High-strength hypoeutectoid steel and preparation method thereof

By strictly controlling the chemical composition in the hypoeutectoid steel and adopting normalization, quenching and tempering processes, the problem of low mechanical properties of metal materials in the prior art is solved, and high strength and excellent tensile performance and low-temperature impact performance are achieved. , suitable for high-demand occasions such as oil drilling tools.

CN118979200APending Publication Date: 2024-11-19QINGDAO HONGXINTIAN MACHINERY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411045276.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, the mechanical properties and quality of metal materials are relatively low, making it difficult to meet the safety performance and practical requirements of petroleum drilling tools.

Method used

Prepare a high-strength subeutectoid steel, by strictly controlling the weight percentage of chemical components (carbon, silicon, manganese, phosphorus, sulfur, chromium, nickel, molybdenum, and copper, and adopting normalization, quenching and tempering heat treatment processes. Form a high-strength hypereutectic steel with excellent mechanical properties.

Benefits of technology

It realizes excellent mechanical properties and low-temperature impact properties of high-strength subeutectoid steel, suitable for special casting and welding technology, suitable for manufacturing high-stressed parts and vehicle parts in complex occasions, avoiding cracks and shrinkage after casting .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979200A_ABST
    Figure CN118979200A_ABST
Patent Text Reader

Abstract

The invention provides high-strength hypoeutectoid steel and a preparation method thereof, and belongs to the technical field of metal materials. The high-strength hypoeutectoid steel provided by the invention comprises the following composition elements in percentage by weight: 0.18-0.24% of carbon; silicon < = 0.6%; 0.8% to 1.2% of manganese; less than or equal to 0.015% of phosphorus; less than or equal to 0.005% of sulfur; 0.5 to 1.0 percent of chromium; 0.8 to 1.3 percent of nickel; 0.5 to 0.7 percent of molybdenum; 0.2 to 0.5 percent of copper; and the balance of iron. The invention also provides a preparation method of the high-strength hypoeutectoid steel, which comprises the following steps: weighing the required base material, manganese, nickel, molybdenum, chromium and copper according to the set weight percentage, smelting the base material, carrying out heat preservation, and sequentially adding manganese, nickel, molybdenum, chromium and copper to obtain molten steel. And casting the molten steel into the roasted shell, covering for heat preservation, cutting a riser after natural cooling, and then carrying out heat treatment to obtain the high-strength hypoeutectoid steel. The high-strength hypoeutectoid steel with excellent tensile property and low-temperature impact property is obtained by strictly controlling the composition and the content of the chemical components and the heat treatment processes of normalizing, quenching and tempering, and the high-strength hypoeutectoid steel is suitable for special casting and is also suitable for being applied to the welding technology; and the composite material can be used for manufacturing high-stress parts and vehicle parts in a transmission system, such as buses, engineering machinery and other complex application occasions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal materials, and in particular to a high-strength hypoeutectoid steel and a preparation method thereof. Background Art

[0002] With the continuous development of society, people's demand for energy in the field of oil and natural gas continues to increase, and higher requirements are also put forward for related energy industries. Oil has become an indispensable and important part of my country's energy industry chain. With the continuous improvement of oil drilling technology, the requirements for safety performance and practicality of wellhead tools and downhole drilling tools are also increasing day by day, which requires us to improve the performance and life of related products. Therefore, how to obtain a hypoeutectoid steel material with higher mechanical properties and higher quality has become a technical problem that needs to be solved in this field. Summary of the invention

[0003] The object of the present invention is to provide a high-strength hypoeutectoid steel and a preparation method thereof, so as to solve the technical problem of low mechanical properties and quality of metal materials in the prior art.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a high-strength hypoeutectoid steel, wherein the weight percentage of each component in the high-strength hypoeutectoid steel is:

[0006] Carbon: 0.18~0.24%; Silicon ≤0.6%; Manganese: 0.8~1.2%; Phosphorus ≤0.015%; Sulfur ≤0.005%; Chromium: 0.5~1.0%; Nickel: 0.8~1.3%; Molybdenum: 0.5~0.7%; Copper: 0.2~0.5%; The balance is iron.

