Pipeline and preparation method and application thereof

By covering the protective layer on the surface of the zirconium or zirconium alloy tube blank and performing multiple hydrogen permeation treatments, the problem of insufficient uniformity of sample length and hydrogen content in the prior art was solved, and long pipe samples suitable for fatigue tests were prepared to achieve Efficient performance characterization.

CN118979175APending Publication Date: 2024-11-19STATE NUCLEAR ZIRCONIUM & HAFNIUM PHYSICAL & CHEMICAL TESTING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411058889.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art is difficult to prepare a fatigue sample of nuclear-grade zirconium alloy thin-walled pipe with a length greater than 30 mm, and the surface of the sample is oxidized and the fatigue, creep, and high-temperature oxidation performance cannot be characterized.

Method used

A pipeline preparation method is adopted, including covering the surface of the zirconium or zirconium alloy tube blank with multiple layers of protective layer, performing two hydrogen permeation treatments, and pickling and water washing after removing the protective layer to ensure uniformity of hydrogen content and surface cleaning.

Benefits of technology

Nuclear-grade zirconium or zirconium alloy pipelines with a length of 250-350mm, hydrogen content of 0.0600-0.1200%, and uniformity are prepared. They are suitable for fatigue tests under simulated working conditions and efficiently inspect the performance of nuclear-grade zirconium and zirconium alloy thin-walled pipes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979175A_ABST
    Figure CN118979175A_ABST
Patent Text Reader

Abstract

The invention provides a pipeline and a preparation method and application thereof, the pipeline comprises a body, and the body is of a tubular structure; the length of the body ranges from 250 mm to 350 mm, and the wall thickness of the body ranges from 0.3 mm to 0.6 mm. The body is made of zirconium or / and zirconium alloy; the mass content of hydrogen in the body is 0.0600-0.1200%, and the deviation of the mass content of hydrogen in each part of the body is less than 0.0120%. The pipeline disclosed by the invention is large in length, high in hydrogen content and good in uniformity, and can be widely applied to a fatigue test under a certain hydrogen absorption amount condition under a simulated working condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of rare metal material analysis and detection, and in particular to a pipeline and a preparation method and application thereof. Background Art

[0002] Zirconium has a very low thermal neutron absorption cross section, high hardness, ductility and corrosion resistance. The main use of zirconium alloys is in the field of nuclear technology, such as cladding tubes, instrument tubes, guide tubes, grid ring tubes, etc. in fuel assemblies in nuclear reactors.

[0003] Fuel assemblies are the core components of nuclear reactors, and their performance directly affects the reliability, safety and economy of nuclear power plants. As an important structure of fuel assemblies, the spacer grid should ensure that the reactor has good thermal and hydraulic performance, sufficient strength and rigidity during its service life. In addition to positioning, supporting and guiding, its functions also need to reasonably distribute flow and limit the vibration level of fuel rods. Therefore, through static tests and analysis, the mechanical parameters of the spacer grid are studied to examine whether its overall rigidity and strength meet the design requirements. Under actual operating conditions, fuel assemblies are exposed to harsh environments such as high temperature, high pressure and irradiation for a long time. With the increase of fuel consumption, the spring sheets and rigid convexities on the spacer grid may become loose due to irradiation growth and creep, resulting in different degrees of changes in the mechanical performance parameters of the grid, which will have a significant impact on the modal parameters of the fuel rods and further affect the service life of the fuel assembly. Therefore, fatigue tests under certain hydrogen absorption conditions under simulated working conditions are an important test to test the performance of nuclear-grade zirconium and zirconium alloy thin-walled pipes. In related research, there are quantitative hydrogen content samples of nuclear-grade zirconium alloy thin-walled tubes with a length of less than 30 mm, but the samples have the following defects: the surface is oxidized after hydrogen permeation, and the sample length is too short to characterize fatigue, creep, high-temperature oxidation and other performance. Therefore, it is urgent to develop a longer (length greater than or equal to 250 mm) nuclear-grade zirconium alloy thin-walled tube quantitative hydrogen content fatigue sample and its preparation method, so that it has a higher hydrogen content and hydrogen content uniformity. Summary of the invention

[0004] In view of this, one object of the present application is to provide a pipeline with a large length, a high hydrogen content and good uniformity, which can be widely used in fatigue tests under certain hydrogen absorption conditions under simulated working conditions.

[0005] Another object of the present application is to provide a method for preparing a pipeline.

[0006] Yet another object of the present application relates to the use of pipelines.

[0007] To achieve the above-mentioned objectives, the first aspect of the present application proposes a pipe, comprising a body, which is a tubular structure; the length of the body is 250-350 mm, and the wall thickness of the body is 0.3-0.6 mm; the material of the body includes zirconium and / or zirconium alloy; the mass content of hydrogen in the body is 0.0600-0.1200%, and the mass content deviation of hydrogen in various parts of the body is less than 0.0120%.

[0008] In some embodiments, the body is made of nuclear grade zirconium and / or nuclear grade zirconium alloy.

[0009] In some embodiments, a ratio of an outer diameter of the body to a wall thickness of the body is greater than 16 and less than 20.

[0010] A second embodiment of the present application provides a method for preparing a pipeline, comprising:

[0011] At least two first protective layers that allow hydrogen to permeate are coated and fixed on the outer surface of the main tube blank;

[0012] At least one second protective layer that allows hydrogen to permeate is coated and fixed at a middle position of the outer surface of the first protective layer as the outermost layer to obtain a coated main body tube blank;

[0013] The coated main tube blank is subjected to a first hydrogenation to obtain a first intermediate product;

[0014] removing the first protective layer and the second protective layer from the first intermediate product, and then pickling, washing with water, and drying the product to obtain a second intermediate product;

[0015] The second intermediate product is subjected to a second hydrogenation to obtain the main body.

