MOF-quantum dot down-conversion light conversion adhesive film and preparation method thereof
By using MOF-quantum dot downconversion technology in photovoltaic films, the problems of ultraviolet absorption efficiency and distribution uniformity of existing down-transfer films are solved, the power and stability of photovoltaic modules are improved, and the ultraviolet absorbers are reduced. The dependence of the company achieves more efficient photoelectric conversion and longer service life.
Patent Information
- Application Number
- CN202411109817.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-19
AI Technical Summary
The existing down-transfer adhesive films have limited efficiency in ultraviolet absorption, and the uneven distribution of the optical converter makes it difficult to increase the power of the photovoltaic module and require additional expensive ultraviolet absorbers to protect the substrate.
The MOF-quantum dot down-conversion photoconversion adhesive film is used to coat the quantum dots in the MOF structure, and the light capture ability of the MOF improves the light conversion efficiency, and the surface modifier avoids quantum dot agglomeration, thereby improving stability.
It improves the photoelectric conversion efficiency and service life of photovoltaic modules, reduces the damage to ultraviolet light, reduces the dependence on ultraviolet absorbers, and improves the long-term stability and cost-effectiveness of the adhesive film.
Smart Images

Figure BDA0004991850840000031 
Figure BDA0004991850840000111 
Figure FDA0004991850830000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photovoltaic adhesive films, and in particular relates to a MOF-quantum dot down-conversion light-converting adhesive film and a preparation method thereof. Background Art
[0002] As fossil energy is becoming increasingly depleted, solar energy, as a renewable green energy source, has become the focus of development and research, among which solar cell technology has developed rapidly. The distribution of the solar spectrum is a broadband spectrum from 200nm to 2500nm. For crystalline silicon solar photovoltaic cells, due to its semiconductor band gap of 1.1eV, it can only respond to light waves from 200nm to 1200nm. For high-energy photons, such as ultraviolet light and blue-green light, since the absorption of one photon can only produce one electron-hole pair, the other energy is lost in the form of heat through lattice resonance; and light with a wavelength greater than 1200nm cannot be absorbed by crystalline silicon solar photovoltaic cells, and this part of the sunlight energy is completely lost. According to calculations, for the energy in the solar spectrum, the part that can be effectively utilized by the crystalline silicon solar photovoltaic cells currently on the market is about 486W / m 2 Of the energy that cannot be effectively utilized, 164W / m 2 The part that can be used for down conversion (UV to visible light) is 149W / m 2 .
[0003] At present, it is difficult to increase the power of photovoltaic modules. A 0.2% increase in module power, combined with the scale effect of the photovoltaic industry, is of considerable value. As an important component of photovoltaic modules, photovoltaic light conversion films have made certain contributions to the improvement of photovoltaic module power. The more common conventional photovoltaic light conversion films are the down-conversion mode. For example, patent application CN116741866A discloses a composite film and a photovoltaic module. The composite film includes a cut-off layer, a first isolation layer and a lower light conversion layer stacked in sequence. The cut-off layer is a film containing a cut-off agent for controlling the spectral irradiation range; the lower light conversion layer is a film with a down-conversion function for converting the ultraviolet band into the visible light band. The first isolation layer is used to isolate the cut-off layer and the lower light conversion layer from each other. The photovoltaic module includes a cell, and the above-mentioned composite film is provided on at least one side of the cell. The lower light conversion layer of the composite film is close to the cell, and the cut-off layer is far away from the cell. Photovoltaic modules encapsulated with composite films can maintain a high light conversion effect for a long time, ensure the maximum light conversion effect, and greatly improve the output power and reliability of the module.
