Preparation method of single-walled carbon nano antistatic emulsion
Modified single-wall carbon nanotubes were prepared by vacuum tightly coupled induction furnace and chemical vapor deposition method, and non-covalent modification was performed, which solved the purity and electrostatic problems of carbon nanotubes, and achieved efficient anti-static, heat resistance and antibacterial effects.
Patent Information
- Application Number
- CN202411461022.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing carbon nanotubes have low purity, poor uniformity, poor solubility and dispersion, which lead to agglomeration and static problems in applications, making it difficult to meet the high antistatic needs of industries such as consumer electronics and automotive paint.
Spherical composite nanoparticles were prepared by vacuum tightly coupled induction furnace, single-wall carbon nanotubes were prepared by chemical vapor deposition, and non-covalent modification was performed by modified antistatic agents to form an antistatic emulsion, which improved conductivity, stability and durability. sex.
It improves the conductivity and stability of carbon nanotubes, enhances the anti-static effect, reduces the accumulation of static electricity, improves the heat resistance and antibacterial properties of the emulsion, and extends the service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of antistatic emulsions, in particular to a method for preparing a single-walled carbon nanometer antistatic emulsion. Background Art
[0002] Acrylic resin is a resin made by copolymerization of acrylic acid esters, methacrylic acid esters and other olefinic monomers. Different types of polyacrylic acid resins can be obtained by selecting different copolymer monomers, different formulas and production processes during preparation, so as to meet different uses and functions in actual production and life. Acrylic emulsions are widely used in the coatings market and adhesives market, such as automotive spray paint and adhesives for the electronics industry. With the progress of industrial production, the market has put forward higher requirements for the antistatic properties of acrylic resins. The existing polyacrylic acid emulsion materials can no longer meet the production needs of the current consumer electronics and automotive spray paint industries.
[0003] The excellent mechanical, electrical, optical, and thermal properties of carbon nanotubes make them a hot topic of research in many fields such as materials, batteries, electronic devices, optical devices, sensors, catalysis, and biomedicine. However, there are still some problems in the practical application of carbon nanotubes. For example, carbon nanotubes themselves have some defects. The carbon nanotubes prepared by ordinary methods are not pure and uniform. After purification, they still contain impurities such as amorphous carbon particles, metal catalyst particles, and fullerene carbon. In addition, due to the strong interaction between the molecules of carbon nanotubes themselves, their solubility and dispersibility are poor, and they are prone to agglomeration. These problems will have a certain impact on the application of carbon nanotubes. In order to solve these problems, carbon nanotubes need to be modified or modified. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a single-walled carbon nanometer antistatic emulsion to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a single-walled carbon nano antistatic emulsion, comprising the following preparation steps: (1) 21-35 parts of yttrium oxide are placed in a vacuum melting crucible with a vacuum degree of -0.08 MPa, and 32-46 parts of iron oxide are melted to obtain a molten liquid, and the crucible is placed in a furnace. When the ambient temperature reaches 650-700° C., the molten liquid is atomized and sprayed with argon gas as an atomizing medium, an atomizing pressure of 3.0-4.0 MPa, and an atomizing flow rate of 24-28 m³ / min to obtain composite nanoparticles; (2) In an argon atmosphere with a flow rate of 250-350 sccm, the composite nanoparticles are evenly spread on the surface of a quartz boat, placed in a heating zone, heated to 1000-1100°C, the argon gas is replaced with carbon monoxide gas, and after growing for 30-50 minutes, the argon gas is replaced back to argon gas, cooled to 25°C, and then taken out to obtain a crude product, which is purified to obtain single-walled carbon nanotubes; (3) Dissolve 2-6 parts of 4-chloro-1-(2-thienyl)butanone in 20-60 parts of glacial acetic acid, add 4-12 parts of N-bromosuccinimide at a rate of 1 drop / s under ice-water cooling, stir at 120 rpm in the dark for 12 hours, add 25-65 parts of 2 mol / L NaOH aqueous solution, extract and concentrate