Method and system for industrially and continuously preparing mesophase pitch from coal pitch

Through the dissolution, hydrogenation and thermal polymerization reaction processes of medium and low temperature coal tar asphalt, the problems of high cost, large energy consumption and poor quality of spinning carbon fiber mesophase asphalt are solved, and efficient and low-cost mesophase asphalt preparation is achieved. In the production of high-modulus carbon fiber materials.

CN118978935APending Publication Date: 2024-11-19SHAANXI COAL-BASED SPECIAL FUEL RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411404813.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing preparation methods for spinning carbon fiber mesophase bitumen have problems such as high cost, large energy consumption and poor quality, and it is difficult to achieve continuous production.

Method used

Using medium and low temperature coal tar asphalt as a raw material, high-quality mesophase asphalt is prepared through dissolution, hydrogenation and thermal polymerization reaction processes, including the purification, hydrogenation and thermal polymerization steps of asphalt, and the static mixer can be heated in series and heat. Filtration devices, decanter centrifuges and asphalt polymerization reactors are carried out continuously.

Benefits of technology

The continuous industrial preparation of mesophase asphalt is realized, which reduces cost and energy consumption, improves product quality, and is suitable for the production of high-modulus carbon fiber materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978935A_ABST
    Figure CN118978935A_ABST
Patent Text Reader

Abstract

The invention provides a method and system for industrially and continuously preparing mesophase pitch from coal pitch, and the method comprises the following steps: S1, refining pitch: taking medium and low temperature coal tar pitch as raw material pitch, mixing the heated raw material pitch with a pitch solvent, dissolving, filtering, centrifuging to remove insoluble substances, and then carrying out reduced pressure distillation on the pitch solvent in an evaporator to obtain refined pitch; discharging the refined asphalt from the bottom of the evaporator, and storing the refined asphalt in a refined asphalt temporary storage tank with a tank body at a constant temperature of 80-120 DEG C, so that the refined asphalt is kept in a liquid state; s2, asphalt hydrogenation: reacting a hydrogenation reagent with refined asphalt flowing out of a refined asphalt temporary storage tank for 2-20 hours at the temperature of 300-400 DEG C and under the pressure of 2-8 MPa, and evaporating out a solvent to obtain hydrogenated asphalt; and S3, preparing the intermediate phase through asphalt thermal polymerization. The method can be used for continuously and industrially preparing the mesophase pitch and has the advantages of continuity, low cost, low energy consumption, high quality and the like, and the high-quality mesophase pitch capable of being used for preparing a carbon fiber material is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of mesophase asphalt, a raw material for preparing asphalt-based carbon fibers, and specifically relates to a method and system for industrially continuously preparing mesophase asphalt from coal tar pitch. Background Art

[0002] Coal tar is one of the main by-products in the coal chemical industry. The yield of coal tar in coal chemical projects is about 3~4.5%. The coal tar in Shaanxi and Shanxi regions is mainly medium and low temperature coal tar, and coal tar asphalt accounts for about 55% of the medium and low temperature coal tar. Therefore, how to increase the added value of medium and low temperature coal tar asphalt products has become increasingly important for the coal chemical industry.

[0003] One of the most important and highest value-added directions of mesophase asphalt is the preparation of high modulus carbon fiber. Asphalt-based carbon fiber has the property of ultra-high modulus and is used in aerospace, aircraft manufacturing, communications industry and other fields. However, in terms of the current cost structure of the asphalt-based carbon fiber industry, direct materials are its main cost, accounting for more than 80%, followed by labor costs and manufacturing costs. Therefore, improving the preparation process of asphalt-based carbon fiber, using cheap medium and low temperature coal tar asphalt, and continuous process operation can effectively reduce the manufacturing cost of asphalt-based carbon fiber. However, the raw asphalt currently used in the preparation of mesophase asphalt in China requires a complex refining process, and the raw asphalt used to prepare mesophase asphalt is strictly regulated internationally, which greatly restricts the development and application of asphalt-based carbon fiber in China.

[0004] Patent CN116023968 introduces a process for continuously producing mesophase asphalt using petroleum slurry as raw material. However, the adsorption and filtration of the heavy components of the slurry in its refining unit are prone to clogging of the adsorbent and the filter screen. At the same time, there is no clear hydrogenation effect, and the carbon-hydrogen ratio of the asphalt cannot be effectively adjusted, and the softening point and the content of the mesophase asphalt cannot be controlled.

[0005] Patent CN 113680301 introduces a device for preparing spinnable mesophase asphalt, which is a vertical tube reactor with multiple layers of rotating blades and a temperature control unit inside, and is used to prepare asphalt into mesophase asphalt. It can be considered that the reaction device uses refined raw asphalt to directly prepare mesophase asphalt without hydrogenation and other steps, which has certain defects and cannot effectively control the control indicators such as the carbon-hydrogen ratio and softening point of the asphalt molecules.