[0004] However, on the one hand, the light-converting agent used in the existing lower light-converting adhesive film has limited absorption of ultraviolet rays. In order to avoid damage to the substrate EVA by ultraviolet light, it is necessary to add an ultraviolet absorber (or set a cutoff layer). However, the ultraviolet absorber only has absorption and reflection properties for the ultraviolet band of 200nm-400nm and is expensive. On the other hand, the existing light-converting adhesive film generally adopts a melt casting film forming process of blending the light-converting agent with EVA particles and other components. When the light-converting agent component is less, it is very easy to cause uneven distribution of the light-converting agent in the adhesive film, and when the component is more, it is easy to cause the light-converting agent to agglomerate.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a MOF-quantum dot down-conversion light-converting adhesive film and a preparation method thereof. The present invention uses MOFs materials to cover the surface of quantum dots. On the one hand, the light capture ability of the MOF material itself can be used to improve the light conversion efficiency of the quantum dots through energy transfer, increase the photoelectric conversion efficiency of the component, and improve the service life of the component; on the other hand, the quantum dots are encapsulated in the MOF structure and the surface of the quantum dots is modified, which not only avoids the agglomeration between the quantum dots, improves the compatibility of the quantum dots with the matrix material, but also provides good protection for the quantum dots, making them have more excellent stability, thereby improving the long-term stability of the light conversion performance of the photovoltaic component.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] A method for preparing a MOF-quantum dot down-conversion light-converting adhesive film, wherein the preparation method comprises the following steps:
[0009] Step 1: Surface modification of quantum dots
[0010] Using a surface modifier to modify the surface of the quantum dots to obtain modified quantum dots;
[0011] Step 2: Synthesis of MOF-quantum dot nanomaterials
[0012] The modified quantum dots are encapsulated inside the MOF organic framework to synthesize MOF-quantum dot nanomaterials;
[0013] Step 3: Preparation of MOF-quantum dot masterbatch particles
[0014] The MOF-quantum dot nanomaterials are mixed with EVA particles, and then melted, extruded, and granulated to obtain MOF-quantum dot masterbatch particles;
[0015] Step 4: Preparation of MOF-quantum dot light-converting adhesive film
[0016] The MOF-quantum dot masterbatch particles, EVA particles, and other components are uniformly mixed and then tape-cast to obtain a MOF-quantum dot light-converting adhesive film.
[0017] The MOF-quantum dots used in the present invention have the characteristics of high absorption coefficient and high fluorescence efficiency for ultraviolet rays, so there is no need to add ultraviolet absorbers, and the transmittance requirements of the light-converting film in the ultraviolet region can be achieved, and this part of ultraviolet light can be converted into visible light for use, instead of the ultraviolet absorbers that can only absorb and reflect ultraviolet light, causing waste of solar energy. In addition, the present invention first mixes the light-converting agent, MOF-quantum dots, with EVA particles for extrusion granulation to form EVA masterbatch particles, and then makes the masterbatch particles, EVA particles and other components into a film, which greatly ensures the uniformity of the distribution of the light-converting agent.
[0018] Furthermore, in step 1,
[0019] The surface modifier is one or more of pyridine, mercaptopropionic acid, mercaptoalkanoic acid, tri-n-octylphosphine oxide, polyethylene glycol, polyamide-amine, polyacrylic acid-1,2-distearoyl-sn-glycerol-3-phosphatidylethanolamine, and cucurbituril;
[0020] The quantum dots are one or more of CdSe, CdS, CdZnSe, CdZnS, CdZnSeS, CdSe / ZnS, CdSe / CdZnS, CdZnS / ZnS, CdZnSeS / ZnS, CdZnSe / CdZnS, CdSe / ZnSe, ZnSe / ZnS, CdSe / CdZnS / ZnS, CsPbBr3, CsPb(Cl / Br)3, and InP.
[0021] Furthermore, in step 2, the MOF organic framework is one or more of IRMOF-3, MOF-5, UiO-66, PCN-333, PCN-224, ZIF-8, ZIF-67, ZIF-365, MIL-88B, MIL-101, MIL-100, and MIL-125.
[0022] Furthermore, in step 3, the content of MOF-quantum dot nanomaterials in the MOF-quantum dot masterbatch particles is 1%-10%.
[0023] Furthermore, in step 4, the other ingredients include a cross-linking agent, a co-cross-linking agent, a silane coupling agent, a light stabilizer and an antioxidant.
[0024] Furthermore, in step 4, the amounts of the components are as follows:
[0025]
[0026] Further,
[0027] The cross-linking agent is one or more of tert-butyl peroxy-2-ethylhexyl carbonate, 1,1-di-tert-butyl peroxide-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, and tert-amyl peroxy-2-ethylhexyl carbonate;
[0028] The auxiliary cross-linking agent is one or more of triallyl isocyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, triallyl cyanurate, ethoxymethylpropane triacrylate, and propoxy trimethylolpropane triacrylate;
[0029] The silane coupling agent is one or more of γ-(methacryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane, vinyltriethoxysilane, and γ-glycidyloxypropyltrimethoxysilane;
[0030] The light stabilizer is one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinylethanol) succinate, and bis(1,2,2,6,6-pentamethylpiperidinol) sebacate;
[0031] The antioxidant is one or more of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-thiobis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], tris[2.4-di-tert-butylphenyl] phosphite, bis(2.4-di-tert-butylphenyl) pentaerythritol diphosphite, tris(nonylphenyl) phosphite, and triphenyl phosphite.
[0032] Furthermore, in step 3, the temperature of the feeding section, the extrusion section and the discharge section of the granulator are all 70-120°C, preferably 80-100°C.
[0033] Furthermore, in step 4, the temperature in the tape casting process is 120-150° C., and the thickness of the film is 0.2-0.5 mm.
