Pre-paving type composite waterproof coiled material
By using modified polyester material and multi-layer composite barrier film technology in the waterproof roll material, the waterproof and flame retardant performance are improved, the problem of insufficient performance of the waterproof roll material is solved, and higher quality of use and convenient construction are achieved.
Patent Information
- Application Number
- CN202411194874.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-19
AI Technical Summary
The waterproof coil is difficult to improve at the same time in both waterproof and flame retardant properties, resulting in poor performance of other performances and affecting the quality of use.
The pre-paved composite waterproof coil is designed with a seven-layer structure, in which the carcass reinforcement layer is prepared by modified polyester material, combined with phenethylphosphonic acid, N-bromosuccinimide and other raw materials to prepare flame retardant and waterproof intermediates, and improve overall performance through multi-layer composite barrier film and modified asphalt glue layer.
It effectively improves the flame retardant and waterproof performance of pre-paved composite waterproof coils, and simplifies the construction process, avoids environmental pollution, and has high bonding and peeling strength, so there is no need to fire in construction.
Smart Images

Figure CN118978873A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof roll materials, and in particular to a pre-laid composite waterproof roll material. Background Art
[0002] Waterproof rolls are rolls of waterproof materials made of asphalt, rubber or other organic materials. The waterproof material products made by impregnating asphalt or polymer waterproof materials on the base are provided in the form of rolls, which are called waterproof rolls; Chinese patent CN209904116U discloses a composite pre-laid waterproofing membrane, including an upper and lower mullite sand layer, wherein the upper and lower mullite sand layers include a high-adhesion self-adhesive rubber layer, a sewed polyester cloth reinforcement layer, a polyester base layer, and a thermosetting EVA film layer in order from top to bottom, wherein the mullite sand layer is made of mullite sand with a particle size of 8 to 12 meshes, the high-adhesion self-adhesive rubber layer is a polymer modified asphalt rubber layer, and the sewed polyester cloth reinforcement layer is arranged in the middle of the high-adhesion self-adhesive rubber layer, and mullite sand is pre-laid on the polymer modified asphalt layer; It improves construction efficiency and bonding with post-poured concrete, and enhances base bonding and waterproofing effects; however, the waterproof and flame-retardant properties of the waterproof membrane cannot be improved together, which will result in poor performance of other properties of the waterproof membrane, affecting its quality of use. Summary of the invention
[0003] The purpose of the present invention is to provide a pre-laid composite waterproofing membrane. The technical problem solved by the present invention is that if the waterproofing membrane cannot achieve the effect of jointly improving the waterproofing performance and the flame retardant performance, the waterproofing membrane will have poor performance in other properties, affecting its use quality.
[0004] The purpose of the present invention can be achieved through the following technical solutions: A pre-laid composite waterproofing membrane, the pre-laid composite waterproofing membrane consists of a seven-layer structure, which is composed of a bonding protective layer, a glue layer, a carcass reinforcement layer, a glue layer, a carcass reinforcement layer, a glue layer and a protective layer from top to bottom; Among them, the carcass reinforcement layer is a modified polyester tire; The modified polyester tire is prepared from modified polyester, and the preparation process of the modified polyester comprises the following steps: Step 1: under nitrogen protection, phenylethylphosphonic acid is added to carbon tetrachloride, the temperature is lowered to 0°C, and N-bromosuccinimide is added in three batches under light conditions; after the addition of N-bromosuccinimide is completed, light is maintained and the reaction temperature is controlled at 40°C to prepare intermediate 1; Step 2: Dissolve the intermediate 1 in ethanol, heat to 60°C with stirring, slowly add magnesium hydroxide after it is completely dissolved, raise the temperature to 80°C, reflux and continue stirring, react for 6 hours to obtain the intermediate 2; Step 3: reacting polyetheramine D230 and 1,3-di(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane at a constant temperature for 5 hours to obtain intermediate 3; Intermediate 2, N,N-diisopropylethylamine and tetrahydrofuran are mixed, and nitrogen is introduced for protection. At a speed of 200-300 r / min and a temperature of 0-5°C, the mixture is stirred for 10-20 min, and then intermediate 3 is added. The mixture is reacted for 3-5 h to obtain intermediate 4. Step 4: Mix terephthalic acid, intermediate 4, ethylene glycol and antimony trioxide to obtain a modified polyester material.