[0006] Patent CN 112852462 also introduces a method for continuously preparing mesophase asphalt using oil slurry as raw material, but the process of removing solid impurities from the crude oil by hot filtration and ion exchange involves intermittent operation of replacing filter materials and ion exchange materials. Ionic surfactants are introduced during the catalytic hydrogenation process, resulting in a certain amount of salt in the prepared mesophase asphalt, which reduces the quality of the mesophase asphalt.

[0007] Therefore, there is a need to develop an improved industrial continuous preparation process or system for mesophase asphalt. Summary of the invention

[0008] The present invention provides a method and system for industrially continuously preparing mesophase asphalt from asphalt, so as to solve the problems of the existing preparation method of mesophase asphalt that can be used for spinning carbon fiber, such as the lack of continuous production, high cost and energy consumption, and poor quality.

[0009] The technical solution of the present invention is as follows: According to one aspect of the present invention, there is provided a method for industrially continuously preparing mesophase asphalt from coal tar pitch, comprising the following steps: S1. Refining of asphalt: taking medium-low temperature coal tar pitch as raw material asphalt, the heated raw material asphalt is mixed with an asphalt solvent, and after dissolving, filtering and centrifuging to remove insoluble matter, the asphalt is distilled under reduced pressure to obtain refined asphalt and stored in a refined asphalt temporary storage tank whose tank body is kept at a constant temperature of 80°C to 120°C, so that the refined asphalt remains in a liquid state; S2. Asphalt hydrogenation: reacting a hydrogenation reagent and the refined asphalt flowing out of the refined asphalt temporary storage tank at a temperature of 300°C to 400°C and a pressure of 2MPa to 8MPa for 2 to 20 hours, and distilling off the solvent to obtain hydrogenated asphalt; S3. Preparation of mesophase by thermal polymerization of asphalt: reacting the hydrogenated asphalt in an asphalt polymerization reactor at a temperature of 350°C to 500°C, a pressure of 0.2MPa to 2MPa and under nitrogen bubbling for 4h to 42h to obtain mesophase asphalt.

[0010] Optionally, in the above-mentioned method for industrially continuously preparing mesophase asphalt from coal tar pitch, in step S1, the asphalt solvent is selected from one or a mixture of two or more of tar fraction oil at 230°C to 300°C, coal tar fraction oil at 280°C to 360°C, top circulating oil, quinoline, dichloromethane, and N,N-dimethylformamide.

[0011] Optionally, in the above-mentioned method for industrial continuous preparation of intermediate phase asphalt from coal tar, in step S1, a series of heatable static mixers with a heating device on the outer wall are used to mix the raw asphalt and the asphalt solvent, and the temperature in the series of heatable static mixers is between 100°C and 250°C, so that the raw asphalt is completely dissolved in the asphalt solvent. After filtration and sedimentation through a 0.1 micron to 20 micron filter mesh in a hot filtration device, impurities are centrifuged at a centrifugal speed of 3000rpm to 6000rpm in a horizontal screw centrifuge, and then the asphalt solvent is separated in a scraped film evaporator to obtain refined asphalt.

[0012] Optionally, in the above-mentioned method for industrially continuously preparing mesophase asphalt from coal tar pitch, in step S2, the hydrogenation reagent and refined asphalt are both pressurized to 2MPa~10MPa, mixed and reacted in a two-stage hydrogenation reactor, wherein the temperature of the first-stage hydrogenation reactor is 300℃~350℃, and the temperature of the second-stage hydrogenation reactor is 350℃~400℃.

[0013] Optionally, in the above-mentioned method for industrially continuously preparing mesophase asphalt from coal tar, in step S2, the hydrogenation reagent is selected from one or a mixture of two or more of tetralin, decalin, and the vacuum tower bottom product oil of coal tar hydrogenation, and the mass ratio of refined asphalt to hydrogenation reagent is 1:0.5~2.

[0014] Optionally, in the above-mentioned method for industrially continuously preparing mesophase asphalt from coal tar, in step S2, the hydrogenation reagent is selected from the vacuum tower bottom product oil of coal tar hydrogenation, or a mixed product of tetralin and the vacuum tower bottom product oil of coal tar hydrogenation in a mass ratio of 0.2~0.4:1.

[0015] According to another aspect of the present invention, a system for industrially continuously preparing intermediate phase asphalt from coal tar is provided, comprising an asphalt storage tank, a series-type heatable static mixer, a hot filtration device, a horizontal screw centrifuge, a scraping evaporator, a refined asphalt temporary storage tank, a heatable static mixer, a first-stage hydrogenation reactor, a second-stage hydrogenation reactor, an evaporator, an asphalt polymerization reactor and an intermediate phase asphalt storage tank, which are fluidically connected in sequence, and the system also comprises a solvent storage tank fluidically connected to the series-type heatable static mixer, and a hydrogenation reagent storage tank fluidically connected to the heatable static mixer via a hydrogenation reagent booster pump, wherein a first condenser is connected to the top of the scraping evaporator, the first condenser is connected to a solvent collection tank, a first vacuum tank, and a first vacuum pump in sequence, the solvent storage tank is also connected to the solvent collection tank via a solvent recovery pump, the top of the evaporator is connected to a second condenser, the second condenser is connected to a by-product collection tank, the top of the intermediate phase asphalt storage tank is connected to a third condenser, the third condenser is connected to a small molecule by-product collection tank, a vacuum, a second vacuum tank and a second vacuum pump in sequence.

