Polyacid-based CO2-flooding oil reservoir heterogeneous supramolecular inclusion synergistic system as well as preparation method and application of polyacid-based CO2-flooding oil reservoir heterogeneous supramolecular inclusion synergistic system
By using a heterogeneous supramolecular inclusion and efficiency enhancement system of polyacid during CO2 oil displacement, the gas trapping problem is solved, efficient sealing of gas trapping channels and improving oil displacement efficiency, and providing low-cost CO2 trapping sealing Technique.
Patent Information
- Application Number
- CN202410935688.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Air traversal problems are prone to occur during CO2 oil flooding, resulting in a reduction in oil flooding efficiency. The prior art air traversal prevention and control methods are costly or low in efficiency, and are difficult to exist in the formation for a long time.
Using a heterogeneous supramolecular inclusion and efficiency system based on polyacid-based CO2 oil reservoirs, the inclusion of acid-resistant hydrophobic polymer microspheres and acid-resistant cyclodextrin polymers is combined with polyacid to form a supramolecular network, which improves the Viscosity and seal the air duct.
Effectively seal the air trajectory, improve the CO2 oil displacement effect, reduce the problems of poor injection and poor sealing effect, and provide low-cost CO2 air displacement technology, which improves the recovery rate of CO2 oil displacement.
Smart Images

Figure BDA0004941252460000021 
Figure BDA0004941252460000041 
Figure BDA0004941252460000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oilfield chemistry, and in particular relates to a CO2 flooding reservoir heterogeneous supramolecular inclusion synergistic system based on polyacids, and a preparation method and application thereof. Background Art
[0002] As the development stage of most medium- and high-permeability oil fields in my country has reached the middle and late stages, the recoverable reserves of medium- and high-permeability oil fields have dropped sharply year by year. The necessity of improving the recovery rate of crude oil in low-permeability oil reservoirs has become increasingly prominent. The exploration, development and utilization of low-permeability oil reservoirs are of great significance to ensure the sustainable development of oil and gas in my country. The commonly used development method at present is water injection production. However, due to the low porosity, low permeability and strong heterogeneity of these reservoirs, the efficiency of water injection development is generally low. Gas drive technology has become the main technology for the development of such oil reservoirs with a growing trend and significant results year by year.
[0003] CO2 gas has stable chemical properties. It does not burn and does not support combustion. It is a low-density, non-viscous, and highly fluid fluid. Its injection capacity is significantly higher than that of water injection, and its seepage resistance is small. It is easier to establish an effective displacement system than water injection. CO2 can undergo a series of physical and chemical reactions with underground fluids, resulting in phenomena such as crude oil volume expansion, reduced crude oil viscosity, and increased water viscosity. Under certain conditions, CO2 can be miscible with crude oil, greatly reducing interfacial tension, thereby improving the efficiency of oil displacement. During the oil displacement process, part of CO2 is stored in the reservoir, which can achieve CO2 burial. CO2 flooding can not only significantly improve crude oil recovery, but also solve geological storage problems, protect the atmospheric environment, and inhibit the greenhouse effect. It has broad application prospects. However, the heterogeneity of the reservoir, fracture characteristics, and CO2 fluid characteristics determine that gas channeling is prone to occur during CO2 gas injection development. Once gas channeling occurs, the swept volume of the gas will drop significantly, the oil displacement efficiency will be significantly reduced, and the effect of gas injection development will be seriously affected.
[0004] In order to solve the gas channeling problem in the CO2 flooding process, domestic and foreign experts and scholars have also proposed a variety of solutions: CO2 self-viscosity enhancement, foam plugging, gel plugging, etc. Although these methods have played a certain role, there are also problems. CO2 viscosity enhancement is costly and has low benefits. Although foam has good injection capacity, it has poor stability and is difficult to exist in the formation for a long time. The gel has high viscosity, poor injection capacity, and the gelation time is uncontrollable. Therefore, for CO2 gas injection development, it is urgent to develop new gas channeling prevention and control technologies to overcome the defects of existing technologies, which is of great significance for preventing and plugging gas channeling and improving gas injection effects. Summary of the invention
[0005] In view of the deficiencies of the prior art, the present invention provides a polyacid-based CO2 flooding reservoir heterogeneous supramolecular inclusion enhancement system and its preparation method and application. The supramolecular inclusion enhancement system of the present invention is composed of acid-resistant hydrophobic polymer microspheres, acid-resistant cyclodextrin polymers and polyacids. The hydrophobic cavity structure in the acid-resistant cyclodextrin polymer molecular chain can efficiently identify the hydrophobic groups on the surface of the acid-resistant hydrophobic polymer microspheres, and the acid-resistant hydrophobic polymer microspheres are included through the host-guest inclusion action to form a new aggregate structure, and then a certain mass of polyacid is added thereto to construct a supramolecular network through electrostatic interaction to form a supramolecular inclusion enhancement system. The system has shear recovery. When injected, the supramolecular effect is destroyed under high shear conditions, and the viscosity of the system is reduced to improve the injectability; when injected into the underground, the in-situ viscosity increase of the formation after shearing is achieved through self-assembly, and the gas channel is effectively blocked, which is of great significance for improving the CO2 flooding effect.
[0006] The technical solution of the present invention is as follows:
[0007] A polyacid-based CO2 flooding reservoir heterogeneous supramolecular inclusion synergistic system is prepared by including the following components in parts by weight: 1-10 parts of acid-resistant hydrophobic polymer microspheres, 1-5 parts of acid-resistant cyclodextrin polymers, 1-5 parts of polyacids, and 80-120 parts of water.
