Low-conductivity electric vehicle cooling liquid composition and preparation method thereof

By using low-conductivity electric vehicle coolant compositions in new energy vehicles, the problem of high conductivity of traditional coolant is solved, the safety and stability of the electric vehicle thermal management system is improved, and the spontaneous combustion caused by leakage is delayed time.

CN118978899APending Publication Date: 2024-11-19河北京脉科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411068626.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, there are few researches on coolants for new energy vehicles. Traditional fuel vehicle coolants have high conductivity problems in new energy vehicles, which leads to insufficient safety and stability of the thermal management system, which can easily lead to electrical failures and Spontaneous combustion risk.

Method used

Provide a low-conductive electric vehicle coolant composition containing water, ethylene glycol, alcohol amine, water-based epoxy resin, silicone coupling agent and triazole and thiazole compounds, through specific formulations and preparation methods, It forms a coolant with low conductivity, used in the thermal management system of electric vehicles, with metal corrosion inhibition and insulation characteristics.

Benefits of technology

It achieves good metal corrosion inhibition and heat exchange effects in the electric vehicle thermal management system, and delays the short-circuit spontaneous combustion time during leakage, significantly reducing the stability of conductivity and pH value, and improving safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980137960000071
    Figure BDA0004980137960000071
Patent Text Reader

Abstract

The invention belongs to the technical field of cooling liquid preparation, and particularly relates to a low-conductivity electric vehicle cooling liquid composition and a preparation method thereof, and the low-conductivity electric vehicle cooling liquid composition comprises the following components by weight: 40-60 parts of water; 40 to 60 parts of ethylene glycol; 2 to 8 parts of alcohol amine; 0.05 to 0.2 part of water-based epoxy resin; 0.05 to 0.2 part of carboxylic acid; 0.05 to 0.2 part of a siloxane coupling agent; and 0.05 to 0.2 part of a triazole and thiazole compound. Epoxy resin is adopted as a main corrosion inhibitor, a siloxane coupling agent is adopted as a resin polymerization inhibitor, organic carboxylic acid, amine, triazole and thiazole compounds are adopted as metal corrosion inhibitors, water and dihydric alcohol are adopted as base liquid, water-based epoxy resin is adopted as a corrosion inhibitor, and the formula design is reasonable; the product can be used for an electric vehicle battery pack, a resin protection film is formed on the inner surface of an electric vehicle thermal management system without difference, and the influence of various kinds of corrosion on a cooling channel of the thermal management system is physically isolated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coolant preparation, and specifically relates to a low-conductivity electric vehicle coolant composition and a preparation method thereof. Background Art

[0002] As a strategic emerging industry, new energy vehicles represent the development direction of the automobile industry and have positive significance in reducing air pollution, changing the energy structure, and promoting the transformation and upgrading of the transportation industry. Compared with traditional fuel vehicles, the biggest change in new energy vehicles lies in the power system.

[0003] Similar to the core component engine of traditional fuel vehicles, the ambient temperature inside the battery pack (Pack) of the battery power system of new energy vehicles has a great impact on the reliability, life and performance of the battery cell (Cell). Therefore, it is particularly important to maintain the battery pack within a certain temperature range (the optimal operating temperature range of the battery cell is 20-35°C). The temperature control technology of the battery thermal management system (BMS) is mainly achieved through cooling or heating, and liquid cooling is the first choice. Liquid cooling technology uses liquid convection heat transfer to take away the heat generated by the battery and reduce the battery temperature. The liquid heat dissipation medium has a high heat transfer coefficient, large heat capacity, and fast cooling speed. It has a significant effect on reducing the maximum temperature and improving the consistency of the battery pack temperature field. At the same time, the volume of the thermal management system is relatively small.

[0004] Electric vehicle coolant is a heat exchange medium used in the cooling system of new energy vehicles such as pure electric vehicles that use power batteries as energy storage power sources to ensure the normal operation of the vehicle thermal management system. One of the core technologies of new energy vehicles is thermal management, and coolant is an important functional product that is indispensable for achieving the temperature control target of the battery thermal management system. Electric vehicle coolant is the largest working liquid used in new energy vehicles. As an emerging product, there is relatively little research on electric vehicle-specific coolants at home and abroad. Most pure electric vehicles on the market use traditional fuel vehicle coolants, while hydrogen fuel cell vehicles use an ultra-low conductivity coolant (≤5us / cm). Although the use of fuel vehicle coolant temporarily solves the problem of the source of liquid cooling medium, it is actually a "helpless move." With the use of liquid cooling temperature control systems, the market capacity of the new energy vehicle coolant market is rapidly increasing.

[0005] The objects of electric vehicle coolant service involve high-voltage electrical components such as power batteries, motors and electronic controls. Coolant leakage or failure will lead to serious thermal runaway risks or electrical failures, so special attention is paid to the coolant conductivity safety. Summary of the invention

[0006] The purpose of the present invention is to overcome the above-mentioned problems existing in the traditional technology and provide a low-conductivity electric vehicle coolant composition and a preparation method thereof. The product can be used in the thermal management system of electric vehicle battery packs, motors and control systems to play the basic functions of metal corrosion inhibition, heat exchange, etc., and in the event of leakage, it can delay the spontaneous combustion time caused by the short circuit of the three-electric system by virtue of its low conductivity insulation characteristics, thereby playing a good passive safety role.