[0016] Optionally, in the above-mentioned system for industrially continuously preparing intermediate phase asphalt from coal tar, a solvent metering pump is provided between the solvent storage tank and the series-type heatable static mixer, an asphalt metering pump is provided between the asphalt storage tank and the series-type heatable static mixer, an asphalt high-pressure pump is provided between the refined asphalt temporary storage tank and the heatable static mixer, an asphalt delivery pump is provided between the scraper evaporator and the refined asphalt temporary storage tank, a delivery pump is provided between the horizontal screw centrifuge and the scraper evaporator, and a hydrogenated asphalt delivery pump is provided between the evaporator and the asphalt polymerization reactor.

[0017] Optionally, in the above-mentioned system for industrially continuously preparing mesophase asphalt from coal tar pitch, the system also includes a solvent heater electrically connected to the hot filtration device, the solvent storage tank, and the solvent collection tank.

[0018] Optionally, in the above-mentioned system for industrially continuously preparing mesophase asphalt from coal tar pitch, the pipeline where the asphalt exists is provided with electric heating, and the heating temperature before hydrogenation is 80°C~150°C, and the heating temperature after hydrogenation is 200°C~300°C.

[0019] According to the technical solution of the present invention, the beneficial effects produced are: The method and system for industrially continuously preparing mesophase asphalt from asphalt of the present invention use medium-low temperature coal tar asphalt as raw material, and obtain mesophase asphalt that can be used for spinning carbon fiber by dissolving, refining, hydrogenating, and thermally polycondensing the medium-low temperature coal tar asphalt. The present invention can continuously prepare mesophase asphalt industrially, and has the advantages of continuity, low cost, low energy consumption, and high quality. It solves the problem of difficult preparation of mesophase asphalt from the raw material end, and obtains high-quality mesophase asphalt that can be used for preparing carbon fiber materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the specific implementation of the present invention or the technical solution in the prior art, the drawings required for use in the specific implementation or the description of the prior art are briefly introduced below.

[0021] Figure 1 It is a schematic flow chart of the method for industrially continuously preparing mesophase asphalt from asphalt of the present invention; Figure 2 This is a process flow chart of the asphalt industrial continuous preparation system of mesophase asphalt of the present invention. Among them: 001 solvent storage tank, 002 asphalt storage tank, 003 solvent metering pump, 004 asphalt metering pump, 005 serial heated static mixer, 006 hot filtration device, 007 asphalt filtration residue, 008 solvent heater, 009 horizontal screw centrifuge, 010 asphalt centrifugal residue, 011 delivery pump, 012 scraping evaporator, 013 first condenser, 014 solvent collection tank, 015 recovery solvent pump, 016 first vacuum tank, 017 first vacuum pump, 018 asphalt delivery pump, 019 refined asphalt temporary storage tank, 020 asphalt high pressure pump , 021 hydrogenation reagent storage tank, 022 hydrogenation reagent booster pump, 023 heatable static mixer, 024 first-stage hydrogenation reactor, 025 second-stage hydrogenation reactor, 026 pressure reducing valve, 027 evaporator, 028 second condenser, 029 by-product collecting tank, 030 hydrogenation reagent by-product, 031 hydrogenation asphalt delivery pump, 032 asphalt polymerization reactor, 033 pressure regulating valve, 034 intermediate phase asphalt storage tank, 035 intermediate phase asphalt, 036 third condenser, 037 small molecule by-product collecting tank, 038 second vacuum tank, 039 second vacuum pump. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical method and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and specific examples. These examples are only illustrative and not limiting of the present invention.

[0023] The method for industrially continuously preparing mesophase asphalt from asphalt of the present invention comprises the following steps: raw asphalt is mixed with an asphalt solvent, dissolved, hot filtered, and centrifuged to remove insoluble residues, and the solvent is evaporated to obtain refined asphalt; the refined asphalt is mixed with a hydrogenation reagent and then reacted under high temperature and high pressure, and the hydrogenated asphalt is obtained after the by-product of the hydrogenation reagent is separated; finally, the hydrogenated asphalt is thermally polycondensed under nitrogen bubbling at a higher temperature, and the mesophase asphalt is obtained after small molecular substances are removed.