[0007] The present invention provides a method for preparing high-strength hypoeutectoid steel, comprising the following steps:

[0008] (1) Weighing the required substrate, manganese, nickel, molybdenum, chromium, and copper according to the set weight percentage;

[0009] (2) After the base material is smelted and kept warm, manganese, nickel, molybdenum, chromium and copper are added in sequence to obtain molten steel;

[0010] (3) The molten steel is poured into the sintered shell, covered with a cover to keep it warm, and after natural cooling, the riser is cut and then heat treated to obtain high-strength hypoeutectoid steel.

[0011] Furthermore, the substrate in step (1) is 20 steel, and the weight percentage of phosphorus in the 20 steel is ≤0.015%, and the weight percentage of sulfur is ≤0.005%.

[0012] Furthermore, the smelting temperature in step (2) is 1580-1590° C., the smelting time is 30-35 min, and the insulation time is 25-35 min.

[0013] Furthermore, in step (3), the time from when the molten steel is taken out of the furnace to when the casting is completed is ≤2 minutes, the time for covering and keeping warm is 20 to 25 minutes, and the molten steel is naturally cooled to 200 to 260°C.

[0014] Furthermore, the heat treatment in step (3) includes normalizing, quenching and tempering.

[0015] Furthermore, the normalizing temperature is 895-905° C., the heat preservation time is 2.5-3.5 hours, and the steel is cooled in the air after being taken out of the furnace.

[0016] Furthermore, the quenching temperature is 875-885° C., the holding time is 2.5-3.5 hours, and the medium is fast cooling circulating water.

[0017] Furthermore, the tempering temperature is 585-595° C., the insulation time is 3.5-4.5 hours, and the steel is rapidly cooled with water after being taken out of the furnace.

[0018] Furthermore, the time from the end of quenching to the completion of loading the furnace for tempering is ≤15min.

[0019] Beneficial effects of the present invention:

[0020] The high-strength hypoeutectoid steel of the present invention has excellent mechanical properties and is suitable for special casting purposes as well as applications in welding technology. It can also be used to manufacture high-stress components in transmission systems, vehicle parts, such as buses, engineering machinery and other complex applications.

[0021] The high-strength hypoeutectoid steel of the present invention strictly controls the weight percentage of phosphorus in the chemical composition to be ≤0.015%, and the weight percentage of sulfur to be ≤0.005%, and through the heat treatment process of normalizing, quenching and tempering, the high-strength hypoeutectoid steel simultaneously achieves excellent tensile properties and low-temperature impact properties.

[0022] The heat treatment process of the present invention refines the grains and makes the structure uniform through normalizing; achieves the equilibrium state of steel through quenching, thereby improving the hardness, strength and wear resistance; and reduces the internal stress in the material during the quenching process through tempering, increases the toughness, and reduces the strength of the material at the same time. The occurrence of cracks, shrinkage and the like in high-strength hypoeutectoid steel after casting is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A physical picture of the ingot cast with the furnace / heat treated in the same furnace prepared in Example 1 of the present invention;

[0024] Figure 2 This is a mold shell pouring and riser diagram of the present invention;

[0025] Figure 3 This is a physical picture of the product prepared in Example 1 of the present invention when undergoing NDE testing;

[0026] Figure 4 This is a microstructure diagram of the ingot prepared in Example 1 of the present invention through furnace casting / heat treatment in the same furnace. DETAILED DESCRIPTION

[0027] The present invention provides a high-strength hypoeutectoid steel, wherein the weight percentages of the components in the high-strength hypoeutectoid steel are:

[0028] Carbon: 0.18~0.24%; Silicon ≤0.6%; Manganese: 0.8~1.2%; Phosphorus ≤0.015%; Sulfur ≤0.005%; Chromium: 0.5~1.0%; Nickel: 0.8~1.3%; Molybdenum: 0.5~0.7%; Copper: 0.2~0.5%; The balance is iron.