[0034] The present invention also provides a MOF-quantum dot down-conversion light-converting adhesive film prepared by the preparation method.
[0035] Compared with the prior art, the present invention has the following advantages:
[0036] (1) The present invention utilizes the light capture ability of MOFs materials to cover the surface of quantum dots, and improves the light conversion efficiency of quantum dots through energy transfer (improves ultraviolet absorption ability and luminous efficiency). As a result, the available visible light increases, and the photoelectric conversion efficiency of the component increases accordingly; the ultraviolet absorption ability is improved, the impact of ultraviolet light on photovoltaic components is reduced, and the service life of the components is extended accordingly.
[0037] (2) In the present invention, due to the strong ultraviolet absorption ability of MOF-quantum dot nanomaterials, there is no need to add additional ultraviolet absorbers or set ultraviolet cutoff layers during the preparation of the film. The structure is simple, which can not only increase the visible light transmittance of the film, but also reduce costs.
[0038] (3) In addition to improving efficiency, MOFs materials can coat and modify quantum dots, which can not only prevent the agglomeration of quantum dots, but also protect the quantum dots and improve the stability of quantum dots, thereby ensuring the long-term effectiveness of the film's light conversion performance. DETAILED DESCRIPTION
[0039] The following are specific embodiments of the present invention, and the embodiments are intended to further describe the present invention rather than to limit the present invention.
[0040] Example 1. Preparation of IRMOF3-CdZnS / ZnS light-converting adhesive film
[0041] Step 1: Surface modification of quantum dots
[0042] A 100 mg / ml CdZnS / ZnS quantum dot hexane solution (1 ml) was repeatedly precipitated-dispersed-precipitated twice with chloroform-acetone-chloroform, and finally dispersed with pyridine. The resulting dispersed solution was heated to 80°C and stirred to allow the quantum dots and pyridine to fully exchange ligands. After the upper layer liquid was clarified, it was cooled to room temperature, and excess chloroform was added to precipitate the quantum dots. Pyridine (1 ml) was used for dispersion again to obtain a 100 mg / ml CdZnS / ZnS pyridine solution.
[0043] Step 2: Synthesis of MOF-quantum dot nanomaterials
[0044] 2-aminoterephthalic acid (0.1mmol) and triethylamine (0.20mmol) were added to DMF solution (10mL) in advance and mixed and stirred to obtain a neutral 2-aminoterephthalic acid / DMF solution; 10μL of the CdZnS / ZnS pyridine solution obtained in step 1 was added to 9ml of DMF solution for dilution to obtain a CdZnS / ZnS / DMF solution; a DMF solution containing Zn(OAc)2·2H2O (30mmol) and a neutral 2-aminoterephthalic acid / DMF solution were respectively added dropwise into the CdZnS / ZnS / DMF solution at a rate of 1.0mL / h using two syringe pumps. After the addition was completed, stirring was continued for 1h, the suspension was aspirated, and the suspension was continued to be stirred at room temperature for 24h. The product was collected by centrifugation, and then washed three times with DMF / ethanol and dried under reduced pressure to obtain an IRMOF3-CdZnS / ZnS composite nanomaterial.
[0045] Step 3: Preparation of MOF-quantum dot masterbatch particles
[0046] Take 10g IRMOF3-CdZnS / ZnS composite nanomaterial and 90g EVA particles, mix them evenly, and add them into a twin-screw extruder granulator. The temperatures of the feed section, extrusion section and discharge section of the granulator are set to 80℃, 85℃ and 90℃ respectively. After melting, extrusion, wire drawing and pelletizing, MOF-quantum dot masterbatch particles with a particle size of 1mm are finally obtained.
[0047] Step 4: Preparation of MOF-quantum dot light-converting adhesive film
[0048] Take 10gMOF-quantum dot masterbatch particles, 990gEVA particles, 10g crosslinker tert-butyl peroxy-2-ethylhexyl carbonate, 5g auxiliary crosslinker triallyl isocyanurate, 5g silane coupling agent vinyl trimethoxysilane, 5g antioxidant β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl ester, 5g light stabilizer bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and mix them evenly, then pour them into an extruder, heat them to 140°C, inject the molten raw materials into a mold, and finally obtain an IRMOF3-CdZnS / ZnS light-converting film with a film thickness of 0.2mm after being cast.
[0049] Example 2: Preparation of MOF-5-CdZnSeS / ZnS light-converting adhesive film
[0050] Step 1: Surface modification of quantum dots
[0051] A 100 mg / ml CdZnSeS / ZnS quantum dot hexane solution (1 ml) was repeatedly precipitated-dispersed-precipitated twice with chloroform-acetone-chloroform, and finally dispersed with pyridine. The resulting dispersed solution was heated to 80°C and stirred to allow the quantum dots and pyridine to fully exchange ligands. After the upper layer liquid was clarified, it was cooled to room temperature, and excess chloroform was added to precipitate the quantum dots. Pyridine (1 ml) was used for dispersion again to obtain a 100 mg / ml CdZnSeS / ZnS pyridine solution.