[0016] In some embodiments, the first protective layer and the second protective layer both include at least one of tin foil and aluminum foil.

[0017] In some embodiments, the first protective layer and the second protective layer are fixed by bonding at the joints along the axial direction of the main tube billet, between the first protective layer and the outer surface of the main tube billet, between two adjacent first protective layers, and between the second protective layer and the outer surface of the outermost first protective layer.

[0018] In some embodiments, the length, wall thickness, material, and ratio of outer diameter to wall thickness of the main body tube are the same as those of the main body; the mass content of hydrogen in the main body tube is less than 15ppm, and the mass content deviation of hydrogen in various parts of the main body tube is 10-20%.

[0019] In some embodiments, the thickness of the first protective layer and the second protective layer are both 0.35-0.5 mm.

[0020] In some embodiments, the second protective layer has a first end and a second end, the main tube blank has a third end and a fourth end, the third end is adjacent to the first end, the fourth end is adjacent to the second end, and the spacing between the first end and the third end and the spacing between the second end and the fourth end are both 11-20% of the length of the main tube blank.

[0021] In some embodiments, the first hydrogenation and the second hydrogenation both include introducing flowing hydrogen into the body tube.

[0022] In some embodiments, the hydrogen flow rate of the first hydrogenation is 25-50 ml / min.

[0023] In some embodiments, the temperature of the first hydrogenation is 380-440°C.

[0024] In some embodiments, the first hydrogenation time is 4-6 hours.

[0025] In some embodiments, the hydrogen flow rate of the second hydrogenation is 25-50 ml / min.

[0026] In some embodiments, the temperature of the second hydrogenation is 380-440°C.

[0027] In some embodiments, the second hydrogenation time is 3-5 hours.

[0028] In some embodiments, the method for preparing the pipe further comprises the step of pretreating the body tube before coating and fixing at least two first protective layers that allow hydrogen to permeate onto the outer surface of the body tube.

[0029] In some embodiments, the pretreatment comprises:

[0030] The main tube blank is degreased, washed and dried; the washing method includes at least one of water washing, acid washing and ultrasonic cleaning.

[0031] In some embodiments, the method for preparing the pipeline further includes a step of performing a first temperature reduction after the first hydrogen permeation.

[0032] In some embodiments, the first cooling rate is less than 3°C / min.

[0033] In some embodiments, the method for preparing the pipeline further comprises a second cooling step after the second hydrogenation.

[0034] In some embodiments, the second temperature reduction rate is less than 3°C / min.

[0035] The embodiments of the third aspect of the present application relate to the application of the pipeline described in the present application or the pipeline prepared by the pipeline preparation method described in the present application in fatigue tests, creep tests, high-temperature oxidation tests, etc.

[0036] The pipeline described in this application can at least bring the following beneficial effects:

[0037] 1. The pipeline has a large length, high hydrogen content and good uniformity, and can be widely used in fatigue tests under simulated working conditions with a certain amount of hydrogen absorption.

[0038] 2. When the material of the body is nuclear grade zirconium or / and nuclear grade zirconium alloy, fatigue testing can effectively test the performance of nuclear grade zirconium and zirconium alloy thin-walled pipes.

[0039] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings.

[0041] in:

[0042] Figure 1 The present invention is a flowchart of a method for preparing a pipeline according to an exemplary embodiment of the present application.

[0043] Figure 2 This is a diagram (cross-sectional view) showing the relative position relationship between the first protective layer and the second protective layer in a method for preparing a pipeline according to an exemplary embodiment of the present application.

[0044] Reference numerals:

[0045] 1-first protective layer; 2-second protective layer; 201-first end; 202-second end; 3-main tube blank; 301-third end; 302-fourth end. DETAILED DESCRIPTION

[0046] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, but cannot be understood as limiting the present application.

[0047] In this application, the disclosure of numerical ranges includes all values ​​within the entire range and the disclosure of further subdivided ranges, including the endpoints and sub-ranges given in these ranges.

[0048] In this application, the raw materials, equipment, etc. involved, unless otherwise specified, are all raw materials and equipment that can be made through commercial channels or known methods; the methods involved, unless otherwise specified, are all conventional methods.

[0049] <Pipeline>

[0050] The pipe of the embodiment of the present application includes a body, which is a tubular structure. The length of the body is more than 250 mm, and the wall thickness of the body is 0.3-0.6 mm; the material of the body includes zirconium and / or zirconium alloy; the mass content of hydrogen in the body is 0.0600-0.1200%, and the mass content deviation of hydrogen in various parts of the body is less than 0.0120%.

[0051] Exemplarily, the length of the body is 250-350 mm, including but not limited to 250 mm, 280 mm, 300 mm, 310 mm, 320 mm, 330 mm, 340 mm or 350 mm, etc.

[0052] Exemplarily, the wall thickness of the body includes but is not limited to 0.3 mm, 0.4 mm, 0.5 mm, 0.57 mm or 0.6, etc.

[0053] Exemplarily, the mass content of hydrogen in the body includes but is not limited to 0.0600%, 0.0700%, 0.0800%, 0.0900%, 0.1000%, 0.1100% or 0.1200%. The mass content of hydrogen in the body is 0.0600-0.1200%, which can simulate the effect of hydrogen content after hydrogen absorption under different power conditions in a nuclear reactor. The hydrogen content in this range conforms to the actual working conditions; if it is less than 0.0600%, the nuclear reactor absorbs less than 0.0600% hydrogen under different power conditions, the pipe is not easy to fail, and research and testing are not convenient for detecting the material limit design capacity; if it is greater than 0.1200%, the hydrogen content is too high, the hydride phase is a brittle phase, the strength of the pipe itself is sharply reduced, and the test loses practical significance.