to obtain 4-chloro-1-(2-thienyl)butanone bromide; (4) Under a nitrogen atmosphere, 10-16 parts of 4-chloro-1-(2-thienyl)butanone bromide, 12-20 parts of triphenylphosphine, and 80-128 parts of N-dimethylformamide were mixed evenly, reacted at 110-130° C. and 100 rpm for 48-72 hours, cooled to 25° C., filtered to obtain a solid, washed three times with ethyl acetate, and dried in an oven at 40-50° C. for 10-16 hours to obtain a composite agent; (5) 11-17 parts of 9-bromotriptycene and 88-136 parts of tetrahydrofuran were mixed uniformly, cooled to 0°C, 1 part of a reactant was added, stirred at 80 rpm for 10-20 min, 8-14 parts of a complexing agent were added dropwise at a rate of 2 drops / s, reacted for 4-6 h, then heated to 25°C and reacted for 8-12 h to obtain a reaction solution, which was crystallized to obtain a modified antistatic agent; (6) 7 to 15 parts of a modified antistatic agent, 14 to 30 parts of single-walled carbon nanotubes, and 20 to 40 parts of dimethyl sulfoxide are mixed uniformly, and ultrasonicated at 50 kHz for 20 to 30 minutes to prepare a modified single-walled carbon nanotube solution; (7) 10-25 parts of modified single-walled carbon nanotube solution, 30-70 parts of acrylic ester slurry, 0.2-0.6 parts of defoaming agent, and 45-105 parts of deionized water are added to a homogenizing emulsifier for high-speed emulsification to prepare a single-walled carbon nanotube antistatic emulsion.
[0006] Furthermore, the iron oxide in step (1) is any one of ferrous oxide, ferric oxide and ferrosoferric oxide.
[0007] Furthermore, the flow rate of the carbon monoxide gas in step (2) is 320-380 sccm.
[0008] Furthermore, the purification step in step (2) is to place 1 portion of the crude product in a container, add 4 mol / L hydrochloric acid solution at a rate of 2 drops / s until the pH is 6-7, filter out the solid, wash it with deionized water 3 times, and dry it in an oven at 45-55°C for 8-16 hours.
[0009] Furthermore, the extraction step in step (3) is to extract with 40 to 100 parts of dichloromethane, which is repeated three times; and the concentration is to concentrate the dichloromethane phase at -0.06 MPa and 30° C. for 2 to 4 hours.
[0010] Furthermore, the reactants in step (5) include 0.8-1.4 parts of bis(1,5-cyclooctadiene)nickel, 14-20 parts of zinc powder, and 0.9-1.5 parts of 4,4-di-tert-butyl-2,2-bipyridine.
[0011] Furthermore, the crystallization step in step (5) is to add 1 part of the reaction solution into 140-210 parts of methanol and stir for 30-40 minutes, filter out the solid, wash it with methanol three times, and dry it in an oven at 40-50°C for 10-16 hours.
[0012] Furthermore, the acrylic slurry model in step (7) is DH-A03.
[0013] Furthermore, the defoaming agent in step (7) is any one of AFE-1410, DENSIPOL PA 240, and EMULTROL DFMAFO3.
[0014] Furthermore, the temperature of the high-speed emulsification in step (7) is 40° C. and the rotation speed is 2000 rpm.
[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The present invention first uses a vacuum tightly coupled induction furnace to combine iron oxide with yttrium oxide in the form of a spray to form a smooth surface spherical composite nanoparticles with a high specific surface area, which can accelerate the graphitization of carbon atoms and reduce the reaction time. At the same time, its smooth surface is not easy to adhere to the carbon nanotubes, avoiding excessive oxidation during purification, indirectly increasing the service life, and reducing the phenomenon of electrons being blocked by impurities during movement, thereby enhancing the conductivity and stability of the carbon nanotubes and improving the antistatic effect; then the composite nanoparticles are used as catalysts and a single-walled carbon nanotube is prepared by chemical vapor deposition. Tube, under the interaction between iron oxide and the edge of single-walled carbon nanotube, the reaction activation energy of the cracking process is reduced, the reaction rate is increased, the thermal decomposition of the carbon precursor in the gas phase is reduced, the purity of the carbon nanotube is improved, yttrium oxide is assisted, the influence of elemental composition on the chirality of single-walled carbon nanotube is weakened, the diameter of the nanotube is reduced, and the surface area of the carbon nanotube is increased, thereby improving the thermal conductivity and enhancing the thermal stability; finally, through the interaction between the modified antistatic agent and the single-walled carbon nanotube, it is attached to the surface of the single-walled carbon nanotube for non-covalent modification and made into an emulsion to achieve the effects of heat resistance, antistatic, antibacterial and high durability.