[0052] Step 2: Synthesis of MOF-quantum dot nanomaterials
[0053] Dissolve terephthalic acid (30 mg) and Zn(NO3)2·6H2O (144 mg) in DMF solution (5 ml) and stir evenly. Take the CdZnSeS / ZnS pyridine solution (20 μl) obtained in step 1 and add it dropwise to the DMF solution at a rate of 1.0 mL / h. Subsequently, add polyvinyl pyrrolidone (900 mg) / methanol (6 ml) solution to the above DMF liquid, stir for 1 hour, and transfer the suspension to a high-pressure reactor equipped with a polytetrafluoroethylene liner and react at 120°C for 12 hours. After cooling to room temperature, collect the product by centrifugation and wash it three times with DMF / ethanol, and dry it under reduced pressure to obtain MOF5-CdZnSeS / ZnS composite nanomaterials. Step 3. Prepare MOF-quantum dot masterbatch particles
[0054] Take 10gMOF5-CdZnSeS / ZnS composite nanomaterial and 90gEVA particles, mix them evenly, and add them into a twin-screw extruder granulator. The temperatures of the feed section, extrusion section and discharge section of the granulator are set to 80℃, 85℃ and 90℃ respectively. After melting, extrusion, wire drawing and pelletizing, MOF-quantum dot masterbatch particles with a particle size of 3mm are finally obtained.
[0055] Step 4: Preparation of MOF-quantum dot light-converting adhesive film
[0056] Take 10gMOF-quantum dot masterbatch particles, 990gEVA particles, 10g crosslinker tert-butyl peroxy-2-ethylhexyl carbonate, 5g auxiliary crosslinker triallyl isocyanurate, 5g silane coupling agent vinyl trimethoxysilane, 5g antioxidant β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl ester, 5g light stabilizer bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and mix them evenly, then pour them into an extruder, heat them to 140°C, inject the molten raw materials into a mold, and perform tape casting to finally obtain a MOF-5-CdZnSeS / ZnS light-converting film with a film thickness of 0.5mm.
[0057] Example 3: Preparation of UiO66-CdSe light-converting adhesive film
[0058] Step 1: Surface modification of quantum dots
[0059] A 100 mg / ml CdSe quantum dot hexane solution (1 ml) was repeatedly precipitated-dispersed-precipitated twice with chloroform-acetone-chloroform, and finally dispersed with mercaptopropionic acid. The resulting dispersed solution was heated to 80°C and stirred to allow the quantum dots to fully exchange ligands with oleic acid. After the upper layer liquid was clarified, it was cooled to room temperature, and excess chloroform was added to precipitate the quantum dots. Mercaptopropionic acid (1 ml) was used to disperse again to obtain a 100 mg / ml CdSe mercaptopropionic acid solution.
[0060] Step 2: Synthesis of MOF-quantum dot nanomaterials
[0061] Take the CdSe mercaptopropionic acid solution (10μL) obtained in step 1 and dissolve it in DMF solution (10ml) for dilution to obtain CdSe / DMF solution. Add ZrCl4 (125mg) and terephthalic acid (123mg) to 5mlDMF and stir until completely dissolved. Use two syringe pumps to drop DMF solution (5ml) dissolved in concentrated hydrochloric acid (1ml, 37%) and ZrCl4-terephthalic acid / DMF solution into the CdSe / DMF solution at a rate of 1.0mL / h. After the addition is completed, continue stirring for 1h. Transfer the suspension to a high-pressure reactor equipped with a polytetrafluoroethylene liner and react at 80℃ for 24h. After cooling to room temperature, collect the product by centrifugation, wash it three times with DMF / ethanol solution, and dry it under reduced pressure to obtain UiO66-CdSe composite nanomaterials. Step 3, preparation of MOF-quantum dot masterbatch particles
[0062] Take 10g UiO66-CdSe composite nanomaterial and 90g EVA particles, mix them evenly, and add them into a twin-screw extruder granulator. The temperatures of the feed section, extrusion section and discharge section of the granulator are set to 80℃, 85℃ and 90℃ respectively. After melting, extrusion, wire drawing and pelletizing, MOF-quantum dot masterbatch particles with a particle size of 2mm are finally obtained.