[0024] like Figure 1 and Figure 2 As shown, the method for industrially continuously preparing mesophase asphalt from coal tar pitch of the present invention comprises the following steps: S1. Refining of asphalt: medium-low temperature coal tar asphalt is used as raw material asphalt, the heated raw material asphalt is mixed with an asphalt solvent, dissolved, filtered, centrifuged to remove insoluble matter, and then distilled under reduced pressure to obtain refined asphalt and stored in a refined asphalt temporary storage tank with a constant temperature of 80°C to 120°C to keep the refined asphalt in a liquid state; like Figure 2As shown, the solvent storage tank 001 is used to store the asphalt solvent for dissolving the raw asphalt. The asphalt solvent can be selected from one or a mixture of two or more of tar fraction oil of 230°C to 300°C, coal tar fraction oil of 280°C to 360°C, top cycle oil, quinoline, dichloromethane, N,N-dimethylformamide. Preferably, the asphalt solvent is selected from one or a mixture of two or more of coal tar products distilled above 200°C such as coal tar fraction oil of 280°C to 360°C, tar fraction oil of 230°C to 300°C, top cycle oil, etc. More preferably, the asphalt solvent is selected from coal tar fraction oil of 280°C to 360°C or top cycle oil or a mixture of the two.

[0025] The asphalt solvent is dissolved and delivered to the serial heated static mixer 005 through the solvent metering pump 003. The asphalt solvent is heated to 80~120℃ in the pipeline during the transportation process, and has the same temperature when mixed with the raw asphalt. The asphalt storage tank 002 is used to store medium and low temperature coal tar asphalt or other asphalt. The storage tank has a heating function to ensure that the asphalt is liquid and the temperature of the liquid raw asphalt is controlled between 80~120℃. The asphalt transportation pipeline is equipped with electric heating. The liquid raw asphalt is delivered to the serial heated static mixer 005 through the asphalt metering pump 004. The raw asphalt and the asphalt solvent are mixed in the serial heated static mixer 005 to achieve the dissolution of the asphalt. The use of a series-connected heatable static mixer 005 with a multi-section outer wall and a heating device can achieve the temperature and time required for mixing. The mixing time is between 0.5h and 8h. Preferably, the residence time of the raw asphalt in the series-connected heatable static mixer 005 is 0.5~4h to ensure that the asphalt can be fully mixed with the solvent. At the same time, external heating maintains the temperature between 120~250℃, ensuring the full dissolution of the asphalt.

[0026] The completely dissolved asphalt enters the hot filter device 006, wherein the upper part of the hot filter device has a metal filter screen with a mesh size of 0.1 to 20 microns. The hot filter device 006 has a certain volume, which can reduce the surge of the solvent asphalt and play a dual role of sedimentation and filtration. At the same time, there is a heated solvent pipeline on the top, which can backwash the filter screen to avoid clogging of the filter screen. The asphalt is filtered out of the asphalt filter residue 007 in the hot filter device 006, and the first step of deslagging is completed. At this time, the quinoline insoluble content in the asphalt is reduced to less than 0.5%. The asphalt solution that has completed the first step of deslagging enters the centrifugal device through the heating pipe. The present invention preferably uses a horizontal screw centrifuge 009, and a vertical industrial centrifuge can also be used to achieve continuous centrifugal filtration of the asphalt solution. The asphalt is subjected to high-temperature centrifugal deslagging at 120 to 150° C. at a speed of 3000 to 6000 rpm in the centrifuge. The asphalt centrifugal residue 010 is discharged through the centrifuge screw sheet, and the asphalt solvent enters the distillation equipment-scraping evaporator 012 from the rear end of the centrifuge through the delivery pump 011. The content of quinoline insoluble matter in the asphalt after the second step of deslagging is reduced to below 0.01%, meeting the requirements for preparing mesophase asphalt.

[0027] The purified asphalt solution enters the distillation equipment through the delivery pump 011. The distillation equipment can be a distillation tower, a rotary evaporator or other distillation equipment. The present invention preferably uses a scraped film evaporator 012 to increase the evaporation area, improve the evaporation efficiency and reduce the equipment volume. At the same time, the use of reduced pressure distillation reduces the energy consumption required for evaporation. The asphalt is removed and dissolved in the scraped film evaporator 012 while being heated both inside and outside. The refined asphalt is discharged from the bottom of the scraped film evaporator 012 and transported to the refined asphalt temporary storage tank 019 through the delivery pump 018. The asphalt solvent gas is condensed into liquid through the first condenser 013, collected in the solvent collection tank 014, and sent back to the solvent storage tank 001 through the solvent recovery pump 015 or used to rinse the filter screen of the hot filter device 006 after being heated by the solvent heater 008. The first vacuum pipe 016 and the first vacuum pump 017 provide negative pressure for solvent removal, thereby accelerating the efficiency of solvent removal.

[0028] Refined asphalt temporary storage tank 019 is a heated tank body, which stores the prepared refined asphalt and provides refined asphalt for the hydrogenation process. The tank body is kept at a constant temperature of 80~120℃ to keep the refined asphalt in a liquid state. The softening point of refined asphalt is similar to that of raw asphalt, between 60~75℃.

