High-strength wear-resistant copper alloy and preparation method thereof

Through the combination of laser directional energy deposition 3D printing technology and heat treatment, the problems of segregation and cracking in CuNiSn alloy preparation are solved, and the preparation of high-strength and wear-resistant copper alloys is realized, which simplifies the process flow and reduces costs and meets the bearings and high performance requirements for bushings.

CN118979169APending Publication Date: 2024-11-19SHAANXI HAOTE INNOVATIVE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411086299.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing CuNiSn alloy preparation process has problems such as segregation, cracking, complex process, high cost and low material utilization, especially in the production of bearings and bushings, which are difficult to meet the needs of high strength, high wear resistance and low cost.

Method used

Using a short process preparation method combining laser directional energy deposition 3D printing technology and heat treatment, the raw material powder mixed by ball mill is laser deposition in the 3D printing equipment, and a high-strength wear-resistant copper alloy is formed after heat treatment to achieve the uniformization of the material. and fine crystallization.

Benefits of technology

The short-process preparation of CuNiSn alloy is realized, with excellent material performance, simplified process flow, and reduced cost. It can prepare high-strength wear-resistant copper alloys at predetermined positions or surfaces of parts, improving the performance and material utilization of bearings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979169A_ABST
    Figure CN118979169A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength wear-resistant copper alloy and a preparation method thereof.The preparation method comprises the steps that a preset amount of copper raw materials, nickel raw materials, tin raw materials and strengthening phase raw materials are weighed and subjected to ball-milling mixing, and raw material powder obtained after ball-milling mixing is obtained; obtaining a base material and loading the base material into 3D printing equipment; the raw material powder obtained after ball milling and mixing is loaded into the 3D printing equipment for 3D printing, and a printed blank is obtained; and the printed blank is subjected to heat treatment, so that the high-strength wear-resistant copper alloy is formed on the surface of the base material. According to the preparation method of the high-strength wear-resistant copper alloy, short-process preparation of the nickel-copper alloy is achieved through the laser directional energy deposition 3D printing technology, the material performance is excellent, the composite structure design is adopted, the high-strength wear-resistant copper alloy can be prepared at the preset position or the preset surface of a part, and low cost and high performance are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonferrous metal additive manufacturing, and specifically relates to a high-strength and wear-resistant copper alloy and a preparation method thereof. Background Art

[0002] In the field of large-scale heavy-duty engineering machinery, bearings and sleeves play the role of transmitting energy and frequently rotating, so they are required to have high strength, high wear resistance, no seizure, high corrosion resistance and good self-lubrication. Nickel-copper alloy and beryllium-copper alloy are widely used in heavy-duty engineering machinery due to their high strength, wear resistance and corrosion resistance.

[0003] Since beryllium is toxic and harmful to human body and environment in the production process of beryllium copper alloy, it is gradually eliminated. Nickel copper alloy has excellent high strength and wear resistance, so it is used more and more. However, segregation is easy to occur in the smelting process of nickel copper alloy, and it is easy to crack during hot and cold deformation, which makes the preparation process of nickel copper alloy difficult and costly.

[0004] The invention patent with application number 202210858240.X discloses a method for preparing high-strength and wear-resistant CuNiSn alloy materials for bearing sleeves. It adopts the traditional smelting + deformation treatment process, which has a long process flow, is difficult to control the consistency of process quality, and has low material utilization. The invention patent with application number 202111524750.5 discloses a short-process heat treatment method for CuNiSn alloy bars. This method still uses casting first and then extrusion deformation to improve material properties. This method is difficult to solve the problems of material segregation, long repeated extrusion process flow, and long bar extrusion technology and equipment difficulties; and this method can only produce bars, and the sleeves need to be machined with bars, resulting in large material waste. The invention patent with application number 202310738385.0 discloses a Cu-Ni-Sn alloy with high aging stability and a preparation method thereof. The preparation method adds a third element in the smelting process as a fine grain strengthening effect, and there is no innovation in the preparation process.