[0063] Step 4: Preparation of MOF-quantum dot light-converting adhesive film
[0064] Take 10g MOF-quantum dot masterbatch particles, 900g EVA particles, 30g crosslinker 1,1-di-tert-butyl peroxide-3,3,5-trimethylcyclohexane, 20g auxiliary crosslinker trimethylolpropane trimethacrylate, 20g silane coupling agent γ-(methacryloyloxy)propyltrimethoxysilane, 10g antioxidant tetra[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester, 10g light stabilizer poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate, mix them evenly, pour them into an extruder, heat them to 140°C, inject the molten raw materials into a mold, and finally obtain a UiO66-CdSe light-converting film with a film thickness of 0.3mm after being cast.
[0065] Example 4: Preparation of PCN224-CdZnSe / CdZnS light-converting adhesive film
[0066] Step 1: Surface modification of quantum dots
[0067] A 100 mg / ml CdZnSe / CdZnS quantum dot hexane solution (1 ml) was repeatedly precipitated-dispersed-precipitated twice with chloroform-acetone-chloroform, and finally dispersed with mercaptoalkanoic acid. The resulting dispersed solution was heated to 80°C and stirred to allow the quantum dots to fully exchange ligands with oleylamine. After the upper layer liquid was clarified, it was cooled to room temperature, and excess chloroform was added to precipitate the quantum dots. Mercaptoalkanoic acid (1 ml) was used to disperse again to obtain a 100 mg / ml CdZnSe / CdZnS mercaptoalkanoic acid solution.
[0068] Step 2: Synthesis of MOF-quantum dot nanomaterials
[0069] Dissolve ZrCl4 (120 mg) and 50 mg H2TCPP (50 mg) in DMF solution (6 ml) and ultrasonically vibrate for 20 min until completely dissolved. Dissolve benzoic acid (1200 mg) in DMF solution (2 ml) and ultrasonically vibrate for 10 min until the solution is clear. Mix the above two solutions and ultrasonically treat until uniform. Then, pour the liquid into a glass bottle and place it in a 120°C oven for reaction for 24 h, cool to room temperature, wash three times with DMF / ethanol, and dry under reduced pressure to obtain PCN-224.
[0070] The CdZnSe / CdZnS mercaptoalkanoic acid solution (40μl) obtained in step 1 was dissolved in a DMF solution (2ml) and diluted to obtain a CdZnSe / CdZnS / DMF solution. PCN-224 powder (50mg) was dissolved in a DMF solution (10ml), and ultrasonically vibrated for 30min until completely dissolved to obtain a PCN-224 / DMF solution. The CdZnSe / CdZnS / DMF solution was added dropwise to the PCN-224 / DMF solution at a rate of 1.0mL / h. After the addition was completed, it was stirred at room temperature for 20min. Subsequently, the suspension was transferred to a high-pressure reactor equipped with a polytetrafluoroethylene liner at 120°C for 12h, cooled to room temperature, washed three times with DMF / ethanol, and dried under reduced pressure to obtain a PCN224-CdZnSe / CdZnS composite nanomaterial.
[0071] Step 3: Preparation of MOF-quantum dot masterbatch particles
[0072] Take 10g PCN224-CdZnSe / CdZnS composite nanomaterial and 90g EVA particles, mix them evenly, and add them into a twin-screw extruder granulator. The temperatures of the feed section, extrusion section and discharge section of the granulator are set to 110°C, 115°C and 120°C, respectively. After melting, extrusion, wire drawing and pelletizing, MOF-quantum dot masterbatch particles with a particle size of 2mm are finally obtained.
[0073] Step 4: Preparation of MOF-quantum dot light-converting adhesive film
[0074] 100gMOF-quantum dot masterbatch particles, 950gEVA particles, 5g crosslinking agent tert-butyl peroxy-2-ethylhexyl carbonate, 4g auxiliary crosslinking agent trimethylolpropane triacrylate, 1g silane coupling agent vinyl tri(β-methoxyethoxy)silane, 0.5g antioxidant 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 0.5g light stabilizer sebacate bis(1,2,2,6,6-pentamethylpiperidinol) ester were mixed evenly, poured into an extruder, heated to 140°C, and the molten raw materials were injected into a mold. After being cast, a PCN224-CdZnSe / CdZnS light-converting film with a film thickness of 0.4mm was finally obtained.
[0075] Example 5: Preparation of ZIF67-CsPbBr3 light-converting adhesive film
[0076] Step 1: Surface modification of quantum dots
[0077] A 100 mg / ml CsPbBr3 quantum dot hexane solution (1 ml) was repeatedly precipitated-dispersed-precipitated twice with chloroform-acetone-chloroform, and finally dispersed with polyethylene glycol. The resulting dispersed solution was heated to 80°C and stirred to allow the quantum dots and polyethylene glycol to fully exchange ligands. After the upper layer liquid was clarified, it was cooled to room temperature, and excess chloroform was added to precipitate the quantum dots. Polyethylene glycol (1 ml) was used for dispersion again to obtain a 100 mg / ml CsPbBr3 polyethylene glycol solution.