[0029] In the present invention, the weight percentage of carbon in the high-strength hypoeutectoid steel is preferably 0.19-0.23%, more preferably 0.2-0.22%; the weight percentage of silicon is preferably ≤0.5%, more preferably ≤0.4%; the weight percentage of manganese is preferably 0.9-1.1%, more preferably 0.95-1.05%; the weight percentage of phosphorus is preferably ≤0.01%, more preferably ≤0.005%; the weight percentage of sulfur is preferably ≤0.003%, more preferably ≤0.001%; ​​the weight percentage of chromium is preferably 0.6-0.9%, more preferably 0.7-0.8%; the weight percentage of nickel is preferably 1.0-1.3%, more preferably 1.2-1.3%; the weight percentage of molybdenum is preferably 0.6-0.7%, more preferably 0.65-0.7%; the weight percentage of copper is preferably 0.3-0.4%, more preferably 0.32-0.38%.

[0030] The present invention provides a method for preparing high-strength hypoeutectoid steel, comprising the following steps:

[0031] (1) Weighing the required substrate, manganese, nickel, molybdenum, chromium, and copper according to the set weight percentage;

[0032] (2) After the base material is smelted and kept warm, manganese, nickel, molybdenum, chromium and copper are added in sequence to obtain molten steel;

[0033] (3) The molten steel is poured into the sintered shell, covered with a cover to keep it warm, and after natural cooling, the riser is cut and then heat treated to obtain high-strength hypoeutectoid steel.

[0034] In the present invention, the substrate in step (1) is 20 steel, the weight percentage of phosphorus in the 20 steel is ≤0.015%, preferably ≤0.01%, more preferably ≤0.005%; the weight percentage of sulfur is ≤0.005%, preferably ≤0.003%, more preferably ≤0.001%.

[0035] In the present invention, the smelting temperature in step (2) is 1580-1590°C, preferably 1582-1588°C, and more preferably 1584-1586°C; the smelting time is 30-35min, preferably 31-34min, and more preferably 32-33min; the insulation time is 25-35min, preferably 27-33min, and more preferably 29-31min.

[0036] In the present invention, the time from when the molten steel is taken out of the furnace to when the casting is completed in step (3) is ≤2 min, preferably ≤1.5 min, and more preferably ≤1 min; the time for covering and keeping warm is 20 to 25 min, preferably 21 to 24 min, and more preferably 22 to 23 min; and the steel is naturally cooled to 200 to 260°C, preferably 210 to 250°C, and more preferably 220 to 240°C.

[0037] In the present invention, the heat treatment in step (3) includes normalizing, quenching and tempering.

[0038] In the present invention, the normalizing temperature is 895-905°C, preferably 897-903°C, and more preferably 899-901°C; the insulation time is 2.5-3.5h, preferably 2.7-3.3h, and more preferably 2.9-3.1h; and the steel is cooled in air after being taken out of the furnace.

[0039] In the present invention, the quenching temperature is 875-885°C, preferably 877-883°C, and more preferably 879-881°C; the insulation time is 2.5-3.5h, preferably 2.7-3.3h, and more preferably 2.9-3.1h; and the medium is rapid cooling circulating water.

[0040] In the present invention, the tempering temperature is 585-595°C, preferably 587-593°C, and more preferably 589-591°C; the insulation time is 3.5-4.5h, preferably 3.7-4.3h, and more preferably 3.9-4.1h; and the steel is rapidly cooled with water after being taken out of the furnace.

[0041] In the present invention, the time from the end of quenching to the completion of charging the furnace for tempering is ≤15 min, preferably ≤10 min, and more preferably ≤5 min.