[0008] Preferably according to the present invention, a polyacid-based heterogeneous supramolecular inclusion enhancement system for CO2 flooding reservoirs is prepared by including the following components in parts by weight: 3-5 parts of acid-resistant hydrophobic polymer microspheres, 1-3 parts of acid-resistant cyclodextrin polymers, 2-4 parts of polyacids, and 90-110 parts of water.
[0009] Preferably, the CO2 flooding reservoir heterogeneous supramolecular inclusion enhancement system based on polyacid is prepared by including the following components in parts by weight: 4 parts of acid-resistant hydrophobic polymer microspheres, 2 parts of acid-resistant cyclodextrin polymer, 3 parts of polyacid, and 100 parts of water.
[0010] According to the present invention, the structure of the acid-resistant hydrophobic polymer microspheres is shown as follows:
[0011]
[0012] According to a preferred embodiment of the present invention, a method for preparing acid-resistant hydrophobic polymer microspheres comprises the steps of:
[0013] (1) white oil, Span80 and Tween80 are uniformly mixed to obtain an oil phase;
[0014] (2) fully dissolving acrylamide (AM), hexadecyl dimethyl allyl ammonium chloride (C16DMAAC), and dimethyl diallyl ammonium chloride (DMDAAC) in water, adjusting the pH value of the system, adding N,N-methylenebisacrylamide (MBA) and mixing evenly to obtain an aqueous phase;
[0015] (3) adding the aqueous phase dropwise to the oil phase, and then sequentially adding an aqueous solution of ammonium persulfate and an aqueous solution of sodium bisulfite, reacting, washing, drying, and grinding to obtain acid-resistant hydrophobic polymer microspheres.
[0016] Preferably, in step (1), the mass ratio of white oil, Span80 and Tween80 is 35-40:2-3:0.5-1.5, preferably 39:2.7:0.9.
[0017] Preferably, in step (2), the mass ratio of acrylamide (AM), hexadecyldimethylallylammonium chloride (C16DMAAC), dimethyldiallylammonium chloride (DMDAAC), N,N-methylenebisacrylamide (MBA) and water is 5-6:0.1-0.2:0.1-0.2:0.04-0.06:15-30, preferably 5.25:0.105:0.105:0.0546:21.
[0018] Preferably, in step (2), a sodium hydroxide aqueous solution with a mass concentration of 15%-30% is used to adjust the pH value of the system to 7.
[0019] Preferably, in step (3), the dripping rate of the aqueous phase is 1-5 drops per second, and the dripping is carried out under stirring and under the protection of a protective gas. Further preferably, the protective gas is nitrogen or argon.
[0020] Preferably, in step (3), the mass ratio of acrylamide in the aqueous phase to the mass ratio of the oil phase is 5-6:40-45.
[0021] Preferably, in step (3), the dripping rate of the aqueous ammonium persulfate solution and the aqueous sodium bisulfite solution is 1-5 drops per second, and the dripping is carried out under stirring and protective gas protection. Further preferably, the protective gas is nitrogen or argon.
[0022] Preferably, in step (3), the mass concentrations of the ammonium persulfate aqueous solution and the sodium bisulfite aqueous solution are both 0.02%-0.2%, wherein the mass ratio of ammonium persulfate to sodium bisulfite is 1:1; and the mass ratio of ammonium persulfate to acrylamide in the aqueous phase is 1:475-785.
[0023] Preferably, in step (3), the reaction temperature is 25-40°C, the reaction time is 2-6 hours, and the reaction is carried out under stirring and protective gas protection. Further preferably, the protective gas is nitrogen or argon.
[0024] Preferably according to the present invention, the particle size of the acid-resistant hydrophobic polymer microspheres is 60-320 nm.
[0025] According to the present invention, the structure of the acid-resistant cyclodextrin polymer is as follows:
[0026]
[0027] According to a preferred embodiment of the present invention, a method for preparing an acid-resistant cyclodextrin polymer comprises the steps of:
[0028] Acrylamide (AM) and 6-O-allyl-β-cyclodextrin (DPTD) are dissolved in water, and sodium persulfate and sodium bisulfite are added to fully dissolve to obtain solution A; acrylic acid (AA) and azobisisobutylamidine dihydrochloride are mixed, and the pH value is adjusted to 7-8 to obtain solution B; solution A and solution B are mixed, dimethyldiallylammonium chloride, azobisisobutyronitrile and dibenzoyl peroxide are added, mixed evenly, reacted, and then crushed, precipitated, purified, dried and granulated to obtain an acid-resistant cyclodextrin polymer.
[0029] Preferably, the mass ratio of acrylamide (AM) and 6-O-allyl-β-cyclodextrin (DPTD) is 15-30:1, preferably 18:1; the mass ratio of acrylamide and water is 1:3-8; the mass ratio of acrylamide (AM), sodium persulfate and sodium bisulfite is 3.6:0.0005-0.005:0.001-0.002, preferably 3.6:0.001:0.00151.
[0030] Preferably, the mass ratio of acrylic acid (AA), azobisisobutylamidine dihydrochloride and acrylamide is 1:0.001-0.005:3-4, preferably 1:0.002:3.6.
[0031] Preferably, a NaOH aqueous solution with a mass concentration of 15%-20% is used to adjust the pH.
[0032] Preferably, the mass ratio of dimethyldiallylammonium chloride, azobisisobutyronitrile, dibenzoyl peroxide and acrylamide is 0.1-0.3:0.001-0.005:0.0001-0.001:3-4, preferably 0.2:0.0025:0.0005:3.6.
