Hot-rolled fine-blanked steel produced by adopting CSP production line and production method of hot-rolled fine-blanked steel
By adopting the CSP production line process in hot-rolled fine-brushed steel production, the metallographic structure and carbide distribution of hot-rolled plates are optimized, and the problems of long and high cost of cold-rolled process are solved, achieving high strength and high wear resistance And high-precision fine-brushed steel products significantly improve the product's pass rate and production efficiency.
Patent Information
- Application Number
- CN202411062281.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
In the production of fine-brushed steel, the cold rolling process is long, the cost is high, and it is difficult to meet the needs of high strength and high wear resistance, and the annealing process time and cost are high.
Hot-rolled fine-pulled steel produced by CSP production line is optimized through converter smelting, LF furnace refining, vacuum treatment, rapid cooling, finishing rolling, laminar segment cooling, coiling and hood furnace annealing processes. The metallographic structure refinement and carbide distribution improve the direct spheroidization rate of hot rolling and the accuracy of plate thickness.
The metallographic structure of steel has been refined to level 11 or above, the carbide distribution is uniform, the direct spheroidization rate of hot rolling reaches 85-95%, the plate thickness accuracy reaches ±0.01mm, and the product moldability is accurate, meeting the needs of precision punching. , the pass rate has been significantly increased to more than 99%, reducing production costs and time.
Smart Images

Figure CN118979199A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a steel for stamping parts and a production method, and in particular to a hot-rolled fine-blanking steel produced by a CSP production line and a production method. Background Art
[0002] Fine blanking technology is an efficient and high-quality parts production technology that combines precision blanking and stamping, which is developed on the basis of ordinary stamping technology. In order to meet the requirements of fine blanking technology, the material requirements for fine blanking steel are high, requiring high cleanliness, high structural uniformity, high spheroidization rate, etc. Compared with ordinary materials, it has the disadvantages of increased production costs and a long production process.
[0003] At present, the production of cold-rolled materials involves three different processing workshops: pickling, annealing, and cold rolling. The steel coil transportation process is long, and the total time for annealing heating + insulation + cooling is more than 60 hours. Therefore, a cold rolling process takes more than 1 week. If hot-rolled materials can be directly used after pickling, the problem of long production process can be solved. At the same time, annealing and cold rolling need to increase production costs by 300 yuan and 400 yuan per ton respectively. The cost reduction effect of using hot-rolled coils instead of cold-rolled coils is obvious.
[0004] After searching:
[0005] The document with Chinese patent application number CN201410231375.9 discloses a "method for manufacturing fine blanking steel and fine blanking parts of its adjustment mechanism". The chemical composition (wt%) of the fine blanking steel is as follows: C: 0.12~0.24, Si: ≤0.40, Mn: 0.30~0.80, P≤0.015, S≤0.005%, Cr: ≤0.40, Ni≤0.40, Mo: ≤0.10, Ca: 0.0015~0.0040%, and the remainder is Fe and inevitable inclusions. The method includes the following process route: molten iron - smelting (refining outside the furnace) - casting - heating of ingot - hot rolling - pickling - cold rolling - spheroidizing annealing - fine blanking - heat treatment. According to the present invention, the non-metallic inclusion content of the above-mentioned fine blanking parts is: various inclusions ≤ 1.5 level, elongation after fracture: A ≥ 30%, fine blanking difficulty: S3 level, and fine blanking parts with high dimensional accuracy, high strength and high toughness can be obtained. This document can only manufacture low-strength and low-wear-resistant parts or improve strength and wear resistance through carburizing and quenching to meet high-strength requirements.