[0042] In addition, the applicant has drawn the following conclusions after multiple experiments:

[0043] 1. When preparing the melt of this steel, the sulfur and phosphorus content must be strictly controlled. These two elements have a great influence on the mechanical properties of the material. Both will reduce notch toughness and generally reduce the mechanical properties of the material.

[0044] 2. Copper is an element that expands the austenite phase region, but its solid solubility in iron is not large, and copper does not form carbides with carbon; the effect of copper on the critical temperature and hardenability and its solid solution strengthening effect are similar to those of nickel, so it can be used to replace part of nickel.

[0045] Copper can improve the strength and fatigue strength of steel, especially the yield strength ratio. As the copper content increases, the room temperature impact toughness of steel increases slightly.

[0046] A small amount of copper added to steel can improve the atmospheric corrosion resistance of low alloy structural steel and rail steel, and the effect is more significant when used in combination with phosphorus.

[0047] Copper can slightly improve the high temperature oxidation resistance of steel, improve the fluidity of molten steel, and is beneficial to casting performance. However, steel with a high copper content is prone to cracking during hot working. Adding 2-3% copper by mass to stainless acid-resistant steel can improve the corrosion resistance of steel to sulfuric acid and hydrochloric acid.

[0048] The addition of copper to steel is mainly used in ordinary low-alloy steel, quenched and tempered and carburized structural steel, rail steel, stainless acid-resistant steel and cast steel; copper iron ore reserves are abundant, but the copper in it is not easy to smelt and sort. The copper in steel cannot be separated during the smelting process, so the use of copper-containing scrap steel for repeated smelting will cause the copper content in the steel to accumulate and increase; the prominent role of copper in steel is to improve the atmospheric corrosion resistance of ordinary low-alloy steel, especially when used in combination with phosphorus, adding copper can also improve the strength and yield ratio of steel, without adversely affecting welding performance. Rail steel (U-Cu) containing 0.20-0.50% copper has a corrosion resistance life of 2-5 times that of general carbon rails in addition to wear resistance; when the copper content exceeds 0.75%, after solution treatment and aging treatment, it can produce aging strengthening effect. When the content is low, its effect is similar to that of nickel, but weaker. When the content is high, it is not conducive to hot deformation processing, and copper brittleness occurs during hot deformation processing. 2-3% copper in austenitic stainless steel can improve corrosion resistance to sulfuric acid, phosphoric acid and hydrochloric acid and stability to stress corrosion. Therefore, the content of Cu element is controlled to 0.20%-0.50%.

[0049] 3. Nickel can improve the strength of steel while maintaining good plasticity and toughness. Nickel has high corrosion resistance to acids and alkalis, and has rust and heat resistance at high temperatures. Therefore, in actual smelting, the upper limit of the specified content range can be used.

[0050] 4. Chromium can significantly improve strength, hardness and wear resistance, but at the same time reduce plasticity and toughness. Chromium can also improve the oxidation resistance and corrosion resistance of steel. Therefore, the chromium content can be maintained at the existing smelting analysis content without deliberate adjustment.

[0051] 5. Molybdenum can refine the grains of steel, improve hardenability and heat resistance, and maintain sufficient strength and creep resistance at high temperatures. Adding molybdenum to structural steel can improve mechanical properties and inhibit the brittleness of alloy steel caused by quenching. Therefore, in actual smelting, the upper limit can be exceeded within the specified content range.

[0052] In addition, the present invention also provides a quality control method, which is as follows:

[0053] Quality control of wax parts: After the base material is determined, the shrinkage rate is determined to be 1%. The mold is made by casting the blank drawing, and then the wax parts are made with medium-temperature wax. When making wax parts, the wax injection pressure is selected to be 2.5-3.5MPa, and the pressure is maintained for 2 minutes to ensure that the wax is fully formed in the mold. After taking the wax parts, put them in circulating pure water at 9-11℃ to ensure a stable shrinkage rate.