[0033] Preferably, the reaction temperature is room temperature, the reaction time is 1-4 hours, and the reaction is carried out under static conditions and protective gas protection. Preferably, the protective gas is nitrogen or argon.
[0034] According to the present invention, preferably, the polyacid is pimelic acid, citric acid, disodium ethylenediaminetetraacetate or sodium polyacrylate.
[0035] The preparation method of the above-mentioned polyacid-based CO2 flooding reservoir heterogeneous supramolecular inclusion synergistic system comprises the steps of:
[0036] The acid-resistant hydrophobic polymer microspheres are fully dispersed in water, and subjected to expansion and aging reactions; then the acid-resistant cyclodextrin polymer is added, fully dispersed, and then subjected to aging reactions; polyacids are added, fully dispersed, and allowed to stand to obtain a polyacid-based CO2 flooding reservoir heterogeneous supramolecular inclusion enhancement system.
[0037] Preferably, according to the present invention, the acid-resistant hydrophobic polymer microspheres are added into water and stirred at room temperature at 100-300 r / min for 5-15 min to be fully dispersed.
[0038] Preferably according to the present invention, the expansion is carried out by stirring at room temperature and a rotation speed of 80-120 r / min for 3-5 hours.
[0039] According to the present invention, preferably, the aging is performed by static aging at 40-50°C for 20-30 hours.
[0040] Preferably according to the present invention, after the acid-resistant cyclodextrin polymer is added, stirring is performed at a speed of 80-120 r / min at room temperature for 2-6 hours to fully disperse.
[0041] According to the preferred embodiment of the present invention, the aging reaction after adding the acid-resistant cyclodextrin polymer is to stand and age for 40-50 hours at 40-50°C.
[0042] Preferably according to the present invention, after the polyacid is added, stirring is performed at a speed of 80-120 r / min at room temperature for 0.1-1 hour to fully disperse.
[0043] Preferably according to the present invention, the standing temperature is room temperature and the standing time is 1-3 hours.
[0044] The above-mentioned polyacid-based heterogeneous supramolecular inclusion enhancement system for CO2 flooding reservoirs is applied to plugging gas channeling channels in CO2 flooding reservoirs.
[0045] The preparation routes of the acid-resistant hydrophobic polymer microspheres and the acid-resistant cyclodextrin polymer of the present invention are as follows:
[0046] Acid-resistant hydrophobic polymer microspheres:
[0047]
[0048] Acid-resistant cyclodextrin polymer:
[0049]
[0050] The technical features and beneficial effects of the present invention are as follows:
[0051] (1) The supramolecular inclusion synergistic system provided by the present invention has good acid resistance. For traditional microspheres and polymers, under acidic conditions, the hydrolysis of the amide groups in the microspheres is weak, which is not conducive to the expansion of the microspheres; while the polymer microspheres mainly rely on water absorption to expand and aggregate to achieve plugging, but under acidic conditions, the structural density is large and the water absorption and expansion capacity is poor; at the same time, the traditional polymer is composed of a water-soluble polymer plus a cross-linking agent, and the water-soluble polymer molecular chain exposes many negatively charged anionic groups. In the acidic environment of CO2, its viscosity-enhancing effect is poor, and the viscosity of the acid-resistant polymer decreases, resulting in a poor plugging effect. The present invention introduces an acid-resistant monomer (dimethyldiallyl ammonium chloride (DMDAAC)) into acid-resistant hydrophobic polymer microspheres and acid-resistant cyclodextrin polymers to enhance the acid resistance, so that it can be used under the acidic conditions of supercritical CO2.
[0052] (2) The components in the supramolecular inclusion enhancement system provided by the present invention interact with each other. The acid-resistant hydrophobic polymer microspheres contain hydrophobic long chains, and the acid-resistant cyclodextrin polymer contains cyclodextrin groups. The hydrophobic cavity structure of cyclodextrin can efficiently identify the hydrophobic groups on the surface of the polymer microspheres, and a new aggregate structure is formed through the inclusion reaction of the host and the guest, thereby increasing the fluid dynamic radius and the bulk viscosity; then, a supramolecular network is constructed by using anionic polybasic organic acids and cationic groups in acid-resistant hydrophobic polymer microspheres and acid-resistant cyclodextrin polymers to generate electrostatic interactions to form a supramolecular inclusion enhancement system, which has a stronger thickening effect than traditional polymers.
[0053] (3) The supramolecular inclusion enhancement system provided by the present invention can be used for blocking gas channeling, and can effectively block the gas channeling, thereby improving the CO2 oil recovery effect. Compared with the traditional particle system, the traditional particle system is easily broken through by gas in the formation, because the medium between the particles in the formation is water. In the heterogeneous supramolecular inclusion enhancement system provided by the present invention, the medium between the particles (acid-resistant hydrophobic polymer microspheres) in the formation is a composite system with high viscosity such as cyclodextrin polymer and polyacid. In addition, the cyclodextrin polymer and polyacid can interact with the surface of the particles, and can act as a cross-linking agent to bond the particles together, thereby effectively blocking the gas channeling. However, this effect is not strong, and the above effect will be destroyed under a certain strong shearing action, thereby reducing the viscosity of the system and improving the injectability; when injected into the underground, the in-situ viscosity increase of the formation after shearing is achieved through self-assembly, which not only solves the problem of poor injectability of the system, but also solves the problem of poor sealing effect of underground gas drive, laying the foundation for the application of low-cost CO2 drive sealing technology.