[0029] S2. Asphalt hydrogenation: react the hydrogenation reagent with the refined asphalt flowing out of the refined asphalt temporary storage tank at a temperature of 300-400°C and a pressure of 2-8MPa for 2-20h, and then evaporate the solvent to obtain hydrogenated asphalt; The hydrogenation reagent storage tank 021 is used to store the hydrogenation reagent, which is selected from one or a mixture of two or more of tetralin, decalin, tetrahydroquinoline, and vacuum tower bottom product oil of coal tar hydrogenation; preferably, the vacuum tower bottom product oil of coal tar hydrogenation is used as the hydrogenation reagent, or a mixture of tetralin and vacuum tower bottom product oil of coal tar hydrogenation at a ratio of 0.2 to 0.4:1 is used as the hydrogenation reagent; preferably, the hydrogenation reagent is one or more mixtures of vacuum second-stage tower bottom oil in the coal tar hydrogenation product. The mass ratio of refined asphalt to hydrogenation reagent is between 1:0.5 and 2. Asphalt hydrogenation effectively improves the composition of aromatics and branched aromatics in coal tar, and the prepared mesophase asphalt is more suitable for spinning.

[0030] The refined asphalt enters the heatable static mixer 023 through the refined asphalt metering pump 020 and is evenly mixed with the hydrogenation reagent passing through the hydrogenation reagent booster pump 022, and then enters the first stage hydrogenation reactor 024. At this time, the pressure of the mixed solution of refined asphalt and hydrogenation reagent increases to between 2 and 10 MPa, and then enters the second stage hydrogenation reactor 025 with a higher temperature to continue the hydrogenation reaction. Among them, the hydrogenation reagent is heated to 80-120°C in the pipeline before entering the reactor, and is mixed with the refined asphalt in the heatable static mixer 023 and heated to between 180-200°C. The asphalt high-pressure pump 020 and the hydrogenation reagent booster pump 022 convey the refined asphalt and the hydrogenation reagent, and at the same time provide a reaction pressure of 2-8 MPa for the hydrogenation reactor. The reaction temperature of the first stage hydrogenation reactor is between 300-350°C, and the reaction temperature of the second stage hydrogenation reactor is between 350-400°C. The residence time of the refined asphalt and the hydrogenation reagent in each of the two hydrogenation reactors is 1-10 hours, and the hydrogenation reaction is completed. After the hydrogenated mixed asphalt comes out of the reactor, it is decompressed by the pressure reducing valve 026 and then enters the evaporator 027. The solvent that has completed hydrogenation is evaporated in the evaporator 027, and the hydrogenated asphalt is obtained at the bottom. The solvent that has completed hydrogenation evaporates into gas, which is condensed by the second condenser 028 and stored in the by-product collection tank 029, and the hydrogenation reagent by-product 030 is released. The second vacuum tank 038 provides negative pressure for the evaporation of the hydrogenation reagent by-product, and the second vacuum pump 039 provides vacuum pressure, thereby realizing the reduced pressure distillation of the hydrogenation reagent by-product and controlling the solvent content of the hydrogenated asphalt.

[0031] S3. Preparation of mesophase by thermal polymerization of asphalt: The hydrogenated asphalt is reacted in an asphalt polymerization reactor at a temperature of 350-500°C, a pressure of 0.2-2 MPa and nitrogen bubbling for 4-42 hours to obtain the mesophase asphalt.

[0032] The hydrogenated asphalt is pumped to the asphalt polymerization reactor 032 through the hydrogenated asphalt delivery pump 031, wherein 10~60L / kg.h of nitrogen is introduced into the bottom according to the asphalt flow rate and residence time. The asphalt polymerization reactor 032 heats the asphalt reaction temperature to 350~500℃, preferably 380~500℃, and the pressure is controlled between 0.2~2MPa. The residence time is 4~42h, preferably 4~40h. There are multiple layers of porous partitions in the asphalt polymerization reactor 032 to make the gas-liquid distribution more uniform. The mesophase asphalt that has completed the reaction enters the mesophase asphalt storage tank 034 through the pressure regulating valve 033, and the discharging material from the bottom is cooled by water or under nitrogen protection to obtain the mesophase asphalt 035. The mesophase asphalt and some small molecular weight by-products are obtained by reaction in the asphalt polymerization reactor 032. The small molecular by-products are vaporized by decompression in the mesophase asphalt storage tank 034, and are collected in the small molecular by-product collection tank 037 after condensation by the third condenser 036. Among them, the mesophase asphalt storage tank 034 is equipped with an electric heating device outside to maintain the temperature between 280 and 300°C, so that the mesophase asphalt remains in liquid state, which is convenient for timely discharge. The prepared intermediate small asphalt solid has no pores, a density between 1.5 and 1.6 kg / L, and a complete wide-area streamline shape under a polarizing microscope.