[0054] Riser design and tree control: After many experiments, the applicant concluded that the risers of all products must adopt the bottom pouring process. The bottom pouring process can make impurities float up, reduce the impurity content in the product, and make the product itself fully compensated, reducing the probability of shrinkage. It can also make the product form a regular sequential solidification and reduce shrinkage defects.

[0055] Shell making process control: First, the surface layer is sanded with 200 mesh zircon powder and 80-100 mesh zircon sand, and then slurry is dipped with 200 mesh mullite powder and silica sol. After this process is repeated 6 times, it is tied and reinforced with fine iron wire to prevent deformation and increase the shell membrane strength during subsequent hardening and drying. Secondly, it is dried at a constant temperature of 20°C, and then hardened and dried at a temperature of 22-26°C and a humidity of 30-40% RH.

[0056] Dewaxing process control: After the shell is heated to 800-950℃ in the dewaxing kettle and kept warm for a period of time, the wax in it is completely removed to form a cavity, which is convenient for subsequent casting.

[0057] Shell burning and smelting and casting process control: put the shell into the roasting furnace, the roasting temperature is selected to be 1080~1100℃, and the holding time is 40min before entering the smelting and casting stage.

[0058] Key points of smelting: 100% new material smelting is required, and the smelting time is strictly controlled. Exceeding this time will cause the chemical composition P / S elements to exceed the standard. Strictly control the time from molten steel leaving the furnace to the completion of pouring to prevent decarburization and re-oxidation of molten steel, and avoid defects such as insufficient carbon content and surface pits on the product.

[0059] Key points of casting and cutting risers: Wrap the die head and internal risers with 20mm thick aluminum silicate, cover the barrels for insulation after casting, and cover the barrels for 20 to 25 minutes; after removing the cover, let the cast products cool naturally to 200 to 260℃ before starting to cut the risers (hot cutting) to prevent cold cracks in the internal risers; perform 100% PT flaw detection after cutting, grind the risers after passing the test, and then perform a second PT flaw detection to determine whether there are cracks. The PT flaw detection method complies with ASTM E165, and the acceptance standard complies with AMS2175Class C requirements.

[0060] Key points of heat treatment: Normalizing is to refine the grains and make the structure uniform. The purpose of quenching is to achieve a balanced state of steel, thereby improving hardness, strength and wear resistance. The purpose of tempering is to reduce the internal stress in the material during quenching, increase toughness, and reduce the strength of the material. Generally speaking, the hardness after heat treatment can reflect its tensile properties to a certain extent. When other heat treatment process parameters remain unchanged, the lower the tempering temperature, the higher the hardness, the tensile strength (Rm) and yield strength (Rp0.2) will increase, but the brittleness will increase to a certain extent, therefore, it will often cause the elongation after fracture (A) and the reduction of area (Z) to decrease. At the same time, the low-temperature impact performance depends largely on the grain size, and normalizing can refine the grains. Generally speaking, the higher the grain size grade, the finer the grains, and the better the impact performance.

[0061] In view of the poor hardenability of this special material, in order to fully harden the component and obtain excellent mechanical properties at its core, the quenching medium is selected as fast cooling circulating water. After room temperature quenching, the water temperature increases by less than 10°C and is loaded into the tempering furnace within 15 minutes. After tempering and heat preservation, water rapid cooling must be used to prevent the second type of temper brittleness. When water is used as both the quenching medium and the tempering medium, although some excellent performance indicators can be obtained, it is easy to cause cracks in the casting. At the same time, it was found that this special material is very sensitive to temperature. When we conducted heat treatment experiments, the gradient of the insulation temperature change was 10°C. The insulation time of each process is determined by the maximum thickness of the casting, and is calculated according to the minimum 2.0 minutes / thickness (mm) + 1 hour. Therefore, the heating temperature and insulation time of each process are extremely important.