[0078] Step 2: Synthesis of MOF-quantum dot nanomaterials
[0079] Dissolve the CsPbBr3 polyethylene glycol solution (10μl) obtained in step 1 in DMF solution (7ml), and ultrasonically vibrate for 20min to obtain CsPbBr3 / DMF solution. Add cobalt acetylacetonate (10mg) and 2-methylimidazole (40mg) to DMF solution (10ml), ultrasonically vibrate for 30min, and fully dissolve until the solution is clear. Then, add cobalt acetylacetonate / 2-methylimidazole / DMF solution dropwise to CsPbBr3 / DMF solution at a rate of 1.0mL / h, and stir at room temperature for 1h. After the reaction is completed, wash twice with ethyl acetate, collect the product by centrifugation, and dry under reduced pressure to obtain ZIF67-CsPbBr3 composite nanomaterials.
[0080] Step 3: Preparation of MOF-quantum dot masterbatch particles
[0081] Take 5g ZIF67-CsPbBr3 composite nanomaterial and 95g EVA particles, mix them evenly, and add them into a twin-screw extruder granulator. The temperatures of the feed section, extrusion section and discharge section of the granulator are set to 70℃, 75℃ and 80℃ respectively. After melting, extrusion, wire drawing and pelletizing, MOF-quantum dot masterbatch particles with a particle size of 3mm are finally obtained.
[0082] Step 4: Preparation of MOF-quantum dot light-converting adhesive film
[0083] Take 50gMOF-quantum dot masterbatch particles, 930gEVA particles, 10g cross-linking agent 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 10g auxiliary cross-linking agent ethoxymethylpropane triacrylate, 10g silane coupling agent vinyl triethoxysilane, 5g antioxidant bis(2.4-di-tert-butylphenyl)pentaerythritol diphosphite, 5g light stabilizer poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol) succinate, mix them evenly, pour them into an extruder, heat them to 120°C, inject the molten raw materials into the mold, and finally obtain a ZIF67-CsPbBr3 light-converting film with a film thickness of 0.3mm after being cast.
[0084] Example 6: Preparation of MIL101(Fe)-InP light conversion adhesive film
[0085] Step 1: Surface modification of quantum dots
[0086] The InP quantum dot solution (1 ml) with a concentration of 100 mg / ml was repeatedly precipitated-dispersed-precipitated twice with chloroform-acetone-chloroform, and finally dispersed with mercaptopropionic acid. The resulting dispersed solution was heated to 80°C and stirred to allow the quantum dots and mercaptopropionic acid to fully exchange ligands. After the upper layer liquid was clarified, it was cooled to room temperature, and excess chloroform was added to precipitate the quantum dots. Mercaptopropionic acid (1 ml) was used to disperse again to obtain an InP mercaptopropionic acid solution with a concentration of 100 mg / ml.
[0087] Step 2: Synthesis of MOF-quantum dot nanomaterials
[0088] The InP mercaptopropionic acid solution (20 μl) obtained in step 1 was dissolved in a DMF solution (2 ml) and diluted to obtain an InP / DMF solution. FeCl3·6H2O (2.45 mmol) and benzoic acid (1.24 mmol) were added to a DMF solution (15 ml) and stirred until completely dissolved. The InP / DMF solution was added dropwise to the above liquid at a rate of 1.0 mL / h, and continued to stir until completely dispersed. The liquid was then transferred to a high-pressure reactor equipped with a polytetrafluoroethylene liner and reacted at 110°C for 20 hours. After cooling to room temperature, the product was collected by centrifugation, washed three times with DMF / ethanol, and dried to obtain an InP-MIL101 (Fe) composite nanomaterial.
[0089] Step 3: Preparation of MOF-quantum dot masterbatch particles
[0090] Take 1g InP-MIL101 (Fe) composite nanomaterial and 99g EVA particles, mix them evenly, and add them into a twin-screw extruder granulator. The temperatures of the feed section, extrusion section and discharge section of the granulator are set to 90°C, 95°C and 100°C, respectively. After melting, extrusion, wire drawing and pelletizing, MOF-quantum dot masterbatch particles with a particle size of 2mm are finally obtained.