[0006] The document with Chinese patent application number CN201810048364.5 discloses "A cold-rolled fine-blanked steel strip for a car child seat locking device and a preparation method", wherein the composition of the cold-rolled fine-blanked steel strip includes: C: 0.50-0.55, Si: 0.15-0.35, Mn0.80-1.10, P≤0.015, S≤0.01, Cr 0.90-1.20, V 0.10-0.20, Al≤0.035. The present invention reasonably optimizes the chemical composition of 51CrV4 for the special processing technology and application requirements of the child seat locking device, and reasonably controls the elemental composition of C, S, P Si and other hydrogen embrittlement sensitive factors. Although the document can meet the requirements of high strength and high wear resistance, it needs cold rolling processing, has high production costs and a long processing flow.
[0007] The document with Chinese patent application number CN200910196007.4 discloses "A hot-rolled steel plate for precision stamping and its manufacturing method", whose chemical composition mass percentage is: C: 0.05~0.30; Si: ≤0.50; Mn: 0.50~1.50; P: ≤0.02; S: ≤0.01; Cr: 0.05~1.50; Alt: ≤0.04; Ni: 0.02~0.50; the hot-rolled steel plate also includes one or two of Ti and B, among which Ti: ≤0.05; B: 0.0005~0.010, and Ni+Ti+B≤0.50, and the rest is iron and unavoidable impurities. This document also provides a method for manufacturing the hot-rolled steel plate, comprising the following steps: pre-desulfurization of molten iron; converter smelting; refining outside the furnace; continuous casting; slab reheating, slab heating temperature: 1100-1250°C; rolling, finishing rolling end temperature: 780-950°C; coiling, coiling temperature: 500-700°C; spheroidizing annealing, spheroidizing annealing temperature: 700-740°C. The steel plate of this document is not only easy to fine-blanket, but also can obtain a good match between strength and toughness. This document introduces a low-carbon chromium-manganese-nickel steel, which belongs to hot-rolled fine-blanketing steel. Since its carbon content is less than 0.30%, it is only suitable for manufacturing low-strength parts.
[0008] The document with Chinese patent application number CN201510523289.X discloses "A medium-high carbon hot-rolled strip with excellent fine blanking performance and production method". The chemical composition and weight percentage of the strip are: C: 0.50-0.65%, Si: 0.60-1.50%, Mn: 0.50-1.70%, Ca: 0.0030-0.0070%, B: 0.0008-0.005%, Als: 0.015-0.030%, P≤0.015%, S≤0.008%, and the rest are Fe and unavoidable impurities. The present invention utilizes the principle of Si element to increase the activity of carbon atoms in austenite, adopts a rapid spheroidizing annealing process, and shortens the holding time at the annealing temperature to 1h-2h. Although it can reduce costs, save energy, and ultimately produce hot-rolled steel strips with excellent punching performance, its high silicon content design makes hot-rolling production difficult and iron sheet indentations are prone to occur on the surface, making it only suitable for automotive parts with low surface requirements.
[0009] The document with Chinese patent application number CN201510345809.2 discloses "A spring steel fine blanking processing method", which includes: soft annealing steps, hot rolling slitting steps, pickling steps, rolling steps, three-step spheroidizing annealing steps and leveling steps, wherein the soft annealing condition is 20-30°C below the spheroidizing temperature of the spring steel, and the three-step spheroidizing annealing condition is heating to 690°C, keeping it warm for 3 hours, heating to 730°C, keeping it warm for 3 hours, cooling down to 670°C in stages, keeping it warm for 3 hours, heating to 720°C, keeping it warm for 3 hours, cooling down to 690°C, keeping it warm for 3 hours, heating to 720°C, keeping it warm for 3 hours, cooling down to 690°C, keeping it warm for 3 hours, heating to 720°C, keeping it warm for 3 hours, cooling down to 690°C, keeping it warm for 3 hours, cooling down after heating to 690°C, keeping it warm for 3 hours. Although this invention effectively reduces the production cost and improves the yield rate, it still belongs to the scope of cold-rolled fine blanking steel. Summary of the invention
[0010] The present invention aims to overcome the shortcomings of the prior art and provide a hot-rolled plate production process that is optimized to improve the metallographic structure of steel to more than 11 levels, and to make the carbide distribution uniform, with a hot-rolled direct spheroidization rate of 85-95%, a plate thickness accuracy of ±0.01mm, and the product after hot-rolled pickling and annealing can meet the fine blanking requirements. The prepared product has accurate formability and a significantly improved pass rate, and a hot-rolled fine blanking steel and a production method produced by a CSP production line.