[0054] (4) The ratio of the acid-resistant hydrophobic polymer microspheres, the acid-resistant cyclodextrin polymer and the polyacid in the present invention needs to be appropriate. If an excessive amount of the acid-resistant cyclodextrin polymer is added, the hydrophobic groups in the microspheres will be completely encapsulated, so that the positively charged hydrophobic groups on the surface of the polymer microspheres cannot interact with the polyacid. In addition, if an excessive amount of the polyacid is added, the excessive negative charge will cause the hydrophobic chains to move away from each other, destroying the spatial network structure formed by the electrostatic interaction.
[0055] (5) In the process of synthesizing the acid-resistant cyclodextrin polymer in the present invention, a three-stage composite initiator system is used, that is, a low-temperature-medium-temperature-high-temperature three-stage composite initiator is used as the initiator system, and the molecular weight of the product is improved by matching different initiators. Among them, the redox agent sodium persulfate / sodium bisulfite as a low-temperature initiator system has the advantages of high decomposition rate and fast initiation reaction; and the azo initiator azobisisobutylamidine dihydrochloride as a medium-temperature initiator can further expand the relative molecular mass of the polymer in the middle stage of the reaction; azobisisobutyronitrile / dibenzoyl peroxide is used as a high-temperature initiator to continue the two-stage reaction and promote the complete reaction. The composite emulsifier used in the synthesis process of the acid-resistant hydrophobic polymer microspheres of the present invention has better stability than a single emulsifier. This is because the complex formed by the composite emulsifier molecules at the oil-water interface makes the two-phase interface more concentrated, and the composite emulsifier increases the mixing entropy, which also makes the emulsification effect better. DETAILED DESCRIPTION
[0056] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0057] Example 1
[0058] A method for preparing a CO2 flooding reservoir heterogeneous supramolecular inclusion synergistic system based on polyacids, comprising the steps of:
[0059] (1) Synthesis of acid-resistant hydrophobic polymer microspheres
[0060] Weigh 39g white oil, 2.7g Span80, and 0.9g Tween80, add them into a four-necked flask equipped with a thermometer, a stirrer, and a condensation reflux device, stir and mix them evenly at a speed of 600r / min, and pass nitrogen for more than 30min to remove dissolved oxygen in the system;
[0061] Weigh 0.105 g of dimethyldiallyl ammonium chloride (DMDAAC), 5.25 g of acrylamide (AM), and 0.105 g of hexadecyldimethylallyl ammonium chloride (C16DMAAC) in a beaker, dissolve them in 21 g of deionized water, stir evenly with a magnetic stirrer, and after stirring and dissolving, adjust the pH value of the system to 7 with NaOH (aqueous solution, 20 wt%), weigh 0.0546 g of N, N-methylenebisacrylamide, add it to the beaker and stir evenly; after each agent is completely dissolved, continue stirring for 5 minutes before dissolving other agents. After all agents are evenly dissolved, pass nitrogen for 15 minutes and ultrasonically oscillate for 15 minutes to fully remove oxygen in the aqueous phase.
[0062] After the oil phase was stirred for 20 min, the aqueous phase was added dropwise at 600 r / min under nitrogen protection, and the aqueous phase was added dropwise to the oil phase at a rate of 1-2 drops per second. After the microemulsion became clear and transparent, the rotation speed was reduced to 350 r / min, and a 0.2% aqueous solution of ammonium persulfate (wherein the mass of ammonium persulfate was 0.01092 g) and a 0.2% aqueous solution of sodium bisulfite (wherein the mass of sodium bisulfite was 0.01092 g) were added to the microemulsion in sequence at a rate of 1-2 drops per second. After the addition was completed, the reaction was continued with stirring at 40° C. under nitrogen protection for 4 h.
[0063] After the reaction is completed, cool and stand at room temperature; repeatedly wash the microemulsion with anhydrous ethanol for 3-5 times to fully remove the oil phase adhering to the solid surface of the microspheres, and separate the solid and liquid with filter paper; place the solid in a 50°C drying oven for 24 hours to fully dry, grind the solid microspheres, and obtain acid-resistant hydrophobic polymer microspheres with an average particle size of 82nm.
[0064] (2) Synthesis of acid-resistant cyclodextrin polymers
[0065] 3.6 g acrylamide and 0.2 g 6-O-allyl-β-cyclodextrin were weighed, dissolved in 20 g deionized water, and placed in a 250 mL three-necked flask, 0.001 g sodium persulfate and 0.00151 g sodium bisulfite were added, and the mixture was dissolved by stirring under N2. 1 g acrylic acid was weighed, 0.002 g azobisisobutylamidine dihydrochloride was added, and the pH value was adjusted to about 7 to 8 with a 20% NaOH aqueous solution, and then transferred to a flask. 0.2 g dimethyldiallylammonium chloride was added, and 0.0025 g azobisisobutylonitrile and 0.0005 g dibenzoyl peroxide were added with a syringe, and the mixture was stirred and mixed uniformly. When the reaction system becomes viscous, stirring is stopped and the three-necked flask is sealed and placed for reaction under nitrogen protection at room temperature for 4 hours to obtain a transparent colloidal product. The product is taken out and cut into small pieces, and purified by acetone precipitation three times. The acid-resistant cyclodextrin polymer particles are obtained by vacuum drying and granulation.