[0016] Among them, the modified antistatic agent is to first brominate 4-chloro-1-(2-thienyl)butanone to provide a reaction site for subsequent coupling; then the chlorinated side chain is changed into a quaternary phosphonium salt structure through triphenylphosphine, which can reduce the static electricity accumulation on the surface while achieving the antibacterial effect. On this basis, the surface tension of the emulsion is reduced, and the contact between the emulsion and other objects is more firmly, thereby improving the durability; the composite agent is then reacted and combined with 9-bromotriptycene through a catalyst, and its rigid support structure can effectively inhibit the π-π molecular stacking between adjacent molecules, reduce the stacking and complexing between molecules, and significantly improve the overall thermal stability and dispersibility. The introduction of multiple benzene rings can further enhance the overall thermal stability of the emulsion. Combined with the pyrrolidine ring and sulfur atom in thiophene, it has strong conductivity, can absorb and transfer charges in an electrostatic field, and reduce the cumulative effect of static electricity, thereby achieving an antistatic effect. DETAILED DESCRIPTION
[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0018] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the test methods of the single-walled carbon nano antistatic emulsion prepared in the following examples as follows: Take the same mass of the embodiment and the comparative example, add 1% of their mass of diacetoacetate platinum (platinum content 100 ppm), mix well, use a 5# standardized Meyer rod to coat the mixture on the surface of a 25 μm PET film, and cure it at 160°C for 1 min to obtain an antistatic film sample.
[0019] Surface resistivity: The surface resistivity of the antistatic film sample was tested using an electrostatic tester SIMCO ST-4.
[0020] Antibacterial rate: The antibacterial properties of antistatic film samples were tested using the direct contact method.
[0021] Peel force test: lightly press the standard test tape (TESA7475) on the film longitudinally. The film sample is larger than 175mm*25mm. Roll the film back and forth 3 times at 300mm / min. Fix the sample on a stainless steel plate with double-sided tape. Press a stainless steel block on the sample at 25℃ (pressure of 20g / cm 2 ) for 20 minutes. After the block is taken out, use a tensile tester or a release machine to test the peeling force at a speed of 300 mm / min. Each sample is tested in parallel 3 times, and the average of the 3 test results is taken.
[0022] 70℃ aging peel strength test: lightly press the standard test tape (TESA7475) on the film longitudinally. The film sample is larger than 175mm*25mm. Roll the film 3 times at 300mm / min. Fix the sample on the stainless steel plate with double-sided tape. Press the stainless steel block on the sample at 70℃ (pressure is 20g / cm 2 ) for 20 hours, after the block is taken out, place it at 25℃ for 4 hours, and use a tensile tester or a release machine to test the peeling force at a speed of 300mm / min. Each sample is tested in parallel 3 times, and the average of the 3 test results is taken.