[0011] Measures to achieve the above objectives:
[0012] A hot-rolled fine blanking steel produced by a CSP production line has the following components and weight percentage contents: C: 0.15-0.56%, Si: 0.10-0.50%, Mn: 0.10-1.20%, Cr: 0.01-1.20%, Mo: 0.01-0.30%, B: 0.001-0.005%, P≤0.010%, S≤0.005%, and satisfies: H=C+0.2Mn+0.2Cr+Mo+50B in the range of 0.4-1.2%, and the rest is iron and unavoidable impurities.
[0013] The invention is characterized in that: the weight percentage content of V is 0.01-0.40%.
[0014] The invention is characterized in that the weight percentage content of Ni is 0.01-0.30%.
[0015] A method for producing hot-rolled fine blanking steel produced by a CSP production line, comprising the following steps:
[0016] 1) After converter smelting, LF refining is carried out, during which: the heating temperature is 1560±20℃, and fine-tuning is performed according to the composition;
[0017] 2) Perform RH vacuum treatment and control the vacuum degree to 30-50Pa, cycle time to 15±2min, and soft blowing to 5±2min;
[0018] 3) After rapid cooling in the thin slab crystallizer to form a slab shell, it is slowly cooled to prevent surface cracks, and directly enters the heating furnace for heating, with an entry temperature of 820-900°C and an exit temperature of 1150-1220°C;
[0019] 4) Finish rolling after descaling with high-pressure water;
[0020] 5) Carry out finish rolling and control the reduction rate of each pass as follows:
[0021] The reduction ratios of the first and second passes are both between 40% and 60%;
[0022] The reduction rates of the third and fourth passes are both between 30% and 50%;
[0023] The reduction rates of the fifth and sixth passes are both between 20% and 40%;
[0024] The reduction rate of the seventh pass is 5-11%;
[0025] And control the final rolling temperature at 820~920℃;
[0026] 7) Adopt laminar flow segmented cooling, the first segment is cooled at a cooling rate of 60-120℃ / S to the fastest phase transformation point of pearlite + 20℃;
[0028] The second stage is air-cooled to coiling temperature;
[0029] 7) Coiling: Control the coiling temperature at 500-700°C;
[0030] 8) After conventional pickling, bell-type furnace annealing is performed, heating to 680-740°C at an annealing heating rate of 30-50°C / h, and the heating time is controlled at 10-16h; and cooling to room temperature at a cooling rate of 10-20°C / h;
[0031] 9) Reserved.
[0032] Preferably, the reduction ratio of each pass of the finishing rolling is as follows:
[0033] The reduction ratios of the first and second passes were both between 47% and 53%;
[0034] The reduction ratios of the third and fourth passes were both between 37% and 43%;
[0035] The reduction rates of the fifth and sixth passes are both between 28% and 33%;
[0036] The reduction rate of the seventh pass is between 9 and 11%.
[0037] Preferably, the first stage of laminar cooling has a cooling temperature of 610-650°C.
[0038] Preferably, the coiling temperature is between 640 and 670°C.
[0039] Preferably, the hood annealing temperature is 690-720° C., and the heating time is 10-12 hours.
[0040] Functions and mechanisms of the components and main processes in the present invention
[0041] C: Carbon in steel mainly plays a role in improving the strength and hardenability of steel. In the hot-rolled structure, carbon exists in the form of carbides, forming pearlite, bainite, etc. After quenching, carbon exists in a solid solution state, and the structure undergoes phase transformation strengthening. After tempering, carbides precipitate, which plays a precipitation strengthening role. Too high carbon content will reduce the plasticity and toughness of steel, and too low carbon content will reduce the hardenability of steel, which is not conducive to the heat treatment of fine blanking steel. The preferred range of carbon content in the present invention is controlled at 0.21-0.51%.