[0054] In the embodiments of the present application, the deviation of the mass content of hydrogen in various parts of the body is less than 0.0120%, and the hydrogen is evenly distributed. Specifically, in the reactor, the pipe is subjected to a high temperature and high pressure working environment. The pipe absorbs hydrogen due to the high temperature and high pressure, which causes the hydrogen to be evenly distributed in the area inside the pipe. Mechanical analysis is performed within the deviation of 0.0120%, and it can be considered that the hydrogen is evenly distributed, and the performance can be characterized normally. If the mass content deviation of hydrogen in various parts of the body is above 0.0120%, the hydrogen distribution is uneven, resulting in excessive local hydrogen content. Because the hydride phase is a brittle phase, excessive concentration directly reduces the strength of the part, and subsequent performance characterization cannot be achieved.

[0055] In some embodiments, the mass content deviation of hydrogen in various parts of the body is less than 0.0110%, further less than 0.0100%, and further less than 0.0090%.

[0056] In some embodiments, the body is made of nuclear grade zirconium.

[0057] In other embodiments, the body is made of nuclear grade zirconium alloy.

[0058] In some other embodiments, the body is made of nuclear grade zirconium and zirconium alloys.

[0059] As an optional example, the nuclear-grade zirconium satisfies: a zirconium alloy having a hafnium content of less than 0.0050 wt %.

[0060] As an optional example, the nuclear-grade zirconium alloy includes the following components in mass percentage: Sn: 1.2-1.7%, Fe: 0.07-0.30%, Nb: <3.0%, etc.

[0061] In some embodiments, the body is a thin-walled tube.

[0062] As an optional example, the ratio of the outer diameter of the body to the wall thickness of the body is greater than 16 and less than 20.

[0063] Exemplarily, the ratio of the outer diameter of the body to the wall thickness of the body includes but is not limited to 16, 17, 18, 19 or 20, etc.

[0064] It should be noted that the pipe of the embodiment of the present application may include, in addition to the body, a Cr coating, etc. Exemplarily, the Cr coating is provided on the outer surface of the body.

[0065] As an alternative example, a pipeline consists of an ontology.

[0066] The pipeline of the embodiment of the present application can at least bring the following beneficial effects:

[0067] 1. The pipeline has a large length, high hydrogen content and good uniformity, and can be widely used in fatigue tests under simulated working conditions with a certain amount of hydrogen absorption.

[0068] 2. When the material of the body is nuclear grade zirconium or / and nuclear grade zirconium alloy, fatigue testing can effectively test the performance of nuclear grade zirconium and zirconium alloy thin-walled pipes.

[0069] <Method of preparing pipe>

[0070] The method for preparing the pipe of the embodiment of the present application can be used for preparing the pipe of the embodiment of the present application.

[0071] The method for preparing a pipeline in an embodiment of the present application comprises the following steps:

[0072] S101, coating and fixing at least two layers of first protective layers 1 (such as Figure 2 shown).

[0073] It should be noted that, except for the hydrogen mass content and the hydrogen mass content deviation of each part, the main tube blank in the embodiment of the present application and the main body in the pipe in the aforementioned embodiment of the present application are the same in other aspects (length, wall thickness, material, ratio of outer diameter to wall thickness).

[0074] Exemplarily, the mass content of hydrogen in the main tube is less than 15ppm, and the mass content of hydrogen in various parts of the main tube has a deviation of more than 2%, such as 10-20%, including but not limited to 10%, 12.5%, 15%, 17.5% or 20%.

[0075] As an optional example, the main tube blank is a nuclear-grade zirconium and zirconium alloy thin-walled tube that meets the requirements, wherein the chemical composition and physical and chemical properties meet the technical requirements of nuclear-grade zirconium and zirconium alloy thin-walled tube products, and the length is greater than or equal to 250 mm.

[0076] In some embodiments, Figure 1 As shown, the method for preparing the pipe further comprises the step of pretreating the body tube before coating and fixing at least two first protective layers that allow hydrogen to permeate on the outer surface of the body tube.

[0077] In the embodiments of the present application, the role of the pretreatment is to remove impurities and oxide layers of the main tube embryo, wherein the impurities include oxide films, oil stains, water stains, etc.

[0078] In some embodiments, the pretreatment includes: degreasing, washing and drying the bulk tube.

[0079] Exemplary degreasing method is: acetone soaking.

[0080] In some embodiments, the washing method includes but is not limited to at least one of water washing, acid washing, ultrasonic cleaning, etc.

[0081] As an optional example, washing includes sequentially washing with water, multiple times (more than 2 times) of acid washing, washing with water, and ultrasonic cleaning.

[0082] Exemplarily, in the pretreatment, the pickling acid includes but is not limited to a mixed pickling solution of hydrofluoric acid, nitric acid, and water.

[0083] Exemplarily, the mass concentration of hydrofluoric acid is above 40 wt %, and the concentration of nitric acid is 65-68 wt %.

[0084] Exemplarily, the cleaning agent used in ultrasonic cleaning includes but is not limited to at least one of a neutral cleaning agent or anhydrous ethanol.

[0085] Exemplarily, in the pretreatment, the drying methods include oven drying, air drying, spray drying, etc.

[0086] In some embodiments, the first protective layer includes but is not limited to at least one of tin foil, aluminum foil, and the like.

[0087] As an optional example, the first protective layer is tin foil.

[0088] In some embodiments, the joints of the first protective layer along the axial direction of the main tube billet, between the first protective layer and the outer surface of the main tube billet, and between two adjacent first protective layers are fixed by bonding.