[0023] Example 1: (1) 21 parts of yttrium oxide were placed in a vacuum melting crucible with a vacuum degree of -0.08 MPa, and 32 parts of ferrous oxide were melted to obtain a molten liquid. The crucible was placed in a furnace. When the ambient temperature reached 650°C, the molten liquid was atomized and sprayed with argon gas as an atomizing medium, at an atomizing pressure of 3.0 MPa and an atomizing flow rate of 24 m³ / min, to obtain composite nanoparticles. (2) In an argon atmosphere with a flow rate of 250 sccm, the composite nanoparticles are evenly spread on the surface of a quartz boat, placed in a heating zone, heated to 1000°C, and the argon gas is replaced with a carbon monoxide gas with a flow rate of 320 sccm. After growing for 30 minutes, the argon gas is replaced back to the argon gas, and the crude product is obtained after cooling to 25°C. A portion of the crude product is placed in a container, and a 4 mol / L hydrochloric acid solution is added at a rate of 2 drops / s until the pH is 6. The solid is filtered and washed with deionized water for 3 times, and dried in an oven at 45°C for 8 hours to obtain single-walled carbon nanotubes; (3) Dissolve 2 parts of 4-chloro-1-(2-thienyl)butanone in 20 parts of glacial acetic acid, add 4 parts of N-bromosuccinimide at a rate of 1 drop / s under ice-water cooling, stir at 120 rpm in the dark for 12 hours, add 25 parts of 2 mol / L NaOH aqueous solution, extract with 40 parts of dichloromethane, repeat three times, take the dichloromethane phase and concentrate at -0.06 MPa and 30°C for 2 hours to obtain 4-chloro-1-(2-thienyl)butanone bromide; (4) Under a nitrogen atmosphere, 10 parts of 4-chloro-1-(2-thienyl)butanone bromide, 12 parts of triphenylphosphine, and 80 parts of N-dimethylformamide were mixed evenly, reacted at 110° C. and 100 rpm for 48 hours, cooled to 25° C., filtered to obtain a solid, washed three times with ethyl acetate, and dried in an oven at 40° C. for 10 hours to obtain a composite agent; (5) 11 parts of 9-bromotriptycene and 88 parts of tetrahydrofuran were mixed uniformly, cooled to 0°C, 0.8 parts of bis(1,5-cyclooctadiene)nickel, 14 parts of zinc powder, and 0.9 parts of 4,4-di-tert-butyl-2,2-bipyridine were added, and stirred at 80 rpm for 10 min. 8 parts of the complexing agent were added dropwise at a rate of 2 drops / s, and the mixture was reacted for 4 h. The mixture was then heated to 25°C and reacted for 8 h to obtain a reaction solution. 1 part of the reaction solution was added to 140 parts of methanol, stirred for 30 min, and the solid was filtered out, washed with methanol 3 times, and dried in an oven at 40°C for 10 h to obtain a modified antistatic agent. (6) 7 parts of modified antistatic agent, 14 parts of single-walled carbon nanotubes, and 20 parts of dimethyl sulfoxide were mixed uniformly, and ultrasonicated at 50 kHz for 20 minutes to prepare a modified single-walled carbon nanotube solution; (7) Add 10 parts of modified single-walled carbon nanotube solution, 30 parts of DH-A03 acrylate slurry, 0.2 parts of AFE-1410 defoaming agent, and 45 parts of deionized water into a homogenizing emulsifier and emulsify at 40° C. and 2000 rpm to obtain a single-walled carbon nanotube antistatic emulsion.
[0024] Example 2: (1) 28 parts of yttrium oxide were placed in a vacuum melting crucible with a vacuum degree of -0.08 MPa, and 39 parts of iron oxide were melted to obtain a molten liquid. The crucible was placed in a furnace. When the ambient temperature reached 675°C, the molten liquid was atomized and sprayed with argon gas as an atomizing medium, an atomizing pressure of 3.5 MPa, and an atomizing flow rate of 26 m³ / min to obtain composite nanoparticles. (2) In an argon atmosphere with a flow rate of 300 sccm, the composite nanoparticles are evenly spread on the surface of a quartz boat, placed in a heating zone, and heated to 1050°C. The argon gas is replaced with a carbon monoxide gas with a flow rate of 350 sccm. After growing for 40 minutes, the argon gas is replaced back to the argon gas. After cooling to 25°C, the crude product is taken out to obtain a crude product. One portion of the crude product is placed in a container, and a 4 mol / L hydrochloric acid solution is added at a rate of 2 drops / s until the pH is 6.5. The solid is filtered and washed with deionized water three times, and dried in an oven at 50°C for 12 hours to obtain single-walled carbon nanotubes; (3) Dissolve 4 parts of 4-chloro-1-(2-thienyl)butanone in 40 parts of glacial acetic acid, add 8 parts of N-bromosuccinimide at a rate of 1 drop / s under ice-water cooling, stir at 120 rpm in the dark for 12 hours, add 45 parts of 2 mol / L NaOH aqueous solution, extract with 70 parts of dichloromethane, repeat three times, take the dichloromethane phase and concentrate at -0.06 MPa and 30°C for 3 hours to obtain 4-chloro-1-(2-thienyl)butanone bromide; (4) Under a nitrogen atmosphere, 