[0042] Si: Silicon in steel improves the strength of steel by solid solution strengthening and refining the pearlite plate spacing, but it reduces plasticity and toughness and increases surface defects of hot-rolled plates. Silicon is the main deoxidizer, and its content in steel is generally above 0.1%, so the preferred range of Si content is controlled at 0.18-0.36%.
[0043] Mn: Manganese in steel improves the strength of steel and combines with S in steel to form MnS, eliminating the effect of S. Mn is a good deoxidizer and can effectively refine pearlite, so the Mn content is preferably in the range of 0.36-0.60%.
[0044] Cr: Chromium can improve strength, hardenability and tempering resistance, and reduce the decarburization layer of hot-rolled plates. However, chromium will significantly increase the banded structure of steel and affect the uniformity of the structure. Therefore, the preferred range of Cr content is 0.36-0.66%.
[0045] V: Vanadium can refine the grain size, improve the strength and toughness, and improve the tempering resistance. The preferred range of V content in the present invention is 0.026-0.036%.
[0046] Ni: Nickel can simultaneously improve the strength and toughness of steel, optimize welding performance and corrosion resistance, and improve low-temperature toughness. The preferred range of nickel content in the present invention is 0.05-0.10%.
[0047] Mo: Molybdenum improves the strength of steel by solid solution strengthening and stabilizing carbides. It can also improve hardenability and inhibit temper brittleness. The preferred range of the content of the present invention is 0.05-0.1%.
[0048] B: A trace amount of boron can improve the strength and hardenability of steel and strengthen grain boundaries. The preferred content range of the present invention is 0.002-0.004%.
[0049] P: Phosphorus comes from ores and is generally considered to be a harmful element in steel, which reduces the toughness and plasticity of steel. The lower the content of phosphorus in the present invention, the better, and the preferred range is 0.005-0.010%.
[0050] S: Sulfur originates from coke, scrap steel, alloy and other steel smelting raw materials. It is generally considered to be a harmful element. It will increase the level of inclusions in steel, improve the level of segregation, reduce ductility and toughness, and cause hot working cracking. The lower the content of sulfur in the present invention, the better. The preferred range is 0.001-0.003%.
[0051] The reason why the present invention controls the heating temperature of molten steel in the LF furnace to be between 1540°C and 1580°C is that high temperature heating is beneficial to the homogenization of the alloy.
[0052] The reason why the present invention controls the vacuum degree at 30-50 Pa, the cycle time at 13-17 min, and the soft blowing at 3-72 min is that harmful gas elements can be removed by RH and the inclusion level can be reduced by soft blowing.
[0053] The reason why the present invention controls the inlet temperature of the casting to 820-900°C and the outlet temperature to 1150-1220°C is that the high temperature entering the heating furnace ensures the temperature uniformity of the casting, and ensures that the inlet temperature of 1150-1220°C can be smoothly finished and the rolling force can be reduced.
[0054] The present invention controls the reduction rate of each pass of finishing rolling as follows:
[0055] The reduction ratios of the first and second passes are both between 40% and 60%;
[0056] The reduction rates of the third and fourth passes are both between 30% and 50%;
[0057] The reduction rates of the fifth and sixth passes are both between 20% and 40%;
[0058] The reduction rate of the seventh pass is 5-11%;
[0059] And control the final rolling temperature at 820~920℃;
[0060] This is because the first two passes are to ensure dynamic recrystallization and grain refinement, the middle pass is to adjust the hot-rolled plate shape, and the last pass is to optimize the edge drop to ensure thickness accuracy.
[0061] The reason why the present invention controls laminar cooling to the fastest pearlite transformation point + 20°C is that this temperature point can quickly transform the pearlite phase, ensure uniform distribution of carbides, and provide easy spheroidization structure for the subsequent hood annealing process.