[0066] (3) Preparation of heterogeneous supramolecular inclusion enhancement system for CO2 flooding reservoirs based on polyacids
[0067] Weigh 0.4g of acid-resistant hydrophobic polymer microspheres, slowly disperse them in 100mL of distilled water, and then stir at high speed at room temperature (stirring rate 200r / min) for 10 minutes so that the acid-resistant hydrophobic polymer microspheres can be well dispersed in water. When the acid-resistant hydrophobic polymer microspheres are evenly dispersed, reduce the stirring speed, and expand at room temperature for 4 hours at a speed of 100r / min. Then stop stirring, and put the acid-resistant hydrophobic polymer microsphere dispersion into a 45°C thermostat for aging for 24 hours. Then weigh 0.2g of acid-resistant cyclodextrin polymer and add it to the acid-resistant hydrophobic polymer microsphere dispersion that has been aged. Stir at room temperature for 4 hours at a speed of 100r / min so that the acid-resistant cyclodextrin polymer is completely dispersed in the acid-resistant hydrophobic polymer microsphere dispersion. Put the prepared composite system into a 45°C thermostat for aging for 48 hours. 0.3 g of pimelic acid was weighed and added to the above inclusion system in a ratio of 1:0.75 between acid-resistant hydrophobic polymer microspheres and polyacid, and stirred at room temperature for 0.5 h at a speed of 100 r / min. Finally, it was allowed to stand at room temperature for 2 h to obtain a heterogeneous supramolecular inclusion enhancement system for CO2 flooding reservoirs based on polyacids.
[0068] Example 2
[0069] A method for preparing a heterogeneous supramolecular inclusion enhancement system for CO2 flooding oil reservoirs based on polyacids is as described in Example 1, except that the ratio of acid-resistant hydrophobic polymer microspheres to polyacids is 1:0.5, that is, the amount of pimelic acid is 0.2 g; the other steps and conditions are the same as in Example 1.
[0070] Example 3
[0071] A method for preparing a heterogeneous supramolecular inclusion enhancement system for CO2 flooding oil reservoirs based on polyacids is as described in Example 1, except that the ratio of acid-resistant hydrophobic polymer microspheres to polyacids is 1:2, that is, the amount of pimelic acid is 0.8 g; the other steps and conditions are the same as in Example 1.
[0072] Example 4
[0073] A method for preparing a heterogeneous supramolecular inclusion enhancement system for CO2 flooding oil reservoirs based on polyacids is as described in Example 1, except that the ratio of acid-resistant hydrophobic polymer microspheres to acid-resistant cyclodextrin polymer is 1:1, that is, the acid-resistant cyclodextrin polymer is 0.4g; the other steps and conditions are the same as in Example 1.
[0074] Example 5
[0075] A method for preparing a heterogeneous supramolecular inclusion enhancement system for CO2 flooding oil reservoirs based on polyacids is as described in Example 1, except that: in the preparation of acid-resistant hydrophobic polymer microspheres in step (1), the amount of dimethyldiallylammonium chloride added is 0.2 g; the other steps and conditions are the same as in Example 1.
[0076] Example 6
[0077] A method for preparing a heterogeneous supramolecular inclusion enhancement system for CO2 flooding oil reservoirs based on polyacids is as described in Example 1, except that: in the preparation of acid-resistant hydrophobic polymer microspheres in step (1), the amount of hexadecyl dimethyl allyl ammonium chloride added is 0.2 g; the other steps and conditions are the same as in Example 1.
[0078] Example 7
[0079] A method for preparing a heterogeneous supramolecular inclusion enhancement system for CO2 flooding oil reservoirs based on polyacids is as described in Example 1, except that: in the preparation of the acid-resistant cyclodextrin polymer in step (2), the amount of dimethyldiallylammonium chloride added is 0.3 g; the other steps and conditions are the same as in Example 1.
[0080] Example 8
[0081] A method for preparing a heterogeneous supramolecular inclusion enhancement system for CO2 flooding oil reservoirs based on polyacids is as described in Example 1, except that: in the preparation of the acid-resistant cyclodextrin polymer in step (2), the addition amount of 6-O-allyl-β-cyclodextrin is 0.12 g; the other steps and conditions are the same as in Example 1.
[0082] Comparative Example 1
[0083] A method for preparing a supramolecular inclusion synergistic system is as described in Example 1, except that the acid-resistant cyclodextrin polymer and the polybasic acid pimelic acid are not added; the details are as follows:
[0084] The preparation of acid-resistant hydrophobic polymer microspheres is the same as step (1);
[0085] Omit step (2);
[0086] Step (3) is as follows:
[0087] Weigh 0.4g of acid-resistant hydrophobic polymer microspheres, slowly disperse them in 100mL of distilled water, and then stir at room temperature at high speed (stirring rate 200r / min) for 10 minutes, so that the acid-resistant hydrophobic polymer microspheres can be well dispersed in water. When the acid-resistant hydrophobic polymer microspheres are evenly dispersed, reduce the stirring speed, and expand at room temperature for 4 hours at a speed of 100r / min. Then stop stirring, put the acid-resistant hydrophobic polymer microsphere dispersion into a 45°C thermostat and age for 24 hours to obtain a supramolecular inclusion synergistic system.