13 parts of 4-chloro-1-(2-thienyl)butanone bromide, 16 parts of triphenylphosphine, and 104 parts of N-dimethylformamide were mixed evenly, reacted at 120° C. and 100 rpm for 60 h, cooled to 25° C., filtered to obtain a solid, washed three times with ethyl acetate, and dried in an oven at 45° C. for 13 h to obtain a composite agent; (5) 14 parts of 9-bromotriptycene and 112 parts of tetrahydrofuran were mixed uniformly, cooled to 0°C, 1.1 parts of bis(1,5-cyclooctadiene)nickel, 17 parts of zinc powder, and 1.2 parts of 4,4-di-tert-butyl-2,2-bipyridine were added, and stirred at 80 rpm for 15 min. 11 parts of the complexing agent were added dropwise at a rate of 2 drops / s, and the mixture was reacted for 5 h. The mixture was then heated to 25°C and reacted for 10 h to obtain a reaction solution. 1 part of the reaction solution was added to 175 parts of methanol, stirred for 35 min, and the solid was filtered out, washed with methanol 3 times, and dried in an oven at 40-50°C for 13 h to obtain a modified antistatic agent. (6) 11 parts of modified antistatic agent, 22 parts of single-walled carbon nanotubes, and 30 parts of dimethyl sulfoxide were mixed evenly, and ultrasonicated at 50 kHz for 25 minutes to prepare a modified single-walled carbon nanotube solution; (7) 17.5 parts of modified single-walled carbon nanotube solution, 50 parts of DH-A03 acrylate slurry, 0.4 parts of DENSIPOLPA 240 defoaming agent, and 75 parts of deionized water were added into a homogenizing emulsifier and emulsified at 40° C. and 2000 rpm to obtain a single-walled carbon nanotube antistatic emulsion.
[0025] Example 3: (1) 35 parts of yttrium oxide were placed in a vacuum melting crucible with a vacuum degree of -0.08 MPa, and 46 parts of ferroferric oxide were melted to obtain a molten liquid. The crucible was placed in a furnace. When the ambient temperature reached 700°C, the molten liquid was atomized and sprayed with argon gas as an atomizing medium, an atomizing pressure of 4.0 MPa, and an atomizing flow rate of 28 m³ / min to obtain composite nanoparticles. (2) In an argon atmosphere with a flow rate of 350 sccm, the composite nanoparticles were evenly spread on the surface of a quartz boat, placed in a heating zone, heated to 1100°C, and the argon was replaced with a carbon monoxide gas with a flow rate of 380 sccm. After growing for 50 minutes, the argon was replaced back to the argon gas, and the crude product was obtained after cooling to 25°C. A portion of the crude product was placed in a container, and a 4 mol / L hydrochloric acid solution was added at a rate of 2 drops / s until the pH was 7. The solid was filtered and washed with deionized water for 3 times, and dried in an oven at 55°C for 16 hours to obtain single-walled carbon nanotubes; (3) 6 parts of 4-chloro-1-(2-thienyl)butanone were dissolved in 60 parts of glacial acetic acid, and 12 parts of N-bromosuccinimide were added at a rate of 1 drop / s under ice-water cooling, and stirred at 120 rpm in the dark for 12 hours, and 65 parts of 2 mol / L NaOH aqueous solution were added, and extracted with 100 parts of dichloromethane, and the mixture was repeated three times. The dichloromethane phase was concentrated at -0.06 MPa and 30° C. for 4 hours to obtain 4-chloro-1-(2-thienyl)butanone bromide; (4) Under a nitrogen atmosphere, 16 parts of 4-chloro-1-(2-thienyl)butanone bromide, 20 parts of triphenylphosphine, and 128 parts of N-dimethylformamide were mixed evenly, reacted at 130° C. and 100 rpm for 72 h, cooled to 25° C., filtered to obtain a solid, washed three times with ethyl acetate, and dried in an oven at 50° C. for 16 h to obtain a composite agent; (5) 17 parts of 9-bromotriptycene and 136 parts of tetrahydrofuran were mixed evenly, cooled to 0°C, 1.4 parts of bis(1,5-cyclooctadiene)nickel, 20 parts of zinc powder, and 1.5 parts of 4,4-di-tert-butyl-2,2-bipyridine were added, and stirred at 80 rpm for 20 min. 14 parts of the complexing agent were added dropwise at a rate of 2 drops / s, and the mixture was reacted for 6 h. The mixture was then heated to 25°C and reacted for 12 h to obtain a reaction solution. 1 part of the reaction solution was added to 210 parts of methanol, stirred for 40 min, and the solid was filtered out, washed with methanol 3 times, and dried in an oven at 50°C for 16 h to obtain a modified antistatic agent. (6) 15 parts of modified antistatic agent, 30 parts of single-walled carbon nanotubes, and 40 parts of dimethyl sulfoxide were mixed evenly, and ultrasonicated at 50 kHz for 30 minutes to prepare a modified single-walled carbon nanotube solution; (7) 25 parts of modified single-walled carbon nanotube solution, 70 parts of DH-A03 acrylic ester slurry, 0.6 parts of EMULTROLDFM AFO3 defoaming agent, and 105 parts of deionized water were added to a homogenizing emulsifier and emulsified at 40° C. and 2000 rpm to obtain a single-walled carbon nanotube antistatic emulsion.