[0062] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0063] Example 1

[0064] Weigh 20 steel, manganese, nickel, molybdenum, chromium, and copper, wherein the weight percentage of each element is 0.21% carbon, 0.3% silicon, 1% manganese, 0.015% phosphorus, 0.005% sulfur, 0.75% chromium, 1.3% nickel, 0.7% molybdenum, 0.35% copper, and 95.37% iron. Smelt the 20 steel at 1585°C for 33 minutes, keep it warm for 30 minutes, then add manganese, nickel, molybdenum, chromium, and copper in sequence to obtain molten steel. Pour the molten steel into the calcined shell within 2 minutes, cover it and keep it warm for 23 minutes, cool it naturally to 230°C, cut the riser, and then perform normalizing, quenching, and tempering to obtain an alloy material.

[0065] The normalizing temperature is 900℃, the holding time is 3h, and it is cooled in the air after being taken out of the furnace; the quenching temperature is 880℃, the holding time is 3h, and the medium is fast cooling circulating water; the time from the end of quenching to the completion of furnace loading for tempering is 10min, the tempering temperature is 590℃, the holding time is 4h, and it is rapidly cooled with water after being taken out of the furnace.

[0066] After testing, the alloy material has a tensile strength of 930MPa, a yield strength of 840MPa, an elongation of 13%, a cross-sectional shrinkage of 28%, an HBW hardness of 313, and an impact energy KV8 of 46J, 45J, and 47J at -40°C, with an average of 46J.

[0067] Example 2

[0068] Weigh 20 steel, manganese, nickel, molybdenum, chromium, and copper, wherein the weight percentage of each element is 0.21% carbon, 0.3% silicon, 1% manganese, 0.015% phosphorus, 0.005% sulfur, 0.75% chromium, 1.0% nickel, 0.6% molybdenum, 0.25% copper, and 95.87% iron. Smelt the 20 steel at 1585°C for 33 minutes, keep it warm for 30 minutes, then add manganese, nickel, molybdenum, chromium, and copper in sequence to obtain molten steel. Pour the molten steel into the calcined shell within 2 minutes, cover it and keep it warm for 23 minutes, cool it naturally to 230°C, cut the riser, and then perform normalizing, quenching, and tempering to obtain an alloy material.

[0069] The normalizing temperature is 900℃, the holding time is 3h, and it is cooled in the air after being taken out of the furnace; the quenching temperature is 880℃, the holding time is 3h, and the medium is fast cooling circulating water; the time from the end of quenching to the completion of furnace loading for tempering is 10min, the tempering temperature is 590℃, the holding time is 4h, and it is rapidly cooled with water after being taken out of the furnace.

[0070] After testing, the alloy material has a tensile strength of 910MPa, a yield strength of 810MPa, an elongation of 16%, a cross-sectional shrinkage of 30%, and an impact energy KV8 of 48J, 41J, and 39J at -40°C, with an average of 43J.

[0071] Example 3

[0072] Weigh 20 steel, manganese, nickel, molybdenum, chromium, and copper, wherein the weight percentage of each element is 0.21% carbon, 0.3% silicon, 1% manganese, 0.015% phosphorus, 0.005% sulfur, 0.75% chromium, 1.3% nickel, 0.7% molybdenum, 0.35% copper, and 95.37% iron. Smelt the 20 steel at 1585°C for 33 minutes, keep it warm for 30 minutes, then add manganese, nickel, molybdenum, chromium, and copper in sequence to obtain molten steel. Pour the molten steel into the calcined shell within 2 minutes, cover it and keep it warm for 23 minutes, cool it naturally to 230°C, cut the riser, and then perform normalizing, quenching, and tempering to obtain an alloy material.

[0073] The normalizing temperature is 895℃, the holding time is 3h, and it is cooled in the air after being taken out of the furnace; the quenching temperature is 875℃, the holding time is 3h, and the medium is fast cooling circulating water; the time from the end of quenching to the completion of furnace loading for tempering is 10min, the tempering temperature is 585℃, the holding time is 4h, and it is rapidly cooled with water after being taken out of the furnace.