[0005] As a further solution of the present invention: in step 1, the dosage ratio of phenethylphosphonic acid, N-bromosuccinimide and carbon tetrachloride is controlled to be 1 mol: 1 mol: 400-600 mL.
[0006] As a further solution of the present invention: in step 2, the usage ratio of the intermediate 1, magnesium hydroxide and ethanol is controlled to be 1 mol: 2-2.2 mol: 700-900 mL.
[0007] As a further solution of the present invention: in step 3, the molar ratio of polyetheramine D230 and 1,3-bis(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane is controlled to be 1.5-1.7:1.
[0008] As a further scheme of the present invention: in step 3, the molar ratio of intermediate 2, intermediate 3 and N,N-diisopropylethylamine is 1:1:0.01-0.03 mol.
[0009] As a further solution of the present invention: in step 4, the mass ratio of terephthalic acid, intermediate 4, ethylene glycol and antimony trioxide is controlled to be 415:125-140:200:0.08.
[0010] As a further scheme of the present invention: in step 4, first start the esterification reaction, control the esterification reaction temperature to 230°C, the esterification reaction pressure to 250KPa, and the reaction time to 1-6h, then release the pressure in the reactor to normal pressure, then start the vacuum system, and at the same time raise the reaction temperature to 275°C, start the polycondensation reaction, control the vacuum degree in the reactor to be below 30Pa, and the reaction time to 1-5h.
[0011] As a further solution of the present invention: the bonding protective layer is mineral sand, resin-coated sand, non-woven fabric fibers, a bonding anti-sticking coating or a bonding polymer film layer.
[0012] As a further solution of the present invention: the protective layer is a multi-layer composite barrier film; the bottom layer material of the barrier film is one of ethylene acrylic acid copolymer, surin resin or TPU resin.
[0013] As a further solution of the present invention: the adhesive layer is any one of a modified asphalt adhesive layer, a hot melt adhesive or a butyl adhesive.
[0014] Beneficial effects of the present invention: The present invention uses phenethylphosphonic acid and N-bromosuccinimide as raw materials, and under light conditions, bromine replaces hydrogen on the phenethyl group to obtain an intermediate 1 of bromophenethylphosphonic acid; the phosphonic acid group of the intermediate 1 of bromophenethylphosphonic acid is reacted with magnesium hydroxide to obtain an intermediate 2 of a functional flame retardant of an organic-inorganic hybrid material; polyetheramine D230 and 1,3-di(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane are used as raw materials to prepare an intermediate 3 of an amino-terminated organic silicon intermediate; intermediate 2 and intermediate 3 are used as raw materials, and two bromines on intermediate 2 are respectively connected with two amino groups on intermediate 3 to obtain intermediate 4, so that intermediate 4 not only has good flame retardant performance of organic-inorganic synergistic effect, but also has waterproof performance of long-chain alkyl silane; terephthalic acid, intermediate 4 and ethylene glycol are used as raw materials to prepare a modified polyester, which can ensure that a copolymer prepared by adding intermediate 4 to a polyester molecular chain has good flame retardant performance and waterproof performance; Therefore, the present invention improves the carcass reinforcement layer in the pre-laid composite waterproof membrane, which can effectively improve the flame retardant and waterproof properties of the reinforcement layer, and based on this, further improve the flame retardant and waterproof properties of the pre-laid composite waterproof membrane; The structural design of the pre-laid composite waterproofing membrane of the present invention ensures that the protective layer does not need to be torn off, which will not pollute the environment and is more convenient to construct. The bottom layer material of the multi-layer composite barrier membrane can be bonded to the polyurethane waterproof coating. During construction, the membrane can be laid after the polyurethane waterproof coating is applied. After the polyurethane waterproof coating is cured, it can be tightly bonded to the membrane. The bonding peeling strength is large, and the peeling strength is ≥2N / 50mm. No fire is required during the construction process. The multi-layer composite barrier membrane has barrier properties and can prevent small molecular oils in asphalt from migrating into the polyurethane, thereby affecting its bonding performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The present invention will be further described below in conjunction with the accompanying drawings.