[0026] Comparative Example 1: The difference between Comparative Example 1 and Example 2 is that there is no step (1), and step (2) is changed to: in an argon atmosphere with a flow rate of 300 sccm, yttrium oxide is evenly spread on the surface of a quartz boat, placed in a heating zone, heated to 1050°C, argon is replaced with carbon monoxide gas with a flow rate of 350 sccm, and after growing for 40 minutes, argon is replaced again, and the argon is cooled to 25°C and then taken out to obtain a crude product, 1 portion of the crude product is placed in a container, 4 mol / L hydrochloric acid solution is added dropwise at a rate of 2 drops / s until the pH is 6.5, the solid is filtered out, washed with deionized water 3 times, and dried in an oven at 50°C for 12 hours to obtain single-walled carbon nanotubes. The remaining steps are the same as in Example 2.
[0027] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that step (1) is omitted, and step (2) is changed to: in an argon atmosphere with a flow rate of 300 sccm, iron oxide is evenly spread on the surface of a quartz boat, placed in a heating zone, heated to 1050°C, argon is replaced with carbon monoxide gas with a flow rate of 350 sccm, and after growing for 40 minutes, argon is replaced again, cooled to 25°C and taken out to obtain a crude product, 1 portion of the crude product is placed in a container, 4 mol / L hydrochloric acid solution is added dropwise at a rate of 2 drops / s until the pH is 6.5, solids are filtered out, washed with deionized water 3 times, and dried in an oven at 50°C for 12 hours to obtain single-walled carbon nanotubes. The remaining steps are the same as those in Example 2.
[0028] Comparative Example 3: The difference between Comparative Example 3 and Example 2 is that step (1) is different. Step (1) is changed to: 28 parts of yttrium oxide and 39 parts of iron oxide are melted in an ultra-high temperature sintering furnace at 2500°C to obtain a molten liquid, and the molten liquid is atomized and sprayed with argon gas as an atomizing medium, at an atomizing pressure of 3.5 MPa and an atomizing flow rate of 26 m³ / min to obtain composite nanoparticles. The remaining steps are the same as those in Example 2.
[0029] Comparative Example 4: The difference between Comparative Example 4 and Example 2 is that there is no step (4), and step (5) is changed to: 14 parts of 9-bromotriptycene and 112 parts of tetrahydrofuran are mixed uniformly, cooled to 0°C, 1.1 parts of bis(1,5-cyclooctadiene)nickel, 17 parts of zinc powder, and 1.2 parts of 4,4-di-tert-butyl-2,2-bipyridine are added, stirred at 80 rpm for 15 min, 11 parts of 4-chloro-1-(2-thienyl)butanone bromide are added dropwise at a rate of 2 drops / s, reacted for 5 h, then heated to 25°C and reacted for 10 h to obtain a reaction solution, 1 part of the reaction solution is added to 175 parts of methanol, stirred for 35 min, the solid is filtered, washed with methanol 3 times, and dried in an oven at 40-50°C for 13 h to obtain a modified antistatic agent. The remaining steps are the same as those in Example 2.