[0091] Step 4: Preparation of MOF-quantum dot light-converting adhesive film
[0092] Take 30gMOF-quantum dot masterbatch particles, 940gEVA particles, 20g cross-linking agent peroxy-2-ethylhexyl carbonate tert-amyl ester, 30g auxiliary cross-linking agent propoxy trimethylol propane triacrylate, 12g silane coupling agent γ-glycidyloxypropyl trimethoxysilane, 8g antioxidant triphenyl phosphite, 8g light stabilizer sebacate bis (1,2,2,6,6-pentamethylpiperidinol) ester and mix them evenly, then pour them into an extruder, heat them to 150°C, inject the molten raw materials into the mold, and finally obtain a MIL101 (Fe) -InP light conversion film with a film thickness of 0.4mm after casting.
[0093] Comparative Example 1: UV cut-off film
[0094] Take 10g of ultraviolet absorber bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, 990g of EVA particles, 10g of cross-linking agent tert-butyl peroxy-2-ethylhexyl carbonate, 5g of auxiliary cross-linking agent triallyl isocyanurate, 5g of silane coupling agent vinyl trimethoxysilane, 5g of antioxidant β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl ester, and 5g of light stabilizer bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, mix them evenly, pour them into an extruder, heat them to 140°C, inject the molten raw materials into a mold, and finally obtain a UV cutoff film with a film thickness of 0.2 mm through cast molding.
[0095] Comparative Example 2: CdZnS / ZnS quantum dots / EVA film
[0096] Step 1: Take 10g of CdZnS / ZnS nanomaterial and 90g of EVA particles, mix them evenly, and add them into a twin-screw extruder granulator. The temperatures of the feed section, extrusion section and discharge section of the granulator are set to 80°C, 85°C and 90°C, respectively. After melting, extrusion, wire drawing and pelletizing, quantum dot masterbatch particles with a particle size of 3mm are finally obtained.
[0097] Step 2: Take 10g quantum dot masterbatch particles, 990g EVA particles, 10g crosslinking agent tert-butyl peroxy-2-ethylhexyl carbonate, 5g auxiliary crosslinking agent triallyl isocyanurate, 5g silane coupling agent vinyl trimethoxysilane, 5g antioxidant β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl ester, 5g light stabilizer bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, mix them evenly, pour them into the extruder, heat them to 140°C, inject the molten raw materials into the mold, and finally obtain a CdZnS / ZnS quantum dot / EVA light-converting film with a film thickness of 0.2mm after being cast.
[0098] Test Example 1
[0099] This test example examines the performance of photovoltaic modules obtained by using the light conversion adhesive films prepared in the embodiments of the present invention and the comparative examples.
[0100] Preparation method of photovoltaic modules: stack photovoltaic glass, lower light-converting adhesive film, solar cell, upper light-converting adhesive film and upper photovoltaic glass in order from bottom to top on photovoltaic glass, put into a vacuum laminator, evacuate for 10 minutes, heat to 120°C, and laminate at a pressure of 25 MPa to obtain photovoltaic modules.
[0101] Test method: The light-converting adhesive films prepared in Comparative Example 1, Comparative Example 2 and Example 1 were used as the upper light-converting adhesive film and the lower light-converting adhesive film, respectively. Three photovoltaic modules were obtained by stacking and laminating according to the above method, and the performance of the three photovoltaic modules was tested. Specifically: The transmittance test standard of the module is carried out in accordance with GB / T29848-2018. The power test standard of the photovoltaic module is carried out in accordance with IEC61215-2:2021, and the anti-PID performance test standard is carried out in accordance with IEC61215-2:2021.
[0102] The test results are shown in Table 1 below:
[0103] Table 1
[0104]
[0105] From the results in Table 1, it can be seen that the addition of CdZnS / ZnS quantum dots in Comparative Example 2 (CdZnS / ZnS quantum dots / EVA light-converting adhesive film) can absorb ultraviolet light that is harmful to the components, and the absorption of ultraviolet light can be comparable to or even higher than that of the UV cutoff film (Comparative Example 1), and the quantum dot light-converting adhesive film converts the absorbed ultraviolet light into visible light that can be photoelectrically converted by photovoltaic components, thereby increasing the initial power, and has a higher light energy utilization rate than the simple UV cutoff film (Comparative Example 1). However, since quantum dots are point light sources, only 20% of the visible light after conversion can be received and utilized by the components at most. Therefore, although the ultraviolet light absorption is high, the initial efficiency after conversion is limited. The light-converting adhesive film of Example 1 of the present invention combines quantum dots with MOFs (metal skeleton structure), and can utilize the microporous structure of the MOFs material to improve the transmittance of the outgoing light. At the same time, when the quantum dots are completely covered by the MOFs material, due to the strong light capture ability of the MOFs material, the luminous efficiency of the quantum dots can be enhanced through energy transfer. Compared with the quantum dot light conversion adhesive film (Comparative Example 2), the visible light transmittance of the light conversion adhesive film of Example 1 of the present invention and the initial power of the photovoltaic module are improved to a certain extent.