[0033] The method for industrially continuously preparing mesophase asphalt from coal tar pitch of the present invention uses medium-low temperature coal tar pitch as raw material, and after refining the asphalt through continuous operations such as heat sedimentation, filtration, centrifugation, etc., the asphalt is directly hydrogenated and desolventized, and then continuously heat-polycondensed to remove small molecules to obtain mesophase asphalt. The prepared mesophase asphalt is mainly used as raw material asphalt for spinning carbon fiber materials. The preparation process adopted by the present invention realizes the industrialized continuous preparation of mesophase asphalt, has the advantages of continuity, low cost, low energy consumption, high quality, etc., and is innovative in terms of industrial application.

[0034] The system for industrially continuously preparing mesophase asphalt from coal tar pitch of the present invention is as follows: Figure 2As shown, it includes an asphalt storage tank 001, a serially heatable static mixer 005, a hot filter 006, a horizontal screw centrifuge 009, a scraping evaporator 012, a refined asphalt temporary storage tank 019, a heatable static mixer 023, a first-stage hydrogenation reactor 024, a second-stage hydrogenation reactor 025, an evaporator 027, an asphalt polymerization reactor 032 and an intermediate phase asphalt storage tank 034, which are fluidically connected in sequence, and also includes a solvent storage tank 001 fluidically connected to the serially heatable static mixer 005, a hydrogenation reagent storage tank 021 fluidically connected to the heatable static mixer 023 via a hydrogenation reagent booster pump 022. , wherein the top of the scraping evaporator 012 is connected to a first condenser 013, the first condenser 013 is connected to a solvent collecting tank 014, a first vacuum tank 016, and a first vacuum pump 017 in sequence, and the solvent storage tank 001 is also connected to the solvent collecting tank 014 via a solvent recovery pump 105; the top of the evaporator 027 is connected to a second condenser 028, the second condenser 028 is connected to a by-product collecting tank 029; the top of the intermediate phase asphalt storage tank 034 is connected to a third condenser 036, the third condenser 036 is connected to a small molecule by-product collecting tank 037, a second vacuum tank 038, and a second vacuum pump 039 in sequence.

[0035] A solvent metering pump 003 is provided between the solvent storage tank 001 and the serially heated static mixer 005, an asphalt metering pump 004 is provided between the asphalt storage tank 002 and the serially heated static mixer 005, an asphalt high-pressure pump 020 is provided between the refined asphalt temporary storage tank 019 and the heated static mixer 023, an asphalt delivery pump 018 is provided between the scraping evaporator 012 and the refined asphalt temporary storage tank 019, a delivery pump 011 is provided between the horizontal screw centrifuge 009 and the scraping evaporator 012, and a hydrogenated asphalt delivery pump 031 is provided between the evaporator 027 and the asphalt polymerization reactor 032.

[0036] The system also includes a solvent heater 008, which is electrically connected to the hot filter device 006, the solvent storage tank 001, and the solvent collection tank 014 respectively; electric heating is provided in the pipeline where the asphalt exists, and the heating temperature before hydrogenation is 80~150℃, and the heating temperature after hydrogenation is 200~300℃, to ensure that the asphalt is in a liquid state in the pipeline, and the asphalt solvent and the hydrogenation reagent are heated to between 80~120℃ after leaving the tank body, to facilitate the mixing of the asphalt and the solvent.

[0037] Combine the following Figure 2 The specific implementation steps of the present invention are further described.

[0038] The process for industrially continuously preparing mesophase asphalt from coal tar pitch of the present invention comprises the following steps: S1. Select medium-temperature coal tar pitch as raw material asphalt, and purify the medium-temperature coal tar pitch: use a coal tar fraction oil with a temperature of 280°C to 360°C as asphalt solvent, pass through the solvent metering pump 003 at a flow rate of 20kg / h and be heated to 80°C through pipeline heating, and pass through the asphalt metering pump 004 with the medium-temperature coal tar pitch of 100°C at a flow rate of 20kg / h, and enter the series-type heatable static mixer 005 for uniform mixing, and the asphalt is completely dissolved in the solvent. The asphalt is heated from 100°C to 180°C in the series-type heatable static mixer 005, and enters the hot filtration device 006. The residence time in the hot filtration device 006 is 4 hours, and the temperature is maintained at 150-180°C. After filtration and sedimentation through a 10-micron stainless steel mesh screen at the top, it enters the horizontal screw centrifuge 009 and is subjected to high-temperature centrifugation at a speed of 4000rpm at 120-150°C. In the hot filtration device 006, 007 asphalt filtration residue with a mass fraction of 5-8% of the raw asphalt is separated, and 3-5% asphalt centrifugal residue is separated in the horizontal screw centrifuge 009. The asphalt solution after centrifugation enters the scraped film evaporator 012 through the delivery pump 011 to quickly separate the solvent and asphalt, wherein the solvent is condensed into liquid through the first condenser 013 and recovered in the solvent collection tank 014, and pumped to the solvent storage tank 001 through the recovery volume pump 015. The recovered solvent can also be heated by the solvent heater 008 and then backwashed to the filter screen of the hot filtration device 006 to improve the service life and filtration efficiency of the filter screen. The refined asphalt obtained at the bottom of the scraped film evaporator 012 is pumped to the refined asphalt temporary storage tank 019 through the asphalt delivery pump 018 to obtain refined asphalt. The first vacuum pump 017 and the first vacuum tank 016 provide a vacuum degree of 0.095-0.098MPa for the solvent recovery system, so that all solvent components below 360°C can be completely evaporated during the distillation process. Asphalt temporary storage tank 019 is equipped with a heating jacket to maintain the asphalt in liquid state at 100~120℃.