[0088] Comparative Example 2
[0089] A method for preparing a supramolecular inclusion synergistic system is as described in Example 1, except that in step (3), no polyacid pimelic acid is added; the details are as follows:
[0090] The preparation of acid-resistant hydrophobic polymer microspheres and acid-resistant cyclodextrin polymers is the same as steps (1) and (2), respectively;
[0091] Step (3) is as follows:
[0092] Weigh 0.4g of acid-resistant hydrophobic polymer microspheres, slowly disperse them in 100mL of distilled water, and then stir at high speed at room temperature (stirring rate 200r / min) for 10 minutes so that the acid-resistant hydrophobic polymer microspheres can be well dispersed in water. When the acid-resistant hydrophobic polymer microspheres are evenly dispersed, reduce the stirring speed, and expand at room temperature for 4 hours at a speed of 100r / min. Then stop stirring, and put the acid-resistant hydrophobic polymer microsphere dispersion into a 45°C thermostat for aging for 24 hours. Then weigh 0.2g of acid-resistant cyclodextrin polymer and add it to the acid-resistant hydrophobic polymer microsphere dispersion that has been aged. Stir at room temperature for 4 hours at a speed of 100r / min so that the acid-resistant cyclodextrin polymer is completely dispersed in the acid-resistant hydrophobic polymer microsphere dispersion. The prepared composite system is placed in a 45°C thermostat for aging for 48 hours to obtain a supramolecular inclusion synergistic system.
[0093] Comparative Example 3
[0094] A method for preparing a supramolecular inclusion synergistic system is as described in Example 1, except that in step (1), the acid-resistant monomer dimethyldiallyl ammonium chloride (DMDAAC) is not added; the other steps and conditions are the same as in Example 1.
[0095] Comparative Example 4
[0096] A method for preparing a supramolecular inclusion synergistic system is as described in Example 1, except that in step (2), the three-stage composite initiation system is changed to an azo reaction system (azobisisobutylamidine dihydrochloride); specifically as follows:
[0097] Step (2) is as follows:
[0098] Weigh 3.6g acrylamide and 0.2g 6-O-allyl-β-cyclodextrin, dissolve in 20g deionized water, and place in a 250mL three-necked flask. Stir continuously to dissolve under the condition of N2; weigh 1g acrylic acid, add 0.002g azobisisobutylamidine dihydrochloride, adjust the pH value to about 7-8 with a 20% NaOH aqueous solution, and then transfer to the flask; add 0.2g dimethyldiallylammonium chloride, stir and mix evenly. Stop stirring when the reaction system becomes viscous, seal the three-necked flask, and react for 4h under nitrogen protection at room temperature to obtain a transparent colloidal product, take it out and cut it into small pieces, precipitate and purify it three times with acetone, and obtain acid-resistant cyclodextrin polymer particles by vacuum drying and granulation.
[0099] The other steps and conditions are the same as in Example 1.
[0100] Comparative Example 5
[0101] A method for preparing a supramolecular inclusion synergistic system is as described in Example 1, except that: in step (3), no acid-resistant cyclodextrin polymer is added; the details are as follows:
[0102] The preparation of acid-resistant hydrophobic polymer microspheres is the same as step (1);
[0103] Omit step (2);
[0104] Step (3) is as follows:
[0105] Weigh 0.4g of acid-resistant hydrophobic polymer microspheres, slowly disperse them in 100mL of distilled water, and then stir at high speed at room temperature (stirring rate 200r / min) for 10 minutes so that the acid-resistant hydrophobic polymer microspheres can be well dispersed in water. When the acid-resistant hydrophobic polymer microspheres are evenly dispersed, reduce the stirring speed, and expand at room temperature for 4 hours at 100r / min. Then stop stirring, and put the acid-resistant hydrophobic polymer microsphere dispersion into a 45°C thermostat for aging for 24 hours. Weigh 0.3g of heptanediol according to the ratio of acid-resistant hydrophobic polymer microspheres to polyacids of 1:0.75 and add it to the above system, stir at room temperature for 0.5h at a speed of 100r / min, and finally stand at room temperature for 2h to obtain a supramolecular inclusion synergistic system.
[0106] Comparative Example 6
[0107] A method for preparing a supramolecular inclusion synergistic system is as described in Example 1, except that in step (1), hexadecyl dimethyl allyl ammonium chloride is replaced by octadecyl dimethyl allyl ammonium chloride; the other steps and conditions are the same as in Example 1.
[0108] Comparative Example 7
[0109] A method for preparing a supramolecular inclusion synergistic system is as described in Example 1, except that in step (2), the acid-resistant monomer dimethyldiallyl ammonium chloride (DMDAAC) is not added; the other steps and conditions are the same as in Example 1.
[0110] Test Example 1
[0111] Shear resistance test. The viscosity values of the synergistic systems obtained in the examples and comparative examples before and after shear were tested. The test method is as follows:
[0112] First, the initial viscosity of the sample at 85°C was measured; then, the viscosity was measured at 1000s -1 The shear rate was 1000 and the shear temperature was 85℃ for 3 minutes. The viscosity at 85℃ after shearing was measured. The viscosity retention rate of the synergistic system after shearing was obtained by analyzing the data. The results are shown in Table 1.
[0113] Table 1 Viscosity data of synergistic system
[0114] system Initial viscosity / mPa·s Viscosity after shearing / mPa·s Viscosity retention rate / % Example 1 112 109 97.4 Example 2 101 92 91.1 Example 3 87 72 82.8 Example 4 97 86 88.7 Example 5 109 104 95.4 Example 6 107 101 94.4 Example 7 105 98 93.3 Example 8 103 94 91.3 Comparative Example 2 74 52 70.3 Comparative Example 3 91 76 83.5 Comparative Example 4 82 60 73.2 Comparative Example 5 65 49 75.4 Comparative Example 6 94 81 86.2 Comparative Example 7 89 71 79.8
[0115] Viscosity From the data in Table 1, it can be seen that the viscosity retention rate of the synergistic system of the present invention is relatively high, indicating that the supramolecular inclusion synergistic system has relatively high viscosity and shear resistance.