[0062] The reason why the coiling temperature is controlled at 500-700° C. in the present invention is to ensure sufficient temperature for coiling, further optimize the structure, and perform pre-annealing.
[0063] The reason why the bell-type furnace annealing is controlled to be heated to 680-740°C at an annealing heating rate of 30-50°C / h, and the heating time is controlled to be 10-16h; and the temperature is lowered to room temperature at a cooling rate of 10-20°C / h is that the high-temperature heating dissolves the carbide into the steel matrix, gradually precipitates in the slow cooling process, forms spheroidized pearlite, reduces the strength, and is conducive to fine blanking processing.
[0064] Compared with the prior art, the present invention optimizes the hot-rolled plate production process to improve the metallographic structure of the steel to more than 11 levels, and the carbide distribution is uniform, the hot-rolled direct spheroidization rate is 85-95%, the spheroidization level is 2.5-3.5, the plate thickness accuracy is ±0.01mm, and the product after hot-rolled pickling and annealing can meet the fine blanking requirements. The product has accurate formability and meets the fine blanking requirements of S3 or above, and the qualified rate is significantly improved to more than 99%, without defects caused by cracking, tearing and other materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] Figure 1 This is a picture of pearlite of the metallographic structure of the present invention;
[0066] Figure 2 This is a metallographic structure picture of the present invention after annealing. DETAILED DESCRIPTION
[0067] The present invention is described in detail below:
[0068] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;
[0069] Table 2 is a list of main process parameters of various embodiments and comparative examples of the present invention;
[0070] Table 3 is a table of performance test results of various embodiments and comparative examples of the present invention.
[0071] Each embodiment of the present invention is produced according to the following steps
[0072] 1) After converter smelting, LF refining is carried out, during which: the heating temperature is 1560±20℃, and fine-tuning is performed according to the composition;
[0073] 2) Perform RH vacuum treatment and control the vacuum degree to 30-50Pa, cycle time to 15±2min, and soft blowing to 5±2min;
[0074] 3) After rapid cooling in the thin slab crystallizer to form a slab shell, it is slowly cooled to prevent surface cracks, and directly enters the heating furnace for heating, with an entry temperature of 820-900°C and an exit temperature of 1150-1220°C;
[0075] 4) Finish rolling after descaling with high-pressure water;
[0076] 5) Carry out finish rolling and control the reduction rate of each pass as follows:
[0077] The reduction ratios of the first and second passes are both between 40% and 60%;
[0078] The reduction rates of the third and fourth passes are both between 30% and 50%;
[0079] The reduction rates of the fifth and sixth passes are both between 20% and 40%;
[0080] The reduction rate of the seventh pass is 5-11%;
[0081] And control the final rolling temperature at 820~920℃;
[0082] 6) Adopt laminar flow segmented cooling, the first segment is cooled at a cooling rate of 60-120℃ / S to the fastest phase transformation point of pearlite + 20℃;
[0084] The second stage is air-cooled to coiling temperature;
[0085] 7) Coiling: Control the coiling temperature at 500-700°C;
[0086] 8) After conventional pickling, bell-type furnace annealing is carried out, and the annealing temperature is heated to 680-740°C at a heating rate of 30-50°C / h.
[0087] The heating time is controlled within 10 to 16 hours; and the temperature is lowered to room temperature at a cooling rate of 10 to 20°C / h; 9) set aside.
[0088] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)
[0089]
[0090] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples
[0091]
[0092]
[0093] Table 2
[0094]
[0095] Table 3
[0096]
[0097]
[0098] Note: The phase change temperature points of the first stage of laminar cooling and segmented cooling in this table are thermodynamically calculated values, and the phase change temperature points of different components are different.
[0099] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples
[0100]
[0101] As can be seen from Table 3, the present invention realizes the steel type that originally required cold rolling annealing process to produce by hot rolling direct annealing, meets the demand for fine blanking steel with high hardness and high wear resistance, and the thickness accuracy reaches the level of cold rolled plate.