[0039] S2. Asphalt hydrogenation: The hydrogenation reagent in the hydrogenation reagent storage tank 021 is a mixture of tetralin and coal tar hydrogenation by-products in a mass ratio of 1:5. It is mixed with 18kg / h of refined asphalt from the asphalt high-pressure pump 020 in a heatable static mixer 023 through the hydrogenation reagent booster pump 022 at a flow rate of 20kg / h. After the refined asphalt and the hydrogenation reagent are pressurized to a pressure of 4MPa, a uniform miscible mixed liquid is formed in the heatable static mixer 023, which is heated to 200°C. The refined asphalt and the hydrogenation reagent enter the first hydrogenation reactor 024 and are rapidly heated to 300°C. After coming out of the first hydrogenation reactor 024, the temperature of the hydrogenated mixed asphalt reaches 350°C, and then enters the second hydrogenation reactor 025. The temperature entering the second hydrogenation reactor 025 is 350°C, and the temperature after leaving the second hydrogenation reactor 025 is 400°C. The residence time of the asphalt in the two hydrogenation reactors is 3h respectively. After the hydrogenation reaction is completed, the mixed solution is decompressed by the pressure reducing valve 026 and enters the evaporator 027. While controlling the vacuum degree between 0.08 and 0.09 MPa, the hydrogenation reagent by-products and hydrogenated asphalt are separated by reduced pressure distillation. The hydrogenation reagent by-product gas is condensed in the second condenser 028 and then collected in the by-product collecting tank 029. The hydrogenation reagent by-product 030 is released. The bottom temperature of the evaporator 027 is maintained between 200 and 250°C to allow the hydrogenation reagent by-products to completely evaporate and obtain hydrogenated asphalt.

[0040] Step 3, thermal polymerization to prepare mesophase asphalt: 200°C liquid hydrogenated asphalt is transported by hydrogenated asphalt delivery pump 031 at a rate of 18kg / h into asphalt polymerization reactor 032, and the temperature is rapidly raised to 400°C. At the same time, 0.5MPa nitrogen with a purity of more than 99.9% is introduced into the bottom, and the nitrogen flow rate is 30L / (kg.h) relative to the mass of asphalt. The introduced nitrogen is preheated to 300°C to bubble the asphalt. The asphalt is gradually heated from 400°C to 450°C in the asphalt polymerization reactor 032, and stays in the asphalt polymerization reactor 032 for 10 hours to complete the polycondensation to obtain the mesophase asphalt. After passing through the pressure regulating valve 033, the mesophase asphalt enters the mesophase asphalt storage tank 034, where the small molecule byproducts are further decompressed and separated. The small molecule byproducts are condensed by the third condenser 036 and then collected in the small molecule byproduct collection tank 037. The second vacuum tank 038 and the second vacuum pump 039 provide negative pressure for the hydrogenation byproducts and the small molecule byproducts to accelerate the separation of the hydrogenation byproducts and the small molecule byproducts. The final asphalt is cooled by water or nitrogen from the bottom of the mesophase asphalt storage tank to obtain the mesophase asphalt 035.

[0041] The impurities of the mesophase asphalt are effectively removed during the preparation process of the mesophase asphalt. The obtained mesophase asphalt shows 100% wide-area streamline after detection by polarized fiber, still has 60% pyridine insoluble matter after being dissolved in pyridine, and the asphalt softening point is between 270 and 290°C.

[0042] The above description is the best embodiment based on the concept and working principle of the invention. The above embodiment should not be understood as limiting the protection scope of the present claims, and other implementations and combinations of implementations according to the concept of the present invention belong to the protection scope of the present invention.

Claims

1. A method for industrially continuously preparing mesophase pitch from coal tar pitch, characterized in that: The following steps are involved: S1. Refining of asphalt: medium-low temperature coal tar asphalt is used as raw material asphalt, the heated raw material asphalt is mixed with an asphalt solvent, dissolved, filtered, centrifuged to remove insoluble matter, and then distilled under reduced pressure to obtain refined asphalt and stored in a refined asphalt temporary storage tank with a constant temperature of 80°C to 120°C to keep the refined asphalt in a liquid state; S2. Asphalt hydrogenation: reacting the hydrogenation reagent and the refined asphalt flowing out of the refined asphalt temporary storage tank at a temperature of 300°C to 400°C and a pressure of 2MPa to 8MPa for 2 to 20h, and distilling off the solvent to obtain hydrogenated asphalt; S3. Preparation of mesophase by thermal polymerization of asphalt: The hydrogenated asphalt is reacted in an asphalt polymerization reactor at a temperature of 350°C to 500°C, a pressure of 0.2MPa to 2MPa and nitrogen bubbling for 4h to 42h to obtain the mesophase asphalt.