[0089] Exemplarily, the above-mentioned bonding uses a high temperature resistant (eg, 450-600°C) tape, such as a 450°C resistant tape, a 500°C resistant tape, a 550°C resistant tape, or a 600°C resistant tape.

[0090] Exemplarily, the first protective layer and the outer surface of the main tube blank and two adjacent first protective layers are fixed by multi-point bonding.

[0091] In some embodiments, the thickness of the first protective layer is 0.35-0.5 mm, including but not limited to 0.35 mm, 0.40 mm, 0.45 mm or 0.5 mm.

[0092] In some embodiments, the number of layers of the first protective layer is 2-4 layers, including but not limited to 2 layers, 3 layers or 4 layers, etc.

[0093] It should be noted that, in the embodiments of the present application, multiple layers of the first protective layer are stacked on the outer surface of the main tube blank and completely cover the outer surface of the main tube blank.

[0094] As an optional example, the number of layers of the first protective layer is 2.

[0095] S102, at least one second protective layer 2 (such as Figure 2 As shown), a coated body tube blank is obtained.

[0096] In the embodiments of the present application, the outermost first protective layer refers to the first protective layer which is farthest from the main tube blank.

[0097] In some embodiments, the second protective layer includes at least one of tin foil, aluminum foil, and the like.

[0098] As an optional example, the second protective layer is tin foil.

[0099] In some embodiments, the joint of the second protective layer along the axial direction of the main tube blank and the outer surface of the second protective layer and the outermost first protective layer are fixed by bonding.

[0100] In the embodiments of the present application, the joint refers to the interface where the two ends of the aluminum foil are butt-jointed along the axial direction of the main tube blank when the outer surface of the main tube blank or the outer surface of the first protective layer is coated with tin foil or the like.

[0101] Exemplarily, the second protective layer is fixed to the outer surface of the outermost first protective layer by means of multi-point bonding.

[0102] In some embodiments, the thickness of the second protective layer is 0.35-0.5 mm, including but not limited to 0.35 mm, 0.40 mm, 0.45 mm or 0.5 mm, etc.

[0103] In some embodiments, the number of layers of the second protective layer is 1-2 layers, including but not limited to 1 layer or 2 layers.

[0104] In some embodiments, Figure 2 As shown, the second protective layer 2 has a first end 201 and a second end 202, the main tube blank 3 has a third end 301 and a fourth end 302, the third end 301 is adjacent to the first end 201, the fourth end 302 is adjacent to the second end 201, and the spacing between the first end 201 and the third end 301, and the spacing between the second end 202 and the fourth end 302 are both 11-20% of the length of the main tube blank 3, including but not limited to 11%, 12.5%, 15%, 17.5% or 20%, etc.

[0105] As an optional example, the number of layers of the second protection layer is 1.

[0106] S103, performing a first hydrogen permeation on the coated main tube obtained in step S102 to obtain a first intermediate product.

[0107] In some embodiments, the first hydrogen impregnation includes introducing flowing hydrogen gas into the bulk tube.

[0108] Illustratively, during the first hydrogenation process, hydrogen comes from the hydrogenation furnace and has a purity of 99.9-99.999wt%, including but not limited to 99.9wt%, 99.95wt%, 99.99wt% or 99.999wt%.

[0109] In some embodiments, the hydrogen flow rate of the first hydrogenation is 25-50 ml / min, including but not limited to 25 ml / min, 35 ml / min, 45 ml / min or 50 ml / min.

[0110] In some embodiments, the temperature of the first hydrogenation is 380-440°C, including but not limited to 380°C, 390°C, 400°C, 410°C, 420°C, 430°C or 440°C.

[0111] In some embodiments, the first hydrogen permeation time is 4-6 hours, including but not limited to 4 hours, 4.5 hours, 5 hours, 5.5 hours or 6 hours.

[0112] In some embodiments, Figure 1 As shown, the method for preparing the pipeline further includes a first temperature reduction step after the first hydrogenation.

[0113] In some embodiments, the first cooling rate is less than 3°C / min. In the embodiment of the present application, the first cooling rate is less than 3°C / min. The cooling rate is slow, which can achieve the homogenization of hydrogen in the pipe and make the hydrogen distribution more uniform; if it is above 3°C / min, the cooling rate is too fast, which will cause the hydrogen to be concentrated at the grain boundaries, stress concentration and other locations, and the homogenization effect will be reduced.

[0114] S104, removing the first protective layer and the second protective layer from the first intermediate product obtained in step S103, pickling, washing with water, and drying to obtain a second intermediate product.

[0115] It should be noted that the first protective layer in step S104 refers to all first protective layers, and the second protective layer refers to all second protective layers. If the layers are bonded by high-temperature resistant tape, this also includes removing the high-temperature resistant tape used for bonding. That is, all the coating materials of the first intermediate product obtained in step S103 are removed.

[0116] In the embodiment of the present application, the first intermediate product obtained in step S103 is pickled, washed with water, and dried after removing the first protective layer and the second protective layer, in order to remove the oxide layer produced by the first hydrogen permeation, because the oxide layer is relatively dense and affects the second hydrogen permeation.

[0117] In some embodiments, the acid used for pickling in step S104 includes but is not limited to a mixed acid solution of hydrofluoric acid, nitric acid and water.

[0118] Exemplarily, the mass concentration of hydrofluoric acid is above 40 wt %, and the concentration of nitric acid is 65-68 wt %.

[0119] In some embodiments, the drying method in step S104 includes oven drying, natural air drying, spray drying, etc.

[0120] S105, subjecting the second intermediate product obtained in step S104 to a second hydrogenation, to obtain a main body.