[0005] The above patent applications still use traditional process methods in the preparation process of CuNiSn alloy. Although the performance is improved, the process flow is long, the preparation process is complicated and the cost is too high. Summary of the invention

[0006] In order to solve the above problems existing in the prior art, the present invention provides a high-strength wear-resistant copper alloy and a preparation method thereof. The technical problem to be solved by the present invention is achieved by the following technical solutions:

[0007] The present invention provides a method for preparing a high-strength wear-resistant copper alloy, comprising:

[0008] S1: weighing a predetermined amount of copper raw material, nickel raw material, tin raw material and reinforcing phase raw material and mixing them by ball milling to obtain raw material powder after ball milling;

[0009] S2: Obtaining a substrate and loading the substrate into a 3D printing device;

[0010] S3: loading the ball-milled mixed raw material powder into the 3D printing device for 3D printing to obtain a printed blank;

[0011] S4: heat treating the printed blank to form a high-strength and wear-resistant copper alloy on the surface of the substrate.

[0012] In one embodiment of the present invention, the S1 includes:

[0013] S1.1: Weigh a predetermined amount of copper raw material, nickel raw material, tin raw material and strengthening phase raw material;

[0014] S1.2: adding one or two of the copper raw material, the nickel raw material, the tin raw material and the strengthening phase raw material to a volatile solvent for mixing to obtain a mixed partial raw material, wherein 1 to 10 drops of the volatile solvent are added per kilogram of the raw material;

[0015] S1.3: The mixed part of the raw materials and the remaining raw materials are loaded into a mixer for ball milling to obtain raw material powder after ball milling, wherein the mass ratio of the grinding balls used for ball milling to the raw materials is 1:1 to 3:1, and the ball milling time is 1 to 5 hours.

[0016] In one embodiment of the present invention, the copper raw material is pure Cu powder, the nickel raw material is pure Ni powder or CuNi alloy powder, the tin raw material is pure Sn powder or CuSn alloy powder, and the strengthening phase raw material is a mixture of one or more of Cr, Si, Mn, V, Co, Cr2Nb, TaB2, CeB6, NaC, TiC or LaB6.

[0017] In one embodiment of the present invention, the particle sizes of the copper raw material, the nickel raw material and the tin raw material are all 20 to 200 microns, and the particle size of the strengthening phase raw material is 0.1 to 100 microns.

[0018] In one embodiment of the present invention, the volatile solvent is anhydrous ethanol, gasoline or hydrocarbon cleaning agent.

[0019] In one embodiment of the present invention, in the raw material powder after ball milling and mixing, the content of Ni element is 14-17wt%, the content of Sn element is 6-10wt%; the content of the strengthening phase raw material is 0.1-2wt%; and the rest is Cu element.

[0020] In one embodiment of the present invention, the substrate is steel, aluminum alloy or titanium alloy, and the shape of the substrate is plate-shaped, rod-shaped or ring-shaped.

[0021] In one embodiment of the present invention, S3 includes:

[0022] The ball-milled mixed raw material powder is loaded into a laser energy deposition 3D printer for 3D printing, so that the ball-milled mixed raw material powder is deposited on the surface to be processed of the substrate by laser, wherein the laser used is red light or blue light + red light laser, the power of the printing laser is 2 to 10 kW, the powder feeding speed is 10 to 100 g / min, the moving speed of the laser spot is 100 to 1000 mm / min, and the printing process is carried out under the protection of inert gas.

[0023] In one embodiment of the present invention, the S4 includes:

[0024] The printed blank is placed in a heat treatment device for heat treatment, wherein the heat treatment temperature is 360-450° C. and the heat preservation time is 3-5 hours.

[0025] Another aspect of the present invention provides a high-strength and wear-resistant copper alloy, which is prepared using the preparation method described in any one of the above embodiments.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The present invention provides a method for preparing a high-strength and wear-resistant copper alloy. The short-process preparation of the nickel-copper alloy is achieved by laser directed energy deposition 3D printing technology + heat treatment. The ultra-fast solidification of 3D printing ensures the homogenization and refinement of the component structure. The process is short and the material properties are excellent. In addition, a composite structure design is adopted, that is, a high-strength and wear-resistant copper alloy is prepared at a predetermined position or predetermined surface of a part, thereby achieving low cost and high performance of the bearing.