[0016] Figure 1 It is a structural schematic diagram of the pre-laid composite waterproofing membrane of the present invention.
[0017] In the figure: 1, bonding protective layer; 2, first rubber layer; 3, first tire body reinforcement layer; 4, second rubber layer; 5, second tire body reinforcement layer; 6, third rubber layer; 7, protective layer. DETAILED DESCRIPTION
[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] Example 1 See also Figure 1 As shown, the present invention is a pre-laid composite waterproofing membrane, which is composed of a seven-layer structure, which is composed of a bonding protective layer 1, a first adhesive layer 2, a first carcass reinforcement layer 3, a second adhesive layer 4, a second carcass reinforcement layer 5, a third adhesive layer 6 and a protective layer 7 from top to bottom; The bonding protective layer 1 is bonded together by pre-laying and pouring with wet concrete, and the bonding protective layer 1 is mineral sand, resin-coated sand, non-woven fabric fiber, bonding anti-stick coating or bonding polymer film layer; The protective layer 7 is a multi-layer composite barrier film; the bottom layer material of the barrier film is one of ethylene acrylic acid copolymer (EAA), sarin resin or TPU resin; The first adhesive layer 2, the second adhesive layer 4 and the third adhesive layer 6 are all any one of modified asphalt adhesive layer, hot melt adhesive or butyl adhesive; The first carcass reinforcement layer 3 and the second carcass reinforcement layer 5 are both modified polyester tires; The first carcass reinforcement layer 3 and the second carcass reinforcement layer 5 have a tensile force of 50-2000N / 50mm and a breaking elongation of 10-1000%; The thickness of the first carcass reinforcement layer 3 and the second carcass reinforcement layer 5 is 0.05 mm to 1.5 mm.
[0020] The overlapping method of the waterproof membrane is a bite-type overlap, the overlap width is 8-15mm, and it is inserted from end A to end B, and can be overlapped by hot melting, welding or self-adhesion; The modified polyester tire is prepared from modified polyester, and the preparation process of the modified polyester comprises the following steps: Step 1: under nitrogen protection, add phenylethylphosphonic acid to carbon tetrachloride, lower the temperature to 0°C, and add N-bromosuccinimide in three batches under light (250W); after the addition of N-bromosuccinimide is completed, keep the light, control the reaction temperature at 40°C during this process, and monitor the progress of the reaction by TLC ((PE:EA)=5:1); after the reaction is completed, filter the reaction solution, evaporate the filtrate to remove carbon tetrachloride, dilute the obtained organic matter with 50mL of ether, and wash twice with saturated sodium chloride; combine the organic layers and dry them with anhydrous sodium sulfate; after drying, filter out the sodium sulfate, evaporate the solvent, and obtain intermediate 1; Wherein, the dosage ratio of phenylethylphosphonic acid, N-bromosuccinimide and carbon tetrachloride is controlled to be 1 mol: 1 mol: 400 mL; Step 2: Dissolve the intermediate 1 in ethanol, stir and heat to 60°C, slowly add magnesium hydroxide after it is completely dissolved, heat to 80°C, reflux and continue stirring, react for 6 hours, filter, wash three times, and dry in an oven for 5 hours to obtain the intermediate 2; Wherein, the dosage ratio of intermediate 1, magnesium hydroxide and ethanol is controlled to be 1 mol: 2 mol: 700 mL; Step 3: reacting polyetheramine D230 and 1,3-di(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane at a constant temperature for 5 hours to obtain intermediate 3; Intermediate 2, N,N-diisopropylethylamine and tetrahydrofuran are mixed, and nitrogen is introduced for protection. At a speed of 200-300 r / min and a temperature of 0-5°C, the mixture is stirred for 10-20 min, and then intermediate 3 is added. The mixture is reacted for 3-5 h to obtain intermediate 4. Wherein, the molar ratio of polyetheramine D230 and 1,3-di(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane is controlled to be 1.5:1; The molar ratio of intermediate 2, intermediate 3 and N,N-diisopropylethylamine is 1:1:0.01 mol; Step 4: terephthalic acid, intermediate 4, ethylene glycol and antimony trioxide are mixed for reaction, and the esterification reaction is first started. The esterification reaction temperature is controlled to be 230°C, the esterification reaction pressure is 250KPa, and the reaction time is 1-6h. Then the pressure in the reactor is released to normal pressure, and then the vacuum system is turned on. At the same time, the reaction temperature is raised to 275°C, and the polycondensation reaction is started. The vacuum degree in the reactor is controlled to be below 30Pa, and the reaction time is 1-5h to obtain a modified polyester material; Among them, the mass ratio of terephthalic acid, intermediate 4, ethylene glycol and antimony trioxide is controlled to be 415:125:200:0.08.