[0074] After testing, the alloy material has a tensile strength of 945MPa, a yield strength of 850MPa, an elongation of 12%, a cross-sectional shrinkage of 25%, an HBW hardness of 321, and an impact energy KV8 of 45J, 40J, and 41J at -40°C, with an average of 42J.

[0075] Example 4

[0076] Weigh 20 steel, manganese, nickel, molybdenum, chromium, and copper, wherein the weight percentage of each element is 0.21% carbon, 0.3% silicon, 1% manganese, 0.015% phosphorus, 0.005% sulfur, 0.75% chromium, 1.3% nickel, 0.7% molybdenum, 0.35% copper, and 95.37% iron. Smelt the 20 steel at 1585°C for 33 minutes, keep it warm for 30 minutes, then add manganese, nickel, molybdenum, chromium, and copper in sequence to obtain molten steel. Pour the molten steel into the calcined shell within 2 minutes, cover it and keep it warm for 23 minutes, cool it naturally to 230°C, cut the riser, and then perform normalizing, quenching, and tempering to obtain an alloy material.

[0077] The normalizing temperature is 905℃, the holding time is 3h, and it is cooled in the air after being taken out of the furnace; the quenching temperature is 885℃, the holding time is 3h, and the medium is fast cooling circulating water; the time from the end of quenching to the completion of furnace loading for tempering is 10min, the tempering temperature is 595℃, the holding time is 4h, and it is rapidly cooled with water after being taken out of the furnace.

[0078] After testing, the alloy material has a tensile strength of 922MPa, a yield strength of 830MPa, an elongation of 16%, a cross-sectional shrinkage of 30%, an HBW hardness of 305, and an impact energy KV8 of 45J, 41J, and 46J at -40°C, with an average of 44J.

[0079] Comparative Example 1

[0080] Only the heat treatment conditions are different from those in Example 1. The normalizing temperature is 910°C, the holding time is 3 hours, and the furnace is cooled in the air; the quenching temperature is 880°C, the holding time is 3 hours, and the medium is rapid cooling circulating water; the time from the end of quenching to the completion of furnace loading for tempering is 15 minutes, the tempering temperature is 580°C, the holding time is 4 hours, and the furnace is rapidly cooled with water.

[0081] After testing, the tensile strength of the alloy material is 940MPa, the yield strength is 907MPa, the elongation after fracture is 6%, the cross-sectional shrinkage is 11%, the HBW hardness is 330, the impact energy KV8 at -40℃ is 36J, 28J, and 39J, with an average of 34J, and the impact energy KV8 at -20℃ is 35J, 45J, and 41J, with an average of 40J.

[0082] Comparative Example 2

[0083] The only difference from Example 1 is the heat treatment conditions. The normalizing temperature is 910°C, the holding time is 3 hours, and the furnace is cooled in the air; the quenching temperature is 880°C, the holding time is 3 hours, and the medium is rapid cooling circulating water; the time from the end of quenching to the completion of the furnace loading and tempering is 15 minutes, the tempering temperature is 590°C, the holding time is 4 hours, and the furnace is rapidly cooled with water.

[0084] After testing, the alloy material has a tensile strength of 910MPa, a yield strength of 832MPa, an elongation of 12%, a cross-sectional shrinkage of 26%, an HBW hardness of 310, and an impact energy KV8 of 29J, 41J, and 36J at -40°C, with an average of 35J. The impact energy KV8 of 48J, 47J, and 28J at -20°C, with an average of 41J.

[0085] The product obtained in Example 1 was subjected to NDE testing, and the castings and heat treatment were inspected by a fully automatic magnetic particle flaw detector (MT). The testing method complies with ASTM E709, and the acceptance criteria comply with the requirements of ASTM E125. No obvious defects were found in the product, which meets the requirements for product surface defect control, and the product surface is qualified.

[0086] The heat-treated product is fully inspected by a radiographic flaw detector (RT). The inspection method complies with ASTM E94 and the acceptance criteria comply with ASTM E446. No obvious defects are found in the product, which complies with the requirements for product internal defect control and the product internal defect control is qualified.