[0028] 2. The traditional production process of CuSnNi alloy is smelting-casting-forging-heat treatment-machining; the process flow is complicated, and the material structure uniformity is poor, and it is easy to crack during the production process; the CuNiSn prepared by the 3D printing technology of the present invention has a short production process, uniform structure, and high yield; it is difficult to add trace elements evenly in the traditional process, especially the ceramic phase cannot be added. The preparation method of the present invention can very well add trace elements (including ceramic phase) into the CuNiSn alloy, which plays a role in improving the material performance and can be evenly distributed.

[0029] 3. In the application of traditional process materials, they can only be made into a whole material, but in practice the useful parts are local. The preparation method of the present invention can be designed as a composite structure during the printing process, that is, a high-strength and wear-resistant copper alloy is prepared at a predetermined position or surface of a part, which can reduce product costs or achieve lightweight, while improving the copper alloy performance of the product or part working area.

[0030] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a flow chart of a method for preparing a high-strength and wear-resistant copper alloy provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0032] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, a high-strength wear-resistant copper alloy and a preparation method thereof proposed according to the present invention are described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0033] The above and other technical contents, features and effects of the present invention are clearly presented in the following detailed description of the specific implementation modes in conjunction with the accompanying drawings. Through the description of the specific implementation modes, the technical means and effects adopted by the present invention to achieve the predetermined purpose can be more deeply and specifically understood. However, the attached drawings are only for reference and explanation purposes and are not used to limit the technical solutions of the present invention.

[0034] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants are intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also other elements that are not explicitly listed. In the absence of more restrictions, the elements defined by the statement "including one..." do not exclude the existence of other identical elements in the article or device including the elements.

[0035] Embodiment 1

[0036] See also Figure 1 , Figure 1 1 is a flow chart of a method for preparing a high-strength wear-resistant copper alloy provided by an embodiment of the present invention. The preparation method comprises:

[0037] S1: weighing a predetermined amount of copper raw material, nickel raw material, tin raw material and reinforcing phase raw material and mixing them by ball milling to obtain raw material powder after ball milling.

[0038] In this embodiment, step S1 includes:

[0039] S1.1: Weigh a predetermined amount of copper raw material, nickel raw material, tin raw material and a small amount of strengthening phase raw material.

[0040] The copper raw material is pure Cu powder, the nickel raw material is pure Ni powder or CuNi alloy powder, the tin raw material is pure Sn powder or CuSn alloy powder, and the strengthening phase raw material is a mixture of one or more metal elements such as Cr, Si, Mn, V, Co or ceramic phases such as Cr2Nb, TaB2, CeB6, NaC, TiC or LaB6. In the strengthening phase raw material, Cr, Si, and Mn can be pure single powders or alloy powders such as CuNi, CuCr, and CuMn. The addition of the strengthening phase raw material can enhance the strength and wear resistance of the prepared copper alloy.

[0041] Preferably, the particle sizes of the copper raw material, the nickel raw material and the tin raw material are all 20 to 200 microns, and the particle size of the reinforcement phase raw material is 0.1 to 100 microns.

[0042] S1.2: Add one or two of the copper raw material, nickel raw material, tin raw material and strengthening phase raw material to a volatile solvent for mixing so that the powder has a certain wettability, and obtain a mixed partial raw material, wherein 1 to 10 drops of volatile solvent are added per kilogram of raw material.

[0043] For example, copper raw materials and nickel raw materials are added to a volatile solvent for mixing, and tin raw materials and reinforcing phase raw materials are added to a volatile solvent for mixing. The purpose is to wet part of the raw materials first to ensure more uniform mixing later.

[0044] In other embodiments of the present invention, three of the copper raw material, the nickel raw material, the tin raw material and the strengthening phase raw material may be added to the volatile solvent for mixing, and the types of raw materials mixed with the volatile solvent are not limited.

[0045] Preferably, the volatile solvent used is anhydrous ethanol, gasoline or hydrocarbon cleaning agent.

[0046] S1.3: Put the mixed part of the raw materials and the remaining raw materials that have not been mixed with the volatile solvent into a three-dimensional mixer for ball milling to obtain raw material powder after ball milling, wherein the mass ratio of the grinding balls used for ball milling to the raw materials is 1:1 to 3:1, and the ball milling time is 1 to 5 hours.