[0030] Comparative Example 5: The difference between Comparative Example 5 and Example 2 is that there is no step (5), and step (6) is changed to: 11 parts of the modified composite agent, 22 parts of single-walled carbon nanotubes, and 30 parts of dimethyl sulfoxide are mixed uniformly, and ultrasonicated at 50 kHz for 25 minutes to obtain a modified single-walled carbon nanotube solution. The remaining steps are the same as in Example 2.
[0031] Effect example Table 1 below shows the performance analysis results of the single-walled carbon nano antistatic emulsions of Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.
[0032] Table 1
[0033] From the comparison of the experimental data of Examples 1, 2, and 3 with those of Comparative Example 1, it can be found that the interaction between iron oxide and the edge of single-walled carbon nanotubes can reduce the activation energy of the cracking process reaction, increase the reaction rate, reduce the thermal decomposition of the carbon precursor in the gas phase, increase the purity of carbon nanotubes, enhance the conductivity, and improve the antistatic effect; from the comparison of the experimental data of Examples 1, 2, and 3 with those of Comparative Example 2, it can be found that yttrium oxide can weaken the influence of elemental composition on the chirality of single-walled carbon nanotubes, reduce the diameter of nanotubes, increase the surface area of carbon nanotubes, improve the thermal conductivity, and enhance the thermal stability; from the comparison of the experimental data of Examples 1, 2, and 3 with those of Comparative Example 3, it can be found that the composite nanoparticles prepared by a vacuum tightly coupled induction furnace are spherical particles with smooth surfaces and have a high specific surface area, which can accelerate the graphitization of carbon atoms and reduce the reaction time. At the same time, its smooth surface is not easy to adhere to the carbon nanotubes, avoiding excessive oxidation during purification, indirectly increasing the service life, and can reduce electron The phenomenon of being blocked by impurities during movement can be avoided, thereby enhancing the conductivity and stability of the carbon nanotubes and improving the antistatic effect; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 4, it can be found that by changing the chlorinated side chain of the carbon nanotubes into a quaternary phosphonium salt structure through triphenylphosphine, while achieving the antibacterial effect, the static electricity accumulation on the surface can be reduced. On this basis, the surface tension of the emulsion is reduced, the contact between the emulsion and other objects is made more firm, and the durability is improved; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 5, it can be found that the composite agent is combined with 9-bromotriptycene, and its rigid support structure can effectively inhibit the π-π molecular stacking between adjacent molecules, reduce the intermolecular stacking and complexation, and significantly improve the overall thermal stability and dispersibility, and the introduction of polyphenyl rings can further enhance the overall thermal stability of the emulsion, cooperate with the pyrrolidine ring and sulfur atom in thiophene, have strong conductivity, can absorb and transfer charges in an electrostatic field, reduce the cumulative effect of static electricity, and thus achieve an antistatic effect.
[0034] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a single-walled carbon nanotube antistatic emulsion, characterized in that: The method comprises the following preparation steps: (1) 21-35 parts of yttrium oxide are placed in a vacuum melting crucible with a vacuum degree of -0.08 MPa, and 32-46 parts of iron oxide are melted to obtain a molten liquid, and the crucible is placed in a furnace. When the ambient temperature reaches 650-700° C., the molten liquid is atomized and sprayed with argon gas as an atomizing medium, an atomizing pressure of 3.0-4.0 MPa, and an atomizing flow rate of 24-28 m³ / min to obtain composite nanoparticles; (2) In an argon atmosphere with a flow rate of 250-350 sccm, the composite nanoparticles are evenly spread on the surface of a quartz boat, placed in a heating zone, heated to 1000-1100°C, the argon gas is replaced with carbon monoxide gas, and after growing for 30-50 minutes, the argon gas is replaced back to argon gas, cooled to 25°C, and then taken out to obtain a crude product, which is purified to obtain single-walled carbon nanotubes; (3) Dissolve 2-6 parts of 4-chloro-1-(2-thienyl)butanone