[0021] Example 2 The difference from Example 1 is that: The modified polyester tire is prepared from modified polyester, and the preparation process of the modified polyester comprises the following steps: Step 1: under nitrogen protection, add phenylethylphosphonic acid to carbon tetrachloride, lower the temperature to 0°C, and add N-bromosuccinimide in three batches under light (250W); after the addition of N-bromosuccinimide is completed, keep the light, control the reaction temperature at 40°C during this process, and monitor the progress of the reaction by TLC ((PE:EA)=5:1); after the reaction is completed, filter the reaction solution, evaporate the filtrate to remove carbon tetrachloride, dilute the obtained organic matter with 50mL of ether, and wash twice with saturated sodium chloride; combine the organic layers and dry them with anhydrous sodium sulfate; after drying, filter out the sodium sulfate, evaporate the solvent, and obtain intermediate 1; Wherein, the dosage ratio of phenylethylphosphonic acid, N-bromosuccinimide and carbon tetrachloride is controlled to be 1 mol: 1 mol: 500 mL; Step 2: Dissolve the intermediate 1 in ethanol, stir and heat to 60°C, slowly add magnesium hydroxide after it is completely dissolved, heat to 80°C, reflux and continue stirring, react for 6 hours, filter, wash three times, and dry in an oven for 5 hours to obtain the intermediate 2; Wherein, the dosage ratio of intermediate 1, magnesium hydroxide and ethanol is controlled to be 1 mol: 2.1 mol: 800 mL; Step 3: reacting polyetheramine D230 and 1,3-di(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane at a constant temperature for 5 hours to obtain intermediate 3; Intermediate 2, N,N-diisopropylethylamine and tetrahydrofuran are mixed, and nitrogen is introduced for protection. At a speed of 200-300 r / min and a temperature of 0-5°C, the mixture is stirred for 10-20 min, and then intermediate 3 is added. The mixture is reacted for 3-5 h to obtain intermediate 4. Wherein, the molar ratio of polyetheramine D230 and 1,3-di(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane is controlled to be 1.6:1; The molar ratio of intermediate 2, intermediate 3 and N,N-diisopropylethylamine is 1:1:0.02 mol; Step 4: terephthalic acid, intermediate 4, ethylene glycol and antimony trioxide are mixed for reaction, and the esterification reaction is first started. The esterification reaction temperature is controlled to be 230°C, the esterification reaction pressure is 250KPa, and the reaction time is 1-6h. Then the pressure in the reactor is released to normal pressure, and then the vacuum system is turned on. At the same time, the reaction temperature is raised to 275°C, and the polycondensation reaction is started. The vacuum degree in the reactor is controlled to be below 30Pa, and the reaction time is 1-5h to obtain a modified polyester material; Among them, the mass ratio of terephthalic acid, intermediate 4, ethylene glycol and antimony trioxide is controlled to be 415:132:200:0.08.