[0047] In this embodiment, in the raw material powder after ball milling and mixing, the content of Ni element is 14-17wt%, the content of Sn element is 6-10wt%; the content of the strengthening phase raw material is 0.1-2wt%; and the rest is Cu element.

[0048] S2: Obtain a substrate and load the substrate into a 3D printing device.

[0049] In one embodiment of the present invention, the substrate is made of high-strength steel, quenched and tempered steel, aluminum alloy or titanium alloy, and the substrate is in a plate, rod or ring shape, depending on the shape and material of the part to be processed or used. The 3D printing device is a laser energy deposition 3D printer.

[0050] The preparation method of the present invention adopts laser energy deposition 3D printing equipment to print parts on a substrate, and can directly shape the part size according to the use requirements, or print and composite on the working surface requiring high strength and wear resistance such as the surface of a bar or the inner wall of a tubular.

[0051] S3: The ball-milled mixed raw material powder is loaded into a 3D printing device for 3D printing to obtain a printed blank.

[0052] Specifically, the raw material powder after ball milling and mixing is loaded into a laser energy deposition 3D printer for 3D printing, so that the raw material powder after ball milling and mixing is deposited on the surface to be processed of the substrate by laser, wherein the laser used is a red light or a blue light + red light laser, the power of the printing laser is 2 to 10 kW, the powder feeding speed is 10 to 100 g / min, and the stable moving speed of the laser spot is 100 to 1000 mm / min. The 3D printing process has high productivity and can reach a production efficiency of 1 to 6 kg / h, which meets the requirements of industrial mass production. In addition, the printing process is carried out under the protection of inert gas, with an oxygen content of less than 500 ppm and a moisture content of less than 100 ppm, which can effectively reduce the oxidation of copper.

[0053] S4: The printed blank is heat treated to form a high-strength and wear-resistant copper alloy on the surface of the substrate.

[0054] Specifically, the printed blank is placed in a heat treatment device for heat treatment, wherein the heat treatment temperature is 360-450°C and the heat preservation time is 3-5 hours. After the heat treatment, the blank is finely processed to obtain a finished part with high strength and excellent wear resistance.

[0055] Embodiment 2

[0056] On the basis of the above-mentioned embodiment 1, this embodiment provides a specific preparation method of CuNi16Sn8-0.2LaB6 copper alloy, comprising the following steps:

[0057] Step 1: Weigh a predetermined amount of copper raw material, nickel raw material, tin raw material and reinforcing phase raw material and mix them by ball milling to obtain raw material powder after ball milling.

[0058] In this embodiment, step 1 includes:

[0059] Step 1.1: Weigh a predetermined amount of copper raw material, nickel raw material, tin raw material and a small amount of strengthening phase raw material. The copper raw material is pure Cu powder, the nickel raw material is pure Ni powder, the tin raw material is CuSn alloy powder, and the strengthening phase raw material is LaB6 ceramic phase powder.

[0060] Step 1.2: Add one or two of the copper raw material, nickel raw material, copper-tin raw material and LaB6 strengthening phase raw material to a volatile solvent and mix them so that the powder has a certain wettability to obtain a mixed partial raw material, wherein 1 to 10 drops of volatile solvent are added per kilogram of raw material.

[0061] For example, pure Cu powder and pure Ni powder are added to a volatile solvent for mixing, and then copper tin powder and LaB6 powder are added to a volatile solvent for mixing, the purpose is to first wet a part of the raw materials to ensure that the subsequent mixing can be more uniform. The volatile solvent used is anhydrous ethanol, gasoline or hydrocarbon cleaning agent.

[0062] Step 1.3: Put the mixed part of the raw materials and the remaining raw materials that have not been mixed with the volatile solvent into a three-dimensional mixer for ball milling to obtain raw material powder after ball milling, wherein the mass ratio of the grinding balls used for ball milling to the raw materials is 2:1 to 3:1, and the ball milling time is 1 to 5 hours.

[0063] In this embodiment, in the raw material powder after ball milling and mixing, the Ni content is 15.5wt%, the Sn content is 8.2wt%; the content of the strengthening phase LaB6 is 0.2wt%; and the rest is Cu powder.

[0064] Step 2: Obtain the substrate and load the substrate into the 3D printing device.