[0116] Test Example 2
[0117] Plugging performance test. The plugging performance of the synergistic system obtained in the embodiment and the comparative example was tested, and the test method was as follows:
[0118] (1) A metal gasket with a width of 0.03 mm was added to the middle of the matrix core to make a fracture core model; the core was then placed in a core holder, and the confining pressure was set to 15 MPa and the back pressure to 7.6 MPa;
[0119] (2) Adjust the constant speed pump flow rate to 0.5 mL min -1 Carry out CO2 gas drive until the pressure is stable, record the injection pressure difference on both sides of the core holder, and calculate the permeability;
[0120] (3) 0.5 mL min -1 Inject 0.6 PV of the enhancement system solution into the core at a rate of 100 μm, heat the displacement device to 60-80°C, and shut down the displacement device for 8-12 hours;
[0121] (4) Again at 0.5 mL min -1 The CO2 gas drive was carried out at a rate of 100 until the pressure was stable, and the injection pressure difference on both sides of the core holder was recorded to calculate the permeability and then the plugging rate.
[0122] The plugging performance of the enhancement system prepared in the embodiment and the comparative example was evaluated through indoor core flooding experiments. The results are shown in Table 2.
[0123] Table 2 Plugging effect data of the synergistic system
[0124] system <![CDATA[Pre - gas drive permeability / ×10 -3 μm 2 > <![CDATA[Back gas drive permeability / ×10 -3 μm 2 > Blockage rate / % Example 1 75.4 0.54 99.28 Example 2 85.8 5.06 94.10 Example 3 75.6 7.12 90.58 Example 4 84.6 6.68 92.10 Example 5 79.9 1.21 98.49 Example 6 81.5 1.90 97.67 Example 7 86.7 2.75 96.82 Example 8 73.3 3.14 95.72 Comparative Example 1 76.9 22.55 70.68 Comparative Example 2 77.2 11.97 84.49 Comparative Example 3 78.2 21.56 72.43 Comparative Example 4 83.6 23.77 71.57 Comparative Example 5 82.8 19.20 76.81 Comparative Example 6 79.7 10.52 86.80 Comparative Example 7 80.7 24.00 70.26
[0125] It can be seen from Table 2 that the supramolecular inclusion enhancement system prepared in the embodiment can be smoothly injected into cracks with a size of 0.03 mm, has good injectability, and has a gas phase blocking rate of almost 90% or more, which can block gas channeling channels. The corresponding microsphere blocking rate is only 70.68%. After adding the acid-resistant cyclodextrin polymer, the blocking rate increases to 84.49%.
[0126] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A heterogeneous supramolecular inclusion enhancement system for CO2 flooding reservoirs based on polyacids, characterized in that: The preparation method comprises the following components in parts by weight: 1-10 parts of acid-resistant hydrophobic polymer microspheres, 1-5 parts of acid-resistant cyclodextrin polymers, 1-5 parts of polyacids, and 80-120 parts of water.
2. The CO2 flooding reservoir heterogeneous supramolecular inclusion synergistic system based on polyacid according to claim 1, characterized in that: The heterogeneous supramolecular inclusion enhancement system for CO2 flooding oil reservoirs based on polyacids is prepared by including the following components in parts by weight: 3-5 parts of acid-resistant hydrophobic polymer microspheres, 1-3 parts of acid-resistant cyclodextrin polymers, 2-4 parts of polyacids, and 90-110 parts of water.
3. The CO2 flooding reservoir heterogeneous supramolecular inclusion synergistic system based on polyacid according to claim 1, characterized in that: The method for preparing acid-resistant hydrophobic polymer microspheres comprises the following steps: (1) white oil, Span80 and Tween80 are uniformly mixed to obtain an oil phase; (2) fully dissolving acrylamide (AM), hexadecyl dimethyl allyl ammonium chloride (C16DMAAC), and dimethyl diallyl ammonium chloride (DMDAAC) in water, adjusting the pH value of the system, adding N,N-methylenebisacrylamide (MBA) and mixing evenly to obtain an aqueous phase; (3) adding the aqueous phase dropwise to the oil phase, and then sequentially adding an aqueous solution of ammonium persulfate and an aqueous solution of sodium bisulfite, reacting, washing, drying, and grinding to obtain acid-resistant hydrophobic polymer microspheres.
4. The CO2 flooding reservoir heterogeneous supramolecular inclusion synergistic system based on polyacid according to claim 3, characterized in that: Includes one or more of the following conditions: i. In step (1), the mass ratio of white oil, Span80 and Tween80 is 35-40:2-3:0.5-1.5, preferably 39:2.7:0.9; ii. In step (2), the mass ratio of acrylamide (AM), hexadecyldimethylallylammonium chloride (C16DMAAC), dimethyldiallylammonium chloride (DMDAAC), N,N-methylenebisacrylamide (MBA) and water is 5-6:0.1-0.2:0.1-0.2:0.04-0.06:15-30, preferably 5.25:0.105:0.105:0.0546:21; iii. In step (2), a sodium hydroxide aqueous solution having a mass concentration of 15% to 30% is used to adjust the pH value of the system to 7; iv. In step (3), the dripping rate of the aqueous phase is 1-5 drops per second, and the dripping is carried out under stirring conditions and protection of a protective gas; further preferably, the protective gas is nitrogen or argon; v. In step (3), the mass ratio of acrylamide in the aqueous phase to the mass ratio of the oil phase is 5-6:40-45; vi. In step (3), the dropping rate of the aqueous ammonium persulfate solution and the aqueous sodium bisulfite solution is 1-5 drops per second, and the dropping is carried out under stirring and protective gas protection; further preferably, the protective gas is nitrogen or argon; vii. In step (3), the mass concentrations of the ammonium persulfate aqueous solution and the sodium bisulfite aqueous solution are both 0.02%-0.2%, wherein the mass ratio of ammonium persulfate to sodium bisulfite is 1:1; the mass ratio of ammonium persulfate to acrylamide in the aqueous phase is 1:475-785; viii. In step (3), the reaction temperature is 25-40° C., the reaction time is 2-6 h, and the reaction is carried out under stirring and protective gas protection; more preferably, the protective gas is nitrogen or argon.