[0022] Example 3 The difference from Example 1 is that the modified polyester tire is prepared from modified polyester, and the preparation process of the modified polyester includes the following steps: Step 1: under nitrogen protection, add phenylethylphosphonic acid to carbon tetrachloride, lower the temperature to 0°C, and add N-bromosuccinimide in three batches under light (250W); after the addition of N-bromosuccinimide is completed, keep the light, control the reaction temperature at 40°C during this process, and monitor the progress of the reaction by TLC ((PE:EA)=5:1); after the reaction is completed, filter the reaction solution, evaporate the filtrate to remove carbon tetrachloride, dilute the obtained organic matter with 50mL of ether, and wash twice with saturated sodium chloride; combine the organic layers and dry them with anhydrous sodium sulfate; after drying, filter out the sodium sulfate, evaporate the solvent, and obtain intermediate 1; Wherein, the dosage ratio of phenylethylphosphonic acid, N-bromosuccinimide and carbon tetrachloride is controlled to be 1 mol: 1 mol: 600 mL; Step 2: Dissolve the intermediate 1 in ethanol, stir and heat to 60°C, slowly add magnesium hydroxide after it is completely dissolved, heat to 80°C, reflux and continue stirring, react for 6 hours, filter, wash three times, and dry in an oven for 5 hours to obtain the intermediate 2; Wherein, the dosage ratio of intermediate 1, magnesium hydroxide and ethanol is controlled to be 1 mol: 2.2 mol: 700-900 mL; Step 3: reacting polyetheramine D230 and 1,3-di(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane at a constant temperature for 5 hours to obtain intermediate 3; Intermediate 2, N,N-diisopropylethylamine and tetrahydrofuran are mixed, and nitrogen is introduced for protection. At a speed of 200-300 r / min and a temperature of 0-5°C, the mixture is stirred for 10-20 min, and then intermediate 3 is added. The mixture is reacted for 3-5 h to obtain intermediate 4. Wherein, the molar ratio of polyetheramine D230 and 1,3-di(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane is controlled to be 1.7:1; The molar ratio of intermediate 2, intermediate 3 and N,N-diisopropylethylamine is 1:1:0.03 mol; Step 4: terephthalic acid, intermediate 4, ethylene glycol and antimony trioxide are mixed for reaction, and the esterification reaction is first started. The esterification reaction temperature is controlled to be 230°C, the esterification reaction pressure is 250KPa, and the reaction time is 1-6h. Then the pressure in the reactor is released to normal pressure, and then the vacuum system is turned on. At the same time, the reaction temperature is raised to 275°C, and the polycondensation reaction is started. The vacuum degree in the reactor is controlled to be below 30Pa, and the reaction time is 1-5h to obtain a modified polyester material; Among them, the mass ratio of terephthalic acid, intermediate 4, ethylene glycol and antimony trioxide is controlled to be 415:140:200:0.08.
[0023] Comparative Example 1 Comparative Example 1 uses the polyester tire in the waterproof membrane with Chinese patent number CN104647845B; The polyester tires of Examples 1-3 and Comparative Example 1 were tested for performance: The test items include: the limiting oxygen index (LOI) test was measured using an HC–2CZ oxygen index instrument (Nanjing Shangyuan Analytical Instrument Factory, Nanjing, China) based on the Chinese standard GB / T1040-92; the specimen size was 130 mm × 6.5 mm × 3.5 mm.
[0024] Water contact angle The water contact angle of polyester tires was tested and analyzed using the JCY series-dynamic and static contact angle meter of Shanghai Fangrui Instrument Co., Ltd. The water contact angle of polyester tires was tested at room temperature, 20 test samples were cut from the fiber membrane, and the volume of the water drop was rotated to 3μL during the test. The software recorded the state of the water drop after falling, and measured the angle of the water drop; the hydrophobic performance of the polyester tire was analyzed according to the numerical value of the water contact angle of the polyester tire; The test results are shown in the table below:
[0025] It can be seen from the above table that the polyester tire prepared in the embodiment of the present invention has better flame retardancy and waterproofness than the existing polyester tire.