[0106] In addition, the power comparison after UV aging of the film was also investigated. It can be seen that after UV aging, the module power of Example 1 can still reach 98.9% of the initial module power, while the module power of Comparative Example 1 is 93.8% of the initial power, and the module power of Comparative Example 2 is 97.5% of the initial power. This is because the UV cut-off film has limited absorption of ultraviolet light, and the ultraviolet light that is not absorbed and reflected reduces the durability of the photovoltaic module. The quantum dot light conversion film can absorb more than 90% of ultraviolet light, and when the quantum dots are completely covered by MOFs material, thanks to the excellent light capture ability of the MOF structure and the modification and protection of the quantum dots, the absorption and stability of the quantum dots to ultraviolet light are improved, and the durability of the module is also improved.
Claims
1. A method for preparing a MOF-quantum dot down-conversion light-converting adhesive film, characterized in that: The preparation method comprises the following steps: Step 1: Surface modification of quantum dots Using a surface modifier to modify the surface of the quantum dots to obtain modified quantum dots; Step 2: Synthesis of MOF-quantum dot nanomaterials The modified quantum dots are encapsulated inside the MOF organic framework to synthesize MOF-quantum dot nanomaterials; Step 3: Preparation of MOF-quantum dot masterbatch particles The MOF-quantum dot nanomaterials are mixed with EVA particles, and then melted, extruded, and granulated to obtain MOF-quantum dot masterbatch particles; Step 4: Preparation of MOF-quantum dot light-converting adhesive film The MOF-quantum dot masterbatch particles, EVA particles, and other components are uniformly mixed and then tape-cast to obtain a MOF-quantum dot light-converting adhesive film.
2. The preparation method according to claim 1, characterized in that: In step 1, The surface modifier is one or more of pyridine, oleic acid, oleylamine, mercaptopropionic acid, mercaptoalkanoic acid, tri-n-octylphosphine oxide, polyethylene glycol, polyamide-amine, polyacrylic acid-1,2-distearoyl-sn-glycerol-3-phosphatidylethanolamine, and cucurbituril; The quantum dots are one or more of CdSe, CdS, CdZnSe, CdZnS, CdZnSeS, CdSe / ZnS, CdSe / CdZnS, CdZnS / ZnS, CdZnSeS / ZnS, CdZnSe / CdZnS, CdSe / ZnSe, ZnSe / ZnS, CdSe / CdZnS / ZnS, CsPbBr3, CsPb(Cl / Br)3, and InP.
3. The preparation method according to claim 1, characterized in that: In step 2, the MOF organic framework is one or more of IRMOF-3, MOF-5, UiO-66, PCN-333, PCN-224, ZIF-8, ZIF-67, ZIF-365, MIL-88B, MIL-101, MIL-100, and MIL-125.
4. The preparation method according to claim 1, characterized in that: In step 3, the content of MOF-quantum dot nanomaterials in the MOF-quantum dot masterbatch particles is 1%-10%.
5. The preparation method according to claim 1, characterized in that: In step 4, the other ingredients include a cross-linking agent, a co-cross-linking agent, a silane coupling agent, a light stabilizer and an antioxidant.
6. The preparation method according to claim 5, characterized in that: In step 4, the amounts of the ingredients are as follows:
7. The preparation method according to claim 6, characterized in that: The cross-linking agent is one or more of tert-butyl peroxy-2-ethylhexyl carbonate, 1,1-di-tert-butyl peroxide-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, and tert-amyl peroxy-2-ethylhexyl carbonate; The auxiliary cross-linking agent is one or more of triallyl isocyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, triallyl cyanurate, ethoxymethylpropane triacrylate, and propoxy trimethylolpropane triacrylate; The silane coupling agent is one or more of γ-(methacryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, vinyltri(β-methoxyethoxy)silane, vinyltriethoxysilane, and γ-glycidyloxypropyltrimethoxysilane; The light stabilizer is one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinylethanol) succinate, and bis(1,2,2,6,6-pentamethylpiperidinol) sebacate; The antioxidant is one or more of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-thiobis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], tris[2.4-di-tert-butylphenyl] phosphite, bis(2.4-di-tert-butylphenyl) pentaerythritol diphosphite, tris(nonylphenyl) phosphite, and triphenyl phosphite.
8. The preparation method according to claim 1, characterized in that: In step 3, the temperature of the feeding section, extrusion section and discharge section of the granulator are all 70-120°C, preferably 80-100°C.
9. The preparation method according to claim 1, characterized in that: In step 4, the temperature in the tape casting process is 120-150° C., and the thickness of the film is 0.2-0.5 mm.
10. A MOF-quantum dot down-conversion light-converting adhesive film prepared by the preparation method according to any one of claims 1 to 9.