[0102] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. A hot-rolled fine blanking steel produced by a CSP production line, wherein the components and weight percentages are: C: 0.15-0.56%, Si: 0.10-0.50%, Mn: 0.10-1.20%, Cr: 0.01-1.20%, Mo: 0.01-0.30%, B: 0.001~0.005%, P≤0.010%, S≤0.005%, and satisfying: H=C+0.2Mn+0.2Cr+Mo+50B is between 0.4~1.2%, and the rest is iron and unavoidable impurities.
2. The hot-rolled fine blanking steel produced by a CSP production line according to claim 1, characterized in that: The weight percentage of V is 0.01-0.40%.
3. The hot-rolled fine blanking steel produced by a CSP production line according to claim 1, characterized in that: The weight percentage content of Ni is 0.01-0.30%.
4. A method for producing hot-rolled fine blanking steel produced by a CSP production line as claimed in claim 1, comprising the following steps: 1) After converter smelting, LF refining is carried out, during which: the heating temperature is 1560±20℃, and fine-tuning is performed according to the composition; 2) Perform RH vacuum treatment and control the vacuum degree to 30-50Pa, cycle time to 15±2min, and soft blowing to 5±2min; 3) After rapid cooling in the thin slab crystallizer to form a slab shell, it is slowly cooled to prevent surface cracks, and directly enters the heating furnace for heating, with an entry temperature of 820-900°C and an exit temperature of 1150-1220°C; 4) Finish rolling after descaling with high-pressure water; 5) Carry out finish rolling and control the reduction rate of each pass as follows: The reduction ratios of the first and second passes are both between 40% and 60%; The reduction rates of the third and fourth passes are both between 30% and 50%; The reduction rates of the fifth and sixth passes are both between 20% and 40%; The reduction rate of the seventh pass is 5-11%; And control the final rolling temperature at 820~920℃; 6) Adopt laminar flow segmented cooling, the first segment is cooled at a cooling rate of 60-120℃ / S to the fastest phase transformation point of pearlite + 20℃; The second stage is air-cooled to coiling temperature; 7) Coiling: Control the coiling temperature at 500-700°C; 8) After conventional pickling, bell-type furnace annealing is performed, heating to 680-740°C at an annealing heating rate of 30-50°C / h, and the heating time is controlled at 10-16h; and cooling to room temperature at a cooling rate of 10-20°C / h; 9) Reserved.
5. A method for hot rolling fine blanking steel produced by a CSP production line according to claim 4, characterized in that: The reduction ratio of each pass of finishing rolling is as follows: The reduction ratios of the first and second passes were both between 47% and 53%; The reduction ratios of the third and fourth passes were both between 37% and 43%; The reduction rates of the fifth and sixth passes are both between 28% and 33%; The reduction rate of the seventh pass is between 9 and 11%.
6. A method for hot rolling fine blanking steel produced by a CSP production line according to claim 4, characterized in that: The first stage of laminar cooling has a temperature between 610 and 650°C.
7. A method for hot rolling fine blanking steel produced by a CSP production line according to claim 4, characterized in that: The coiling temperature is between 640 and 670°C.
8. A method for hot rolling fine blanking steel produced by a CSP production line according to claim 4, characterized in that: The hood annealing temperature is between 690 and 720°C, and the heating time is between 10 and 12 hours.
Citation Information
Patent Citations
Steel plate having excellent fine blanking processability and method for manufacture thereof
CN101379207A
Hot rolling diaphragm spring steel for automobile and production method of hot rolling diaphragm spring
CN102925812A
Hull steel with good plate shape produced by adopting CSP and production method
CN116219304A
Manufacturing method of steel plate having excellent fine blanking workability
JP2007270329A
Medium and high carbon steel plate and manufacturing method of the same
JP2010144242A
Cited By
Method for reducing strip structure defects of wide strip steel in 30MnB5
CN120575026A
High-spheroidization-rate low-strength cold-rolled 30CRMO fine blanking steel strip and manufacturing method thereof
CN121183248A