[0121] In some embodiments, the second hydrogen impregnation includes introducing flowing hydrogen gas into the bulk tube.

[0122] Illustratively, during the second hydrogenation process, hydrogen comes from the hydrogenation furnace and has a purity of 99.9-99.999wt%, including but not limited to 99.9wt%, 99.95wt%, 99.99wt% or 99.999wt%.

[0123] In some embodiments, the hydrogen flow rate of the second hydrogenation is 25-50 ml / min, including but not limited to 25 ml / min, 35 ml / min, 45 ml / min or 50 ml / min.

[0124] In some embodiments, the temperature of the second hydrogenation is 380-440°C, including but not limited to 380°C, 390°C, 400°C, 410°C, 420°C, 430°C or 440°C.

[0125] In some embodiments, the second hydrogenation time is 3-5 hours, including but not limited to 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours.

[0126] In some embodiments, Figure 1 As shown, the method for preparing the pipeline further includes a second cooling step after the second hydrogenation.

[0127] In some embodiments, the second cooling rate is less than 3°C / min. In the embodiment of the present application, the second cooling rate is less than 3°C / min. The cooling rate is slow, which can achieve the homogenization of hydrogen in the pipe and make the hydrogen distribution more uniform); if it is above 3°C / min, the cooling rate is too fast, which will cause the hydrogen to be concentrated at the grain boundaries, stress concentration and other locations, and the homogenization effect cannot be achieved.

[0128] In some embodiments, the second hydrogenation and the first hydrogenation are both performed in a hydrogenation furnace.

[0129] It should be noted that in the embodiments of the present application, the temperatures of the first hydrogenation and the second hydrogenation can be the same or different; the flow rates of hydrogen gas in the first hydrogenation and the second hydrogenation can be the same or different; the rate of the first cooling and the rate of the second cooling can be the same or different.

[0130] The method for preparing the pipe of the embodiment of the present application, in addition to the beneficial effects of the pipe of the embodiment of the present application, can also bring at least the following beneficial effects:

[0131] The preparation method uses easily available tin foil / aluminum foil to coat the pipe surface in multiple layers by adhesion, thereby controlling the uniformity and diffusion rate of hydrogen diffusion, and meeting the requirements of subsequent tests for uniform hydrogen content of samples. Compared with the prior art, long-sized samples can be prepared, overcoming the technical difficulties of uneven gas hydrogen permeation and the problem of deep surface oxidation. The entire preparation method is simple and quick.

[0132] <Application of pipelines>

[0133] The pipes of the embodiments of the present application or the pipes prepared by the methods for preparing the pipes of the embodiments of the present application can be widely used in fatigue tests, creep tests, high-temperature oxidation tests, and the like.

[0134] In some embodiments, the fatigue test is a fatigue test under certain hydrogen absorption conditions under simulated working conditions for testing the performance of nuclear-grade zirconium and zirconium alloy thin-walled pipes. In this case, the pipe of the embodiment of the present application or the pipe prepared by the method for preparing the pipe of the embodiment of the present application can be used as a fatigue sample for the fatigue test.

[0135] Certain features of the present technology are further illustrated in the following non-limiting examples.

[0136] The outer diameter of the nuclear-grade zirconium and zirconium alloy thin-walled pipes involved in each embodiment and comparative example is 9.5 mm, the wall thickness is 0.57 mm, and the chemical composition meets Table 1, which meets the composition requirements of nuclear-grade zirconium and zirconium alloy thin-walled pipes.

[0137] Table 1 Chemical composition of nuclear grade zirconium and zirconium alloy thin-walled pipes involved in various embodiments and comparative examples

[0138]

[0139] Note: The last column in Table 1 indicates that the mass contents of Mn, Ta, Mo, V, Ti, Co and Ni are all less than 0.0025%; the second to last column indicates that the mass contents of Hf, W and Pb are all less than 0.0050%.

[0140] The high temperature resistant tapes involved in the embodiments and comparative examples are all polyimide high temperature tapes resistant to 500°C.

[0141] Example 1

[0142] like Figure 1 and Figure 2 As shown, the pipeline of this embodiment is a fatigue sample, and its preparation method includes the following steps:

[0143] Step 1: Select a 300 mm long nuclear grade zirconium or zirconium alloy thin-walled tube as the main tube blank 3, and perform surface treatments of degreasing, water washing, three times of pickling, water washing, ultrasonic cleaning, and drying in sequence.

[0144] The degreasing method is: immersion in acetone. The pickling method is: immerse the entire sample in a mixed acid solution of (≥40wt%) hydrofluoric acid, (65-68wt%) nitric acid, and water in a volume ratio of 35:90:484, pickle for 20s, remove from the acid solution, rinse in running water, and then pickle again, and repeat this process 3 times. The ultrasonic cleaning method is: use a neutral detergent or anhydrous ethanol for ultrasonic cleaning.

[0145] Step 2. The outer surface of the main tube blank 3 after the surface treatment in step 1 is coated with two layers of the first protective layer 1 in sequence and evenly, and a high-temperature resistant tape is used to stick the inner first protective layer 1 (that is, the first protective layer 1 adjacent to the main tube blank 3) and the outer surface of the tube end of the main tube blank 3, the inner first protective layer 1 and the outer first protective layer 1 (the first protective layer 2 away from the main tube blank 3), and the joints of each first protective layer 1 along the axial direction of the main tube blank 3. Subsequently, a second protective layer 2 is coated in the middle position of the outer surface of the outer first protective layer 1, and a high-temperature resistant tape is used to stick the second protective layer 2 along the joints and ends of the coating layers, along the axial joints of the main tube blank 3, and the outer surface of the second protective layer 2 and the outer first protective layer 1, to obtain a coated main tube blank (such as Figure 2 shown).