[0065] In this embodiment, the substrate is Q45 high-strength steel and is in the shape of a rod. The 3D printing device is a laser energy deposition 3D printer.

[0066] The preparation method of the present invention adopts laser energy deposition 3D printing equipment to print parts on a substrate. The required size and shape can be directly formed on the surface of the rod according to the use requirements, and the high-strength and wear-resistant structural printing composite is required in the preparation working area.

[0067] Step 3: Load the ball-milled mixed raw material powder into a 3D printing device for 3D printing to obtain a printed blank.

[0068] Specifically, the raw material powder after ball milling and mixing is loaded into a laser energy deposition 3D printer for 3D printing, so that the raw material powder after ball milling and mixing is deposited on the surface to be processed of the substrate by laser, wherein the laser used is a red laser, the power of the printing laser is 2.8kw, the powder feeding speed is 55g / min, the moving speed of the laser spot is 300mm / min, and the printing efficiency can reach a production efficiency of 3.3kg / h, which meets the requirements of industrial mass production. In addition, the printing process is carried out under the protection of inert gas, the oxygen content is less than 500ppm, and the water content is less than 100ppm, which can effectively reduce the oxidation of copper.

[0069] Step 4: The printed blank is heat treated to form a high-strength and wear-resistant copper alloy on the surface of the substrate.

[0070] Specifically, the printed blank is placed in a heat treatment device for heat treatment, wherein the heat treatment temperature is 420°C and the heat preservation time is 4 hours. After the heat treatment, the blank is finely processed to obtain a finished part with high strength and excellent wear resistance.

[0071] Another aspect of the present invention provides a high-strength and wear-resistant copper alloy, which is prepared using the preparation method in the above embodiment. Please refer to Table 1, which shows the properties of different types of copper alloys prepared using the method of this embodiment, wherein the tensile strength of the CuNi15Sn8 alloy prepared using the preparation method of the present invention is about 10% higher than that of the traditional method, and the tensile strength of the CuNi15Sn8Cr1 alloy prepared using the preparation method of the present invention is about 10% higher than that of the traditional method. The preparation method of the present invention can be used to prepare the CuNi16Sn8-0.2LaB6 copper alloy that cannot be synthesized by the current traditional method, and the CuNi16Sn8-0.2LaB6 copper alloy prepared using the preparation method of the present invention has beneficial strength and wear resistance.

[0072] Table 1. Properties of different types of copper alloys prepared by the method of this embodiment

[0073]

[0074] The preparation method of the present invention is to 3D print a certain thickness of CuNiSn alloy on a substrate such as high-strength copper or high-strength aluminum by high-speed laser energy deposition, thereby realizing a fast and short process to prepare high-strength and wear-resistant copper alloy composite bearings and sleeves. The production process is simple, the material utilization rate is high, and the prepared material has excellent performance.

[0075] In summary, the present invention provides a method for preparing high-strength and wear-resistant copper alloy, which realizes the short-process preparation of nickel-copper alloy by laser directed energy deposition 3D printing technology + heat treatment. The ultra-fast solidification of 3D printing ensures the homogenization and refinement of the composition structure, the process flow is short, the material properties are excellent, and a composite structure design is adopted, that is, the high-strength and wear-resistant copper alloy is prepared at a predetermined position or predetermined surface of the part, thereby achieving low cost and high performance of the bearing.

[0076] The traditional production process of CuSnNi alloy is smelting-casting-forging-heat treatment-machining; the process flow is complicated, and the material organization uniformity is poor, and it is easy to crack during the production process; the CuNiSn prepared by the 3D printing technology of the present invention has a short production process, uniform organization, and high yield rate; it is difficult to add trace elements evenly in the traditional process, especially the ceramic phase cannot be added. The preparation method of the present invention can very well add trace elements (including ceramic phase) to the CuNiSn alloy, which plays a role in improving the material performance and can be evenly distributed. In the application, the traditional process material can only be made into a whole material, but the useful part is local in practice. The preparation method of the present invention can be designed as a composite structure during the printing process, that is, a high-strength and wear-resistant copper alloy is prepared at a predetermined position or predetermined surface of the part, which can reduce the product cost or achieve lightweight, while improving the copper alloy performance of the product or part working area.