in 20-60 parts of glacial acetic acid, add 4-12 parts of N-bromosuccinimide at a rate of 1 drop / s under ice-water cooling, stir at 120 rpm in the dark for 12 hours, add 25-65 parts of 2 mol / L NaOH aqueous solution, extract and concentrate to obtain 4-chloro-1-(2-thienyl)butanone bromide; (4) Under a nitrogen atmosphere, 10-16 parts of 4-chloro-1-(2-thienyl)butanone bromide, 12-20 parts of triphenylphosphine, and 80-128 parts of N-dimethylformamide were mixed evenly, reacted at 110-130° C. and 100 rpm for 48-72 hours, cooled to 25° C., filtered to obtain a solid, washed three times with ethyl acetate, and dried in an oven at 40-50° C. for 10-16 hours to obtain a composite agent; (5) 11-17 parts of 9-bromotriptycene and 88-136 parts of tetrahydrofuran were mixed uniformly, cooled to 0°C, 1 part of a reactant was added, stirred at 80 rpm for 10-20 min, 8-14 parts of a complexing agent were added dropwise at a rate of 2 drops / s, reacted for 4-6 h, then heated to 25°C and reacted for 8-12 h to obtain a reaction solution, which was crystallized to obtain a modified antistatic agent; (6) 7 to 15 parts of a modified antistatic agent, 14 to 30 parts of single-walled carbon nanotubes, and 20 to 40 parts of dimethyl sulfoxide are mixed uniformly, and ultrasonicated at 50 kHz for 20 to 30 minutes to prepare a modified single-walled carbon nanotube solution; (7) 10-25 parts of modified single-walled carbon nanotube solution, 30-70 parts of acrylic ester slurry, 0.2-0.6 parts of defoaming agent, and 45-105 parts of deionized water are added to a homogenizing emulsifier for high-speed emulsification to prepare a single-walled carbon nanotube antistatic emulsion.
2. The method for preparing a single-walled carbon nanometer antistatic emulsion according to claim 1, characterized in that: The iron oxide in step (1) is any one of ferrous oxide, ferric oxide and ferroferric oxide.
3. The method for preparing a single-walled carbon nanometer antistatic emulsion according to claim 1, characterized in that: The flow rate of the carbon monoxide gas in step (2) is 320-380 sccm.
4. The method for preparing a single-walled carbon nanometer antistatic emulsion according to claim 1, characterized in that: The purification step in step (2) is to place 1 portion of the crude product in a container, add 4 mol / L hydrochloric acid solution at a rate of 2 drops / s until the pH is 6-7, filter out the solid, wash it with deionized water 3 times, and dry it in an oven at 45-55°C for 8-16 hours.
5. The method for preparing a single-walled carbon nano antistatic emulsion according to claim 1, characterized in that: The extraction step in step (3) is to extract with 40 to 100 parts of dichloromethane, which is repeated three times; the concentration step is to concentrate the dichloromethane phase at -0.06 MPa and 30° C. for 2 to 4 hours.
6. The method for preparing a single-walled carbon nano antistatic emulsion according to claim 1, characterized in that: The reactants in step (5) include 0.8-1.4 parts of bis(1,5-cyclooctadiene)nickel, 14-20 parts of zinc powder, and 0.9-1.5 parts of 4,4-di-tert-butyl-2,2-bipyridine.
7. The method for preparing a single-walled carbon nano antistatic emulsion according to claim 1, characterized in that: The crystallization step in step (5) is to add 1 part of the reaction solution into 140-210 parts of methanol and stir for 30-40 minutes, filter out the solid, wash it with methanol three times, and dry it in an oven at 40-50°C for 10-16 hours.
8. The method for preparing a single-walled carbon nanometer antistatic emulsion according to claim 1, characterized in that: The acrylic slurry model in step (7) is DH-A03.
9. The method for preparing a single-walled carbon nano antistatic emulsion according to claim 1, characterized in that: The defoaming agent in step (7) is any one of AFE-1410, DENSIPOL PA 240, and EMULTROL DFM AFO3.
10. The method for preparing a single-walled carbon nano antistatic emulsion according to claim 1, characterized in that: The temperature of the high-speed emulsification in step (7) is 40° C. and the rotation speed is 2000 rpm.
Citation Information
Patent Citations
Poly(glycidyl methacrylate), carbon nano-tube modified by derivative of the same and preparation method thereof
CN101058418A
Ultraviolet curing paint based on carbon nanotubes and preparation method of ultraviolet curing paint
CN106634089A
Environment-friendly carbon nanotube antistatic agent and film
CN114958062A
Preparation method of single-walled carbon nanotube modified antistatic coating
CN117586546A
Organic electron transport material, light-emitting device and display panel