 parts of isophorone diisocyanate, 25-45 parts of modified polyether polyol, 5-10 parts of ring-opening compound, 2-6 parts of dimethylol propionic acid, 0.05-0.1 parts of dibutyltin dilaurate and 80-150 parts of deionized water; The modified polyether polyol is obtained by esterification reaction of 10-20 parts by mass of polyether polyol and 2-5 parts by mass of DOPO; The ring-opening compound is obtained by a ring-opening addition reaction between ethylene glycol diglycidyl ether and pentaerythritol phosphate, and the molar ratio of ethylene glycol diglycidyl ether to pentaerythritol phosphate is 1:
2.
2. A fire retardant coating for buildings according to claim 1, characterized in that: The filler includes one or more of zinc oxide, titanium oxide, zinc borate, expanded vermiculite and sepiolite.
3. A fire retardant coating for buildings according to claim 1, characterized in that: The auxiliary agent comprises 0.2 to 0.4 parts of a defoaming agent, 0.5 to 1.0 parts of a dispersant and 2 to 5 parts of a film-forming auxiliary agent.
4. The method for preparing a fire retardant coating for buildings according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: preparing modified waterborne polyurethane: adding isophorone diisocyanate, modified polyether polyol and ring-opening compound to acetone, adding catalyst dibutyltin dilaurate, stirring and reacting at 50-55°C under nitrogen atmosphere, adding dimethylolpropionic acid after cooling to room temperature, continuing stirring and reacting at 50-55°C, adding triethylamine after the reaction is completed, and then adding deionized water, and evaporating acetone to obtain an emulsion; S2: preparing a fire retardant coating: mixing waterborne polyurethane, filler, additives and water to obtain a fire retardant coating.
5. The method for preparing a fire retardant coating for buildings according to claim 4, characterized in that: The modified polyether polyol is prepared by the following steps: weighing 10-20 parts by mass of polyether polyol and adding it into a three-necked flask, then adding 2-5 parts of DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide), 3-6 parts of triethylamine and 10-30 parts of dichloromethane, dropping 5-10 parts of carbon tetrachloride under ice bath, stirring at room temperature for reaction, diluting with 50-100 parts of water after the reaction is completed, extracting with ethyl acetate, drying with Na2SO4, and spin drying to obtain the modified polyether polyol.
6. The method for preparing a fire retardant coating for buildings according to claim 4, characterized in that: The ring-opening compound is prepared by the following steps: 1 mol of ethylene glycol diglycidyl ether and 2 mol of pentaerythritol phosphate are added into a three-necked flask, 1% of HZSM-5 molecular sieve is added as a catalyst, reacting at 80-90° C. for 5-6 hours, filtering and removing the catalyst to obtain the ring-opening compound.
Citation Information
Patent Citations
Waterproof coating with flame-retardant and fireproof performance
CN113789113A
Composite positive electrode material and preparation method and application thereof
CN115863595A
Preparation method and application of flame-retardant polyester polyol containing DOPO and preparation method of flame-retardant polyurethane
CN116239763A
DOPO reactive flame retardant and preparation method and application thereof
CN117343103A
Polyisocyanate-Based Intumescent Coating
US20160222226A1
Cited By
Preparation process of waterborne polyurethane fireproof coating
CN120505032A
Preparation process of water-based polyurethane fireproof coating
CN120505032B
Preparation method of waterborne polyurethane fireproof coating
CN121555065A
A method for preparing a water-based polyurethane fire-retardant coating
CN121555065B