[0077] In the several embodiments provided by the present invention, it should be understood that the apparatus and method disclosed by the present invention can be implemented in other ways. For example, the apparatus embodiments described above are only illustrative, for example, the division of the modules is only a logical function division, and there may be other division methods in actual implementation, for example, multiple modules or components can be combined or integrated into another system, or some features can be ignored or not executed.

[0078] In addition, each functional module in each embodiment of the present invention may be integrated into one processing module, or each module may exist physically separately, or two or more modules may be integrated into one module. The above-mentioned integrated module may be implemented in the form of hardware or in the form of hardware plus software functional modules.

[0079] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A method for preparing a high-strength wear-resistant copper alloy, characterized in that: include: S1: weighing a predetermined amount of copper raw material, nickel raw material, tin raw material and reinforcing phase raw material and mixing them by ball milling to obtain raw material powder after ball milling; S2: Obtaining a substrate and loading the substrate into a 3D printing device; S3: loading the ball-milled mixed raw material powder into the 3D printing device for 3D printing to obtain a printed blank; S4: heat treating the printed blank to form a high-strength and wear-resistant copper alloy on the surface of the substrate.

2. The method for preparing a high-strength wear-resistant copper alloy according to claim 1, characterized in that: The S1 includes: S1.1: Weigh a predetermined amount of copper raw material, nickel raw material, tin raw material and strengthening phase raw material; S1.2: adding one or two of the copper raw material, the nickel raw material, the tin raw material and the strengthening phase raw material to a volatile solvent for mixing to obtain a mixed partial raw material, wherein 1 to 10 drops of the volatile solvent are added per kilogram of the raw material; S1.3: The mixed part of the raw materials and the remaining raw materials are loaded into a mixer for ball milling to obtain raw material powder after ball milling, wherein the mass ratio of the grinding balls used for ball milling to the raw materials is 1:1 to 3:1, and the ball milling time is 1 to 5 hours.

3. The method for preparing a high-strength wear-resistant copper alloy according to claim 1, characterized in that: The copper raw material is pure Cu powder, the nickel raw material is pure Ni powder or CuNi alloy powder, the tin raw material is pure Sn powder or CuSn alloy powder, and the strengthening phase raw material is a mixture of one or more of Cr, Si, Mn, V, Co, Cr2Nb, TaB2, CeB6, NaC, TiC or LaB6.

4. The method for preparing a high-strength wear-resistant copper alloy according to claim 1, characterized in that: The particle sizes of the copper raw material, the nickel raw material and the tin raw material are all 20 to 200 microns, and the particle size of the strengthening phase raw material is 0.1 to 100 microns.

5. The method for preparing a high-strength wear-resistant copper alloy according to claim 2, characterized in that: The volatile solvent is anhydrous ethanol, gasoline or hydrocarbon cleaning agent.

6. The method for preparing a high-strength wear-resistant copper alloy according to claim 2, characterized in that: In the raw material powder after ball milling and mixing, the content of Ni element is 14-17wt%, the content of Sn element is 6-10wt%; the content of the strengthening phase raw material is 0.1-2wt%; and the rest is Cu element.

7. The method for preparing a high-strength wear-resistant copper alloy according to claim 1, characterized in that: The substrate is steel, aluminum alloy or titanium alloy, and the shape of the substrate is plate-shaped, rod-shaped or ring-shaped.

8. The method for preparing a high-strength wear-resistant copper alloy according to claim 1, characterized in that: The S3 includes: The ball-milled mixed raw material powder is loaded into a laser energy deposition 3D printer for 3D printing, so that the ball-milled mixed raw material powder is deposited on the surface to be processed of the substrate by laser, wherein the laser used is red light or blue light + red light laser, the power of the printing laser is 2 to 10 kW, the powder feeding speed is 10 to 100 g / min, the moving speed of the laser spot is 100 to 1000 mm / min, and the printing process is carried out under the protection of inert gas.

9. The method for preparing a high-strength wear-resistant copper alloy according to claim 2, characterized in that: The S4 includes: The printed blank is placed in a heat treatment device for heat treatment, wherein the heat treatment temperature is 360-450° C. and the heat preservation time is 3-5 hours.

10. A high-strength wear-resistant copper alloy, characterized in that: The method is prepared by the method according to any one of claims 1 to 9.