[0007] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0008] The present invention provides a low-conductivity electric vehicle coolant composition, comprising the following components in parts by weight:

[0009] 40-60 parts of water;

[0010] 40-60 parts of ethylene glycol;

[0011] 2 to 8 parts of alcoholamine;

[0012] 0.05-0.2 parts of water-based epoxy resin;

[0013] 0.05-0.2 parts of carboxylic acid;

[0014] 0.05-0.2 parts of siloxane coupling agent;

[0015] And 0.05 to 0.2 parts of triazole and thiazole compounds.

[0016] Furthermore, the alcoholamine is triethanolamine.

[0017] Furthermore, the water-based epoxy resin is water-based bisphenol A epoxy resin.

[0018] Furthermore, the carboxylic acid is formic acid.

[0019] Furthermore, the siloxane coupling agent is aminopropyltrimethoxysiloxane.

[0020] Furthermore, the triazole and thiazole compounds are benzotriazole and dithiothiadiazole added in a ratio of 1:2.

[0021] The present invention also provides a method for preparing a low-conductivity electric vehicle coolant composition, comprising the following steps:

[0022] Mix water and ethylene glycol, raise the temperature to 75-85°C, add water-based epoxy resin to form a dilute solution, then slowly add siloxane coupling agent and ultrasonically stir for 0.5-1.5 hours, add alcohol amine and stir for 0.5-1.5 hours, finally add carboxylic acid and triazole and thiazole compounds, stir evenly to obtain a low-conductivity electric vehicle coolant composition.

[0023] Further, the following steps are included:

[0024] Mix water and ethylene glycol, heat to 80°C, add water-based epoxy resin to make a dilute solution, then slowly add siloxane coupling agent and ultrasonically stir for 1 hour, add alcohol amine and stir for 1 hour, finally add carboxylic acid and triazole and thiazole compounds, stir evenly to obtain a low-conductivity electric vehicle coolant composition.

[0025] The beneficial effects of the present invention are:

[0026] 1. The present invention provides a low-conductivity electric vehicle coolant composition, which uses epoxy resin as a main corrosion inhibitor, uses a siloxane coupling agent as a resin inhibitor, uses organic carboxylic acid, amine, triazole and thiazole compounds as metal corrosion inhibitors, uses water and diol as the base liquid, uses water-based epoxy resin as the corrosion inhibitor, and has a reasonable formula design; the product can be used in electric vehicle battery packs, and indiscriminately forms a resin protective film on the inner surface of the electric vehicle thermal management system to physically isolate the effects of various corrosions on the cooling channel of the thermal management system; it plays the basic functions of metal corrosion inhibition and heat exchange in the thermal management system of motors and control systems, and in the event of leakage, relies on its low conductivity insulation characteristics to delay the spontaneous combustion time caused by the short circuit of the three-electric system, and plays a good passive safety role.

[0027] 2. Compared with the conductivity of 3000-5000 microsieverts of the traditional water-ethylene glycol coolant, the conductivity of the low conductivity coolant of the present invention is only less than 100 microsieverts. The low conductivity coolant of the present invention has excellent multi-metal corrosion inhibition performance and good pH value and conductivity stability.

[0028] Of course, any product implementing the present invention does not necessarily need to achieve all of the above advantages at the same time. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The present invention provides a low-conductivity electric vehicle coolant composition, comprising the following components in parts by weight:

[0031] 40-60 parts of water;

[0032] 40-60 parts of ethylene glycol;

[0033] 2 to 8 parts of alcoholamine;

[0034] 0.05-0.2 parts of water-based epoxy resin;

[0035] 0.05-0.2 parts of carboxylic acid;

[0036] 0.05-0.2 parts of siloxane coupling agent;

[0037] And 0.05 to 0.2 parts of triazole and thiazole compounds.

[0038] In this embodiment, the alcoholamine is triethanolamine.

[0039] In this embodiment, the water-based epoxy resin is water-based bisphenol A epoxy resin.

[0040] In this embodiment, the carboxylic acid is formic acid.

[0041] In this embodiment, the siloxane coupling agent is aminopropyltrimethoxysiloxane.

[0042] In this embodiment, the triazole and thiazole compounds are benzotriazole and dithiothiadiazole in a ratio of 1:2.

[0043] The method for preparing the low-conductivity electric vehicle coolant composition comprises the following steps:

[0044] Mix water and ethylene glycol, heat to 80°C, add water-based epoxy resin to make a dilute solution, then slowly drop siloxane coupling agent and ultrasonically stir for 1 hour, add alcohol amine and stir for 1 hour, finally add carboxylic acid and triazole and thiazole compounds, stir evenly to obtain a low-conductivity electric vehicle coolant composition

[0045] The relevant specific embodiments of the present invention are as follows:

[0046] Example 1

[0047] A low-conductivity electric vehicle coolant composition comprises the following components in parts by weight: 40 parts of water;

[0048] 60 parts of ethylene glycol;

[0049] 2 parts of ethanolamine;

[0050] 0.2 parts of water-based epoxy resin;

[0051] 0.05 parts of carboxylic acid;

[0052] 0.2 parts of siloxane coupling agent;

[0053] and 0.05 parts of triazole and thiazole compounds.