5. The CO2 flooding reservoir heterogeneous supramolecular inclusion synergistic system based on polyacid according to claim 1, characterized in that: The method for preparing an acid-resistant cyclodextrin polymer comprises the steps of: Acrylamide (AM) and 6-O-allyl-β-cyclodextrin (DPTD) are dissolved in water, and sodium persulfate and sodium bisulfite are added to fully dissolve to obtain solution A; acrylic acid (AA) and azobisisobutylamidine dihydrochloride are mixed, and the pH value is adjusted to 7-8 to obtain solution B; solution A and solution B are mixed, dimethyldiallylammonium chloride, azobisisobutyronitrile and dibenzoyl peroxide are added, mixed evenly, reacted, and then crushed, precipitated, purified, dried and granulated to obtain an acid-resistant cyclodextrin polymer.
6. The CO2 flooding reservoir heterogeneous supramolecular inclusion synergistic system based on polyacid according to claim 5, characterized in that: Includes one or more of the following conditions: i. The mass ratio of acrylamide (AM) and 6-O-allyl-β-cyclodextrin (DPTD) is 15-30:1, preferably 18:1; the mass ratio of acrylamide and water is 1:3-8; the mass ratio of acrylamide (AM), sodium persulfate and sodium bisulfite is 3.6:0.0005-0.005:0.001-0.002, preferably 3.6:0.001:0.00151; ii. The mass ratio of acrylic acid (AA), azobisisobutylamidine dihydrochloride and acrylamide is 1:0.001-0.005:3-4, preferably 1:0.002:3.6; iii. Use a 15%-20% NaOH aqueous solution to adjust the pH; iv. the mass ratio of dimethyldiallylammonium chloride, azobisisobutyronitrile, dibenzoyl peroxide and acrylamide is 0.1-0.3:0.001-0.005:0.0001-0.001:3-4, preferably 0.2:0.0025:0.0005:3.6; v. The reaction temperature is room temperature, the reaction time is 1-4 hours, and the reaction is carried out under static conditions and protection of protective gas; preferably, the protective gas is nitrogen or argon.
7. The heterogeneous supramolecular inclusion synergistic system for CO2 flooding reservoirs based on polyacids according to claim 1, characterized in that: The polyacid is pimelic acid, citric acid, disodium ethylenediaminetetraacetate or sodium polyacrylate.
8. The method for preparing the heterogeneous supramolecular inclusion synergistic system for CO2 flooding reservoir based on polyacid according to any one of claims 1 to 7, comprising the steps of: The acid-resistant hydrophobic polymer microspheres are fully dispersed in water, and subjected to expansion and aging reactions; then the acid-resistant cyclodextrin polymer is added, fully dispersed, and then subjected to aging reactions; polyacids are added, fully dispersed, and allowed to stand to obtain a polyacid-based CO2 flooding reservoir heterogeneous supramolecular inclusion enhancement system.
9. The method for preparing the heterogeneous supramolecular inclusion synergistic system for CO2 flooding reservoir based on polyacid according to claim 8, characterized in that: Includes one or more of the following conditions: i. Add the acid-resistant hydrophobic polymer microspheres into water and stir at room temperature at 100-300 r / min for 5-15 minutes to fully disperse them; ii. Expansion is carried out by stirring at room temperature and 80-120 r / min for 3-5 hours; iii. Aging is to place the sample at 40-50°C for 20-30 hours; iv. After adding the acid-resistant cyclodextrin polymer, stir at room temperature at a speed of 80-120 r / min for 2-6 hours to fully disperse; v. The aging reaction after adding the acid-resistant cyclodextrin polymer is to stand and age for 40-50 hours at 40-50°C; vi. After adding the polyacid, stir at room temperature at a speed of 80-120r / min for 0.1-1 hour to fully disperse; vii. The standing temperature is room temperature and the standing time is 1-3 hours.
10. The use of the polyacid-based heterogeneous supramolecular inclusion enhancement system for CO2 flooding reservoirs according to any one of claims 1 to 7, characterized in that: Applied to plug gas channel in CO2 flooding reservoirs.
Citation Information
Patent Citations
Cation hydrophobic associating polymer oil displacement agent and preparation method thereof
CN102660250A
Temperature-resistant and salt-resistant dendritic supramolecular polymer oil displacement agent as well as preparation method and application thereof
CN111393545A
Synergistic supramolecular inclusion polymer oil displacement system as well as preparation method and application thereof
CN117946652A
Temperature-resistant and salt-resistant amphiphilic polymer, supramolecular oil displacement system and application
CN118146441A
Temperature-resistant and salt-resistant polymer with cyclodextrin structure and preparation method of temperature-resistant and salt-resistant polymer
CN118546303A