[0146] Wherein, the first protective layer 1 and the second protective layer 2 are both tin foil with a thickness of 0.35 mm; Figure 2 As shown, the second protective layer 2 has a first end 201 and a second end 202 that are relatively arranged, and the main tube blank 3 has a third end 301 and a fourth end 302 that are relatively arranged, the third end 301 is adjacent to the first end 201, and the fourth end 302 is adjacent to the second end 201, and the spacing between the first end 201 and the third end 301, and the spacing between the second end 202 and the fourth end 302 are both 16.7% (about 50 mm) of the length of the main tube blank 3.

[0147] Step 3: Place the coated nuclear-grade zirconium and zirconium alloy thin-walled tubes obtained in step 2 in a hydrogen permeation furnace, pass hydrogen with a purity of 99.99wt% at a flow rate of 30ml / min through the coated nuclear-grade zirconium and zirconium alloy thin-walled tubes for the first hydrogen permeation treatment, and then cool to room temperature at a cooling rate of 2.5°C / min to obtain a first intermediate product.

[0148] The temperature of the first hydrogen permeation is 390° C., and the time of the first hydrogen permeation (ie, the time for the hydrogen to flow through the coated nuclear-grade zirconium and zirconium alloy thin-walled pipe) is 4 hours.

[0149] Step 4: Remove all aluminum foil and high temperature resistant tape from the first intermediate product obtained in step 3, then sequentially perform pickling, water washing, and drying to obtain a second intermediate product.

[0150] The pickling method is as follows: immerse the entire sample in a mixed acid solution of (≥40wt%) hydrofluoric acid, (65-68wt%) nitric acid, and water in a volume ratio of 35:90:484, pickle for 20s, remove from the acid solution, rinse in running water, and then pickle again, and repeat this process three times.

[0151] Step 5. Place the coated second intermediate product obtained in step 4 in a hydrogenation furnace, and pass hydrogen with a purity of 99.99wt% at a flow rate of 30ml / min through the second intermediate product for a second hydrogenation treatment, and then cool it to room temperature at a cooling rate of 2.5℃ / min to obtain the pipeline of this embodiment, marked as sample S1#.

[0152] The temperature of the second hydrogenation is 390° C., and the time of the second hydrogenation (ie, the time for hydrogen to flow through the coated nuclear-grade zirconium and zirconium alloy thin-walled pipe) is 4 hours.

[0153] Example 2

[0154] This embodiment is basically the same as Embodiment 1, except that:

[0155] In step 3, the temperature of the first hydrogenation is 400° C., and the time of the first hydrogenation is 4.5 h.

[0156] In step five, the temperature of the second hydrogenation is 400°C, the time of the second hydrogenation is 4.5 hours, and the obtained pipeline is marked as sample S2#.

[0157] Example 3

[0158] This embodiment is basically the same as Embodiment 1, except that:

[0159] In step 3, the temperature of the first hydrogenation is 420° C., and the time of the first hydrogenation is 5.5 h.

[0160] In step five, the temperature of the second hydrogenation is 420°C, the time of the second hydrogenation is 5 hours, and the obtained pipe is marked as sample S3#.

[0161] Example 4 (the first hydrogenation temperature is different from the second hydrogenation temperature, the second hydrogenation temperature is higher, and the rest is the same as Example 1)

[0162] This embodiment is basically the same as Embodiment 1, except that:

[0163] In step five, the temperature of the second hydrogen permeation is 440°C, and the resulting pipe is marked as sample S4#.

[0164] Example 5 (the first hydrogenation temperature is different from the second hydrogenation temperature, the second hydrogenation temperature is lower, and the rest is the same as Example 1)

[0165] This embodiment is basically the same as Embodiment 1, except that:

[0166] In step 3, the temperature of the first hydrogenation is 440°C.

[0167] In step 5, the obtained pipeline is marked as sample S5#.

[0168] Embodiment 6 (lower limit of the first hydrogenation temperature, upper limit of the second hydrogenation temperature, upper limit of the first hydrogenation time, lower limit of the second hydrogenation time, and the rest are the same as in Embodiment 1)

[0169] This embodiment is basically the same as Embodiment 1, except that:

[0170] In step 3, the temperature of the first hydrogenation is 380° C., and the time of the first hydrogenation is 6 hours.

[0171] In step five, the temperature of the second hydrogenation is 440°C, the time of the second hydrogenation is 3 hours, and the obtained pipe is marked as sample S6#.

[0172] Example 7 (lower limit of hydrogen flow rate, the rest is the same as Example 1)

[0173] This embodiment is basically the same as Embodiment 1, except that:

[0174] In step 3, the flow rate of hydrogen is 25 ml / min.

[0175] In step five, the flow rate of hydrogen is 25 ml / min, and the resulting pipeline is marked as sample S7#.

[0176] Example 8 (upper limit of hydrogen flow rate, the rest is the same as Example 1)

[0177] This embodiment is basically the same as Embodiment 1, except that:

[0178] In step 3, the flow rate of hydrogen is 50 ml / min.

[0179] In step five, the flow rate of hydrogen is 50 ml / min, and the resulting pipeline is marked as sample S8#.

[0180] Example 9 (the cooling rate is reduced, and the rest is the same as Example 1)

[0181] This embodiment is basically the same as Embodiment 1, except that:

[0182] In step 3, the cooling rate is 0.5°C / min.

[0183] In step five, the cooling rate is 0.5°C / min, and the resulting pipe is marked as sample S9#.