[0087] It can be seen from the above embodiments that the present invention provides a high-strength hypoeutectoid steel and a preparation method thereof. The constituent elements and weight percentages in the high-strength hypoeutectoid steel of the present invention are carbon: 0.18-0.24%; silicon ≤0.6%; manganese: 0.8-1.2%; phosphorus ≤0.015%; sulfur ≤0.005%; chromium: 0.5-1.0%; nickel: 0.8-1.3%; molybdenum: 0.5-0.7%; copper: 0.2-0.5%; the balance is iron. The present invention also provides a preparation method for the above-mentioned high-strength hypoeutectoid steel, weighing the required substrate, manganese, nickel, molybdenum, chromium, and copper according to the set weight percentage, then smelting and heat-insulating the substrate, and then adding manganese, nickel, molybdenum, chromium, and copper in sequence to obtain molten steel. The molten steel is cast into the calcined shell, covered and heat-insulated, and the riser is cut after natural cooling, and then heat-treated to obtain high-strength hypoeutectoid steel. The present invention obtains high-strength hypoeutectoid steel with excellent tensile properties and low-temperature impact properties by strictly controlling the composition and content of chemical components, as well as the normalizing, quenching and tempering heat treatment processes. The steel is suitable for special casting purposes and applications in welding technology, and can be used to manufacture high-stress components in transmission systems, vehicle parts, such as buses, engineering machinery and other complex applications.

[0088] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A high strength hypoeutectoid steel, characterized in that: The weight percentage of each component in the high-strength hypoeutectoid steel is: Carbon: 0.18~0.24%; Silicon ≤0.6%; Manganese: 0.8-1.2%; Phosphorus ≤ 0.015%; Sulfur ≤ 0.005%; Chromium: 0.5-1.0%; Nickel: 0.8-1.3%; Molybdenum: 0.5-0.7%; Copper: 0.2-0.5%; the balance is iron.

2. The method for preparing high-strength hypoeutectoid steel according to claim 1, characterized in that: The following steps are involved: (1) Weighing the required substrate, manganese, nickel, molybdenum, chromium, and copper according to the set weight percentage; (2) After the base material is smelted and kept warm, manganese, nickel, molybdenum, chromium and copper are added in sequence to obtain molten steel; (3) The molten steel is poured into the sintered shell, covered with a cover to keep it warm, and after natural cooling, the riser is cut and then heat treated to obtain high-strength hypoeutectoid steel.

3. The preparation method according to claim 2, characterized in that: The substrate described in step (1) is 20 steel; The weight percentage of phosphorus in the 20 steel is ≤0.015%, and the weight percentage of sulfur is ≤0.005%.

4. The preparation method according to claim 2 or 3, characterized in that: The smelting temperature in step (2) is 1580-1590° C., the smelting time is 30-35 min, and the insulation time is 25-35 min.

5. The preparation method according to claim 4, characterized in that: The time from when the molten steel is taken out of the furnace to when the casting is completed in step (3) is ≤2min, the time for covering and keeping warm is 20-25min, and the molten steel is naturally cooled to 200-260°C.

6. The preparation method according to claim 2, 3 or 5, characterized in that: The heat treatment described in step (3) includes normalizing, quenching and tempering.

7. The preparation method according to claim 6, characterized in that: The normalizing temperature is 895-905°C, the heat preservation time is 2.5-3.5h, and the steel is cooled in the air after being taken out of the furnace.

8. The preparation method according to claim 6, characterized in that: The quenching temperature is 875-885° C., the holding time is 2.5-3.5 hours, and the medium is fast cooling circulating water.

9. The preparation method according to claim 7 or 8, characterized in that: The tempering temperature is 585-595° C., the holding time is 3.5-4.5 hours, and the furnace is rapidly cooled with water.

10. The preparation method according to claim 9, characterized in that: The time from the end of quenching to the completion of loading the furnace for tempering is ≤15min.