2. The method for industrially continuously preparing mesophase pitch from coal tar pitch according to claim 1, characterized in that: In step S1, the asphalt solvent is selected from one or a mixture of two or more of 230°C to 300°C tar fraction oil, 280°C to 360°C coal tar fraction oil, top circulating oil, quinoline, dichloromethane, and N,N-dimethylformamide.

3. The method for industrially continuously preparing mesophase pitch from coal tar pitch according to claim 1, characterized in that: In step S1, the raw asphalt and the asphalt solvent are mixed using a series-connected heatable static mixer with a heating device on the outer wall. The temperature in the series-connected heatable static mixer is between 100°C and 250°C, so that the raw asphalt is completely dissolved in the asphalt solvent. After filtering and settling through a 0.1 micron to 20 micron filter mesh in a hot filtration device, impurities are centrifuged at a centrifugal speed of 3000rpm to 6000rpm in a horizontal screw centrifuge, and then the asphalt solvent is separated in a scraped film evaporator to obtain the refined asphalt.

4. The method for industrially continuously preparing mesophase pitch from coal tar pitch according to claim 1, characterized in that: In step S2, the hydrogenation reagent and the refined asphalt are pressurized to 2MPa~10MPa, mixed and reacted in a two-stage hydrogenation reactor, wherein the temperature of the first stage hydrogenation reactor is 300℃~350℃, and the temperature of the second stage hydrogenation reactor is 350℃~400℃.

5. The method for industrially continuously preparing mesophase pitch from coal tar pitch according to claim 1, characterized in that: In step S2, the hydrogenation reagent is selected from one or a mixture of two or more of tetralin, decalin, and vacuum tower bottom product oil of coal tar hydrogenation, and the mass ratio of the refined asphalt to the hydrogenation reagent is 1:0.5~2.

6. The method for industrially continuously preparing mesophase pitch from coal tar pitch according to claim 1, characterized in that: In step S2, the hydrogenation reagent is selected from the vacuum tower bottom product oil of coal tar hydrogenation, or a mixed product of tetralin and the vacuum tower bottom product oil of coal tar hydrogenation in a mass ratio of 0.2 to 0.4:

1.

7. A system for industrially continuously preparing mesophase asphalt from coal tar pitch, characterized in that: The invention comprises an asphalt storage tank, a serially heated static mixer, a hot filter, a horizontal screw centrifuge, a scraping evaporator, a refined asphalt temporary storage tank, a heated static mixer, a first-stage hydrogenation reactor, a second-stage hydrogenation reactor, an evaporator, an asphalt polymerization reactor and an intermediate phase asphalt storage tank, which are sequentially fluid-connected. The system further comprises a solvent storage tank in fluid communication with the in-line heatable static mixer, and a hydrogenation reagent storage tank in fluid communication with the heatable static mixer via a hydrogenation reagent booster pump, wherein: The top of the scraped evaporator is connected to a first condenser, which is connected to a solvent collection tank, a first vacuum tank, and a first vacuum pump in sequence. The solvent storage tank is also connected to the solvent collection tank via a solvent recovery pump. The top of the evaporator is connected to a second condenser, and the second condenser is connected to a by-product collection tank. The top of the mesophase asphalt storage tank is connected to a third condenser, and the third condenser is connected to a small molecule by-product collection tank, a vacuum, a second vacuum tank and a second vacuum pump in sequence.

8. The system for industrially continuously preparing mesophase asphalt from coal tar pitch according to claim 7, characterized in that: A solvent metering pump is provided between the solvent storage tank and the serially heated static mixer. An asphalt metering pump is provided between the asphalt storage tank and the serially heated static mixer. An asphalt high-pressure pump is provided between the refined asphalt temporary storage tank and the heatable static mixer. An asphalt delivery pump is provided between the scraping evaporator and the refined asphalt temporary storage tank. A delivery pump is provided between the horizontal screw centrifuge and the scraped evaporator. A hydrogenated asphalt delivery pump is provided between the evaporator and the asphalt polymerization reactor.

9. The system for industrially continuously preparing mesophase pitch from coal tar pitch according to claim 7, characterized in that: The system further comprises a solvent heater electrically connected to the hot filtering device, the solvent storage tank and the solvent collecting tank.

10. The system for industrially continuously preparing mesophase asphalt from coal tar pitch according to claim 7, characterized in that the asphalt The existing pipelines are equipped with electric heating. The heating temperature before hydrogenation is 80℃~150℃, and the heating temperature after hydrogenation is 200℃~300℃.