[0184] Example 10 (the upper limit of the thickness of the tin foil is 0.5 mm, and the rest is the same as Example 1)

[0185] This embodiment is basically the same as Embodiment 1, except that:

[0186] In step 2, the first protective layer 1 and the second protective layer 2 are both tin foil with a thickness of 0.5 mm.

[0187] In step five, the obtained pipeline is marked as sample S10#.

[0188] Example 11 (upper limit of the spacing between the third layer of tin foil is greater than 50, and the rest is the same as Example 1)

[0189] This embodiment is basically the same as Embodiment 1, except that:

[0190] In step 2, the distance between the first end 201 and the third end 301 and the distance between the second end 202 and the fourth end 302 are both 18% (54 mm) of the length of the main tube 3.

[0191] In step five, the obtained pipeline is marked as sample S11#.

[0192] Example 12 (length 320 mm, the spacing between the third layer of tin foil remains unchanged (equivalent to the lower limit ratio), and the rest is the same as Example 1)

[0193] This embodiment is basically the same as Embodiment 1, except that:

[0194] In step 1, the length of the nuclear grade zirconium and zirconium alloy thin-walled tube is 320 mm.

[0195] In step five, the obtained pipeline is marked as sample S12#.

[0196] Example 13 (coating material: aluminum foil, other aspects are the same as in Example 1)

[0197] This embodiment is basically the same as Embodiment 1, except that:

[0198] In step 2, the first protective layer 1 and the second protective layer 2 are both aluminum foils with a thickness of 0.35 mm.

[0199] In step five, the obtained pipeline is marked as sample S13#.

[0200] Comparative Example 1 (completely uncoated)

[0201] This comparative example is substantially the same as Example 2, except that:

[0202] Excluding step 2 and step 4, the nuclear-grade zirconium and zirconium alloy thin-walled tubes after surface treatment in step 1 are directly subjected to the first hydrogenation treatment in step 3 and the second hydrogenation treatment in step 5, and the obtained sample is marked as D1#.

[0203] Comparative Example 2 (without third layer of aluminum foil coating)

[0204] This comparative example is substantially the same as Example 2, except that:

[0205] In step 2, the second protective layer 2 is not coated. That is, step 2 is: the outer surface of the main tube blank 3 after the surface treatment in step 1 is sequentially and evenly coated with two layers of the first protective layer 1, and the inner first protective layer 1 (that is, the first protective layer 1 adjacent to the main tube blank 3) and the outer surface of the tube end of the main tube blank 3, the inner first protective layer 1 and the outer first protective layer 1 (the first protective layer 2 away from the main tube blank 3) and the joints of each first protective layer 1 along the axial direction of the main tube blank 3 are pasted with a high temperature resistant tape at the joint of the coating layer to obtain a coated main tube blank. Among them, the first protective layer 1 is a tin foil with a thickness of 0.35 mm.

[0206] In step 5, the obtained pipeline is marked as sample D2#.

[0207] Comparative Example 3

[0208] This comparative example is substantially the same as Example 2, except that:

[0209] In step 2, the 2 layers of the first protective layer 1 are not coated. That is, step 2 is: a layer of the second protective layer 2 is coated on the middle position of the outer surface of the main tube blank 3 after the surface treatment in step 1, and a high temperature resistant tape is used to stick the second protective layer 2 along the axial joint of the main tube blank 3 and the outer surface of the second protective layer 2 and the outer first protective layer 1 at the joint of the coating layer to obtain the coated main tube blank. Among them, the second protective layer 2 is a tin foil with a thickness of 0.35mm; Figure 2 As shown, the second protective layer 2 has a first end 201 and a second end 202 that are relatively arranged, and the main tube blank 3 has a third end 301 and a fourth end 302 that are relatively arranged, the third end 301 is adjacent to the first end 201, and the fourth end 302 is adjacent to the second end 201, and the spacing between the first end 201 and the third end 301, and the spacing between the second end 202 and the fourth end 302 are both 16.7% (about 50 mm) of the length of the main tube blank 3.

[0210] In step 5, the obtained pipeline is marked as sample D3#.

[0211] Comparative Example 4 (no coating removal after one hydrogenation, removal after two hydrogenation)

[0212] This comparative example is substantially the same as Example 2, except that:

[0213] Step 4 is arranged after step 5. The specific process is: remove all tin foil and high temperature resistant tape covering the product after the second hydrogenation treatment, then carry out acid pickling, water washing and drying in sequence to obtain a pipeline, which is marked as sample D4#.

[0214] In the original step 5, the statement "obtaining the pipeline of this embodiment" is deleted.

[0215] Comparative Example 5 (Hydrogenation only once)

[0216] This comparative example is substantially the same as Example 2, except that:

[0217] Excluding step five, the second intermediate product in step four is the pipeline, marked as sample D5#.

[0218] The samples prepared in each embodiment and comparative example were sampled at intervals of 48 mm along the length direction from end 1 (from end 1 to end 2, the explanation of end 1 and end 2 is shown in the notes below Table 1) for hydrogen content testing, and the sizes of all test data of each sample were compared. The uniformity of the hydrogen content in the sample was evaluated based on whether the difference between the maximum and minimum values ​​was less than 0.0120wt% - if the maximum and minimum values ​​were less than 0.0120wt%, the uniformity of the hydrogen content in the sample was judged to be good; if the maximum and minimum values ​​were above 0.0120wt%, the uniformity of the hydrogen content in the sample was judged to be poor.

[0219] Observe the surface conditions of the samples prepared in each embodiment and comparative example and judge the quality of the surface conditions of the samples. The specific method is: visually inspect the surface color. If the surface shows a metallic color (silver-white) after hydrogen permeation, it can be considered unoxidized. If the surface shows one or more of purple, blue, gray, and yellow, it is oxidized.