[0026] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A pre-laid composite waterproofing membrane, characterized in that: The pre-laid composite waterproof membrane consists of seven layers, from top to bottom: bonding protective layer, glue layer, carcass reinforcement layer, glue layer, carcass reinforcement layer, glue layer and protective layer; Among them, the carcass reinforcement layer is a modified polyester tire; The modified polyester tire is prepared from modified polyester, and the preparation process of the modified polyester comprises the following steps: Step 1: under nitrogen protection, phenylethylphosphonic acid is added to carbon tetrachloride, the temperature is lowered to 0°C, and N-bromosuccinimide is added in three batches under light conditions; after the addition of N-bromosuccinimide is completed, light is maintained and the reaction temperature is controlled at 40°C to prepare intermediate 1; Step 2: Dissolve the intermediate 1 in ethanol, heat to 60°C with stirring, slowly add magnesium hydroxide after it is completely dissolved, raise the temperature to 80°C, reflux and continue stirring, react for 6 hours to obtain the intermediate 2; Step 3: reacting polyetheramine D230 and 1,3-di(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane at a constant temperature for 5 hours to obtain intermediate 3; Intermediate 2, N,N-diisopropylethylamine and tetrahydrofuran are mixed, and nitrogen is introduced for protection. At a speed of 200-300 r / min and a temperature of 0-5°C, the mixture is stirred for 10-20 min, and then intermediate 3 is added. The mixture is reacted for 3-5 h to obtain intermediate 4. Step 4: Mix terephthalic acid, intermediate 4, ethylene glycol and antimony trioxide to obtain a modified polyester material.
2. The pre-laid composite waterproofing membrane according to claim 1, characterized in that: In step 1, the dosage ratio of phenethylphosphonic acid, N-bromosuccinimide and carbon tetrachloride is controlled to be 1 mol: 1 mol: 400-600 mL.
3. The pre-laid composite waterproofing membrane according to claim 1, characterized in that: In step 2, the usage ratio of the intermediate 1, magnesium hydroxide and ethanol is controlled to be 1 mol: 2-2.2 mol: 700-900 mL.
4. The pre-laid composite waterproofing membrane according to claim 1, characterized in that: In step 3, the molar ratio of polyetheramine D230 and 1,3-bis(3-glycidylpropyl)-1,1,3,3-tetramethyldisiloxane is controlled to be 1.5-1.7:
1.
5. The pre-laid composite waterproofing membrane according to claim 1, characterized in that: In step 3, the molar ratio of intermediate 2, intermediate 3 and N,N-diisopropylethylamine is 1:1:0.01-0.03 mol.
6. The pre-laid composite waterproofing membrane according to claim 1, characterized in that: In step 4, the mass ratio of terephthalic acid, intermediate 4, ethylene glycol and antimony trioxide is controlled to be 415:125-140:200:0.
08.
7. The pre-laid composite waterproofing membrane according to claim 1, characterized in that: In step 4, the esterification reaction is first started, the esterification reaction temperature is controlled to 230°C, the esterification reaction pressure is controlled to 250KPa, and the reaction time is 1-6h. Then the pressure in the reactor is released to normal pressure, and then the vacuum system is turned on. At the same time, the reaction temperature is raised to 275°C, and the condensation reaction is started. The vacuum degree in the reactor is controlled to be below 30Pa, and the reaction time is 1-5h.
8. The pre-laid composite waterproofing membrane according to claim 1, characterized in that: The bonding protective layer is mineral sand, resin-coated sand, non-woven fabric fiber, bonding anti-sticking coating or bonding polymer film layer.
9. The pre-laid composite waterproofing membrane according to claim 1, characterized in that: The protective layer is a multi-layer composite barrier film; the bottom layer material of the barrier film is one of ethylene acrylic acid copolymer, sarling resin or TPU resin.
10. The pre-laid composite waterproofing membrane according to claim 1, characterized in that: The adhesive layer is any one of modified asphalt adhesive layer, hot melt adhesive or butyl adhesive.