[0054] Example 2

[0055] A low-conductivity electric vehicle coolant composition comprises the following components in parts by weight: 45 parts of water;

[0056] 55 parts of ethylene glycol;

[0057] 4 parts of ethanolamine;

[0058] 0.15 parts of water-based epoxy resin;

[0059] 0.07 parts of carboxylic acid;

[0060] 0.15 parts of siloxane coupling agent;

[0061] and 0.07 parts of triazole and thiazole compounds.

[0062] Example 3

[0063] A low-conductivity electric vehicle coolant composition comprises the following components in parts by weight: 50 parts of water;

[0064] 50 parts of ethylene glycol;

[0065] 5 parts of ethanolamine;

[0066] 0.1 parts of water-based epoxy resin;

[0067] 0.1 parts of carboxylic acid;

[0068] 0.1 parts of siloxane coupling agent;

[0069] And 0.1 parts of triazole and thiazole compounds.

[0070] Example 4

[0071] A low-conductivity electric vehicle coolant composition comprises the following components in parts by weight:

[0072] 55 parts water;

[0073] 45 parts of ethylene glycol;

[0074] 6 parts of ethanolamine;

[0075] 0.07 parts of water-based epoxy resin;

[0076] 0.15 parts of carboxylic acid;

[0077] 0.06 parts of siloxane coupling agent;

[0078] and 0.15 parts of triazole and thiazole compounds.

[0079] Example 5

[0080] A low-conductivity electric vehicle coolant composition comprises the following components in parts by weight:

[0081] 60 parts water;

[0082] 40 parts of ethylene glycol;

[0083] 8 parts of ethanolamine;

[0084] 0.05 parts of water-based epoxy resin;

[0085] 0.2 parts of carboxylic acid;

[0086] 0.05 parts of siloxane coupling agent;

[0087] And 0.2 parts of triazole and thiazole compounds.

[0088] The corrosion inhibition performance, pH value and conductivity stability of the product in Example 2, BASF G22E+ and Uni-President NE100 were tested using a glassware static corrosion tester. The results are shown in Table 1:

[0089] Table 1

[0090]

[0091] The results in Table 1 show that the low-conductivity coolant of the present invention has a good corrosion inhibition effect on materials such as copper, brass, steel, ZL101A cast aluminum, 3003 aluminum, 4043 aluminum, and 6063 aluminum compared with competing products, and the pH value and conductivity stability have a more significant performance improvement compared with competing products on the market.

[0092] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A low-conductivity electric vehicle coolant composition, characterized in that: Contains the following components in parts by weight: 40-60 parts of water; 40-60 parts of ethylene glycol; 2 to 8 parts of alcoholamine; 0.05-0.2 parts of water-based epoxy resin; 0.05-0.2 parts of carboxylic acid; 0.05-0.2 parts of siloxane coupling agent; And 0.05 to 0.2 parts of triazole and thiazole compounds.

2. The low-conductivity electric vehicle coolant composition according to claim 1, characterized in that: The alcoholamine is triethanolamine.

3. The low-conductivity electric vehicle coolant composition according to claim 1, characterized in that: The water-based epoxy resin is water-based bisphenol A epoxy resin.

4. The low-conductivity electric vehicle coolant composition according to claim 1, characterized in that: The carboxylic acid is formic acid.

5. The low-conductivity electric vehicle coolant composition according to claim 1, characterized in that: The siloxane coupling agent is aminopropyltrimethoxysiloxane.

6. The low-conductivity electric vehicle coolant composition according to claim 1, characterized in that: The triazole and thiazole compounds are benzotriazole and dithiothiadiazole added in a ratio of 1:

2.

7. The method for preparing the low-conductivity electric vehicle coolant composition according to any one of claims 1 to 6, characterized in that: The following steps are involved: Mix water and ethylene glycol, raise the temperature to 75-85°C, add water-based epoxy resin to form a dilute solution, then slowly add siloxane coupling agent and ultrasonically stir for 0.5-1.5 hours, add alcohol amine and stir for 0.5-1.5 hours, finally add carboxylic acid and triazole and thiazole compounds, stir evenly to obtain a low-conductivity electric vehicle coolant composition.

8. The preparation method according to claim 7, characterized in that: The following steps are involved: Mix water and ethylene glycol, heat to 80°C, add water-based epoxy resin to make a dilute solution, then slowly add siloxane coupling agent and ultrasonically stir for 1 hour, add alcohol amine and stir for 1 hour, finally add carboxylic acid and triazole and thiazole compounds, stir evenly to obtain a low-conductivity electric vehicle coolant composition.