[0220] The test results of hydrogen content test of the samples prepared in each embodiment and comparative example at intervals of 48 mm along the length direction are shown in Table 2.

[0221] Table 2 Hydrogen content test results

[0222]

[0223]

[0224] Note: End 1 and End 2 in Table 2 are the positions 2 mm from the two opposite ends of the sample to the middle of the sample, and the difference is the difference between the maximum and minimum hydrogen contents measured at different positions of the corresponding samples.

[0225] The surface condition results of the samples prepared in each embodiment and comparative example are shown in Table 3.

[0226] Table 3 Surface condition results

[0227]

[0228] It can be seen from Tables 2 and 3 that fatigue samples with unoxidized surfaces and uniformly distributed hydrogen content (less than 0.0120wt%) can be prepared according to the embodiments of the present application. The hydrogen content of the samples is uniform, with a deviation of less than 0.0120%, and the surface is unoxidized, meeting the preparation requirements of "uniform hydrogen content and unoxidized surface" for the corresponding fatigue samples; oxidation occurs at different positions on the surface of the samples not prepared according to the present application, and the hydrogen content distribution does not reach the requirement of uniform distribution (less than 0.0120wt%), and the samples do not meet the preparation requirements of the corresponding fatigue samples.

[0229] In summary, the preparation method of the pipe of the present application can be used to prepare fatigue samples of thin-walled pipes. The thin-walled pipe fatigue samples prepared by the preparation method of the pipe of the present application are mainly targeted at products such as nuclear-grade zirconium and zirconium alloy thin-walled pipes widely used in the domestic atomic energy industry. They have the advantages of large length, high hydrogen content and good uniformity, and solve the problem of difficulty in preparing fatigue samples due to large length samples, high hydrogen content and strict requirements on hydrogen content uniformity.

[0230] In the present application, the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0231] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0232] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A pipeline, characterized in that: It includes a main body, which is a tubular structure; the length of the main body is 250-350mm, and the wall thickness of the main body is 0.3-0.6mm; the material of the main body includes zirconium and / or zirconium alloy; the mass content of hydrogen in the main body is 0.0600-0.1200%, and the mass content deviation of hydrogen in various parts of the main body is less than 0.0120%.

2. The pipeline according to claim 1, characterized in that The material of the body is nuclear grade zirconium or / and nuclear grade zirconium alloy.

3. The pipeline according to claim 1 or 2, characterized in that The ratio of the outer diameter of the body to the wall thickness of the body is greater than 16 and less than 20.

4. A method for preparing a pipeline according to any one of claims 1 to 3, characterized in that: include: At least two first protective layers that allow hydrogen to permeate are coated and fixed on the outer surface of the main tube blank; At least one second protective layer that allows hydrogen to permeate is coated and fixed at a middle position of the outer surface of the first protective layer as the outermost layer to obtain a coated main body tube blank; The coated main tube blank is subjected to a first hydrogenation to obtain a first intermediate product; removing the first protective layer and the second protective layer from the first intermediate product, and then pickling, washing with water, and drying the product to obtain a second intermediate product; The second intermediate product is subjected to a second hydrogenation to obtain the main body.

5. The preparation method according to claim 4, characterized in that: The first protective layer and the second protective layer both include at least one of tin foil and aluminum foil; and / or, The joints between the first protective layer and the second protective layer along the axial direction of the main tube billet, between the first protective layer and the outer surface of the main tube billet, between two adjacent first protective layers, and between the second protective layer and the outer surface of the outermost first protective layer are all fixed by bonding.

6. The preparation method according to claim 4 or 5, characterized in that: The length, wall thickness, material, and ratio of outer diameter to wall thickness of the main body tube are the same as those of the main body; the mass content of hydrogen in the main body tube is less than 15ppm, and the mass content deviation of hydrogen in various parts of the main body tube is 10-20%; and / or, The thickness of the first protective layer and the second protective layer are both 0.35-0.5 mm; And / or, the second protective layer has a first end and a second end, the main tube blank has a third end and a fourth end, the third end is adjacent to the first end, the fourth end is adjacent to the second end, and the spacing between the first end and the third end, and the spacing between the second end and the fourth end are both 11-20% of the length of the main tube blank.

7. The preparation method according to claim 4, characterized in that: The first hydrogenation and the second hydrogenation both include introducing flowing hydrogen into the main tube; and / or, The hydrogen flow rate of the first hydrogenation is 25-50 ml / min; and / or, the temperature of the first hydrogenation is 380-440° C.; and / or, the time of the first hydrogenation is 4-6 hours; And / or, the hydrogen flow rate of the second hydrogenation is 25-50 ml / min; and / or, the temperature of the second hydrogenation is 380-440° C.; and / or, the time of the second hydrogenation is 3-5 hours.

8. The preparation method according to claim 4, characterized in that: The method for preparing the pipe further comprises the step of pretreating the body tube blank before coating and fixing at least two first protective layers that allow hydrogen to permeate on the outer surface of the body tube blank; and / or, The method for preparing the pipeline further comprises a step of performing a first cooling step after the first hydrogenation; and / or, The method for preparing the pipeline further comprises a step of performing a second temperature reduction after the second hydrogen permeation.

9. The preparation method according to claim 8, characterized in that: The preprocessing comprises: Degreasing, washing and drying the main tube blank; the washing method includes at least one of water washing, acid washing and ultrasonic cleaning; and / or, The first cooling rate is less than 3°C / min; and / or, The second cooling rate is less than 3°C / min.

10. Use of the pipeline according to any one of claims 1 to 3 or the pipeline prepared by the method for preparing the pipeline according to any one of claims 4 to 9 in fatigue tests, creep tests, and high-temperature oxidation tests.