Wear-resistant steel plate capable of being used in high-temperature working condition and preparation method thereof

By adjusting the chemical composition and process flow in wear-resistant steel, wear-resistant steel plates that maintain high hardness and strength at high temperatures of 300°C to 600°C were prepared, which solved the problem of hardness loss of existing wear-resistant steels at high temperatures. Reduced production costs.

CN118979203APending Publication Date: 2024-11-19NANJING IRON & STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411105995.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing wear-resistant steel has severe hardness loss at working temperatures above 300℃, and its wear-resistant alloy steel used in high-temperature working conditions has high cost and limited performance, which affects its service life.

Method used

Chemical components are C≤0.25%, Si≤0.70%, Mn≤1.60%, P≤0.025%, S≤0.010%, Ni≤1.50%, Cr≤1.40%, Mo≤1.50%, Rare Earth+Nb≤0.1% The steel plate is prepared by electric furnace smelting, casting, rolling and heat treatment processes, including quenching and tempering treatment, controlling the heating temperature and time, and refining the grains with Nb carbides, ensuring solid solution of alloy elements and preventing abnormally long grains. Large, improve hardness and strength.

Benefits of technology

The prepared wear-resistant steel plate maintains high hardness and strength under high temperature conditions of 300℃ to 600℃, with tensile strength ≥1100MPa, surface hardness 370-430HBW, impact work ≥45J in -40℃, high-temperature yield strength ≥600MPa, high-temperature hardness ≥ 300HBW, extending service life and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979203A_ABST
    Figure CN118979203A_ABST
Patent Text Reader

Abstract

The invention discloses a wear-resistant steel plate applicable to a high-temperature working condition and a preparation method thereof, and relates to the technical field of steel production, and the wear-resistant steel plate comprises the following chemical components in percentage by mass: less than or equal to 0.25% of C, less than or equal to 0.70% of Si, less than or equal to 1.60% of Mn, less than or equal to 0.025% of P, less than or equal to 0.010% of S, less than or equal to 1.50% of Ni, less than or equal to 1.40% of Cr, less than or equal to 1.50% of Mo, less than or equal to 0.1% of rare earth + Nb, and the balance of Fe and inevitable impurities. The wear-resistant steel plate capable of being used for the high-temperature working condition can reach the following performance indexes that the tensile strength is larger than or equal to 1100 MPa, the surface hardness is 370-430 HBW, the impact energy at the temperature of-40 DEG C is larger than or equal to 45 J, and the high-temperature yield strength is larger than or equal to 600 MPa and the high-temperature hardness is larger than or equal to 300 HBW at the temperature of 300 DEG C, 400 DEG C, 500 DEG C and 600 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel production, and in particular to a wear-resistant steel plate that can be used in high-temperature working conditions and a preparation method thereof. Background Art

[0002] Wear-resistant steel, as an important wear-resistant material, is widely used in the production and manufacturing of engineering machinery, mining machinery and other equipment due to its good comprehensive performance and relatively low production cost. With the continuous development of science and technology, the service conditions of mechanical parts are becoming more and more severe. Ordinary wear-resistant steel has a serious loss of hardness and a sharp decline in wear resistance at working temperatures above 300°C, which significantly reduces the life of its manufacturing equipment.

[0003] At present, conventional wear-resistant steel is used, and its performance indicators are mainly to ensure strength, hardness and toughness. This type of steel plate mainly uses martensite as the matrix structure, and the production process generally adopts quenching + low-temperature tempering at about 200℃. For example, CN201610540258.X "A low-alloy high-strength wear-resistant steel plate and its production method" adds Ni, Cr, Mo hardenability elements and Nb, V, Ti fine-grained elements. The rolled steel plate is quenched at 925±10℃ and tempered at 230±5℃ to obtain a wear-resistant steel with a Brinell hardness value of 470~510HBW and a longitudinal impact energy of ≥35J at -20℃. The steel materials used in the manufacture of high-temperature wear parts are mainly high-chromium, high-tungsten and high-vanadium alloys. Some patents also add rare elements and rare earths. They are prepared by casting, which is not only extremely costly, but also has a large brittle vector, which is not conducive to the large-scale promotion and use of wear-resistant and consumable parts. For example, invention patent CN1335417 discloses a high-temperature wear alloy steel and a production method thereof, which adds more chromium, molybdenum, vanadium and rare earth elements; invention patent CN1908219 discloses a high-temperature resistant, wear-resistant and oxidation-resistant alloy steel and a preparation method thereof, which not only adds more chromium, nickel and molybdenum elements, but also adds a certain amount of tungsten and cobalt elements.

[0004] The production method of conventional wear-resistant steel involved in the above patent is mainly to improve hardness and low-temperature impact toughness. The tempering temperature is generally around 200°C, and the ambient temperature of use is mostly room temperature, which will not affect the hardness. When the ambient temperature of use exceeds 300°C, the hardness decreases significantly, the wear of wear-resistant parts accelerates, and the service life is seriously affected. The wear-resistant alloy steel used for high-temperature working conditions is mainly high-chromium, high-tungsten and high-vanadium alloys. The addition of a large number of precious elements not only consumes a lot of resources and increases production costs, but also has certain limitations in high-temperature wear resistance. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the disadvantages of the prior art and provide a wear-resistant steel plate that can be used in high-temperature working conditions and a preparation method thereof.

[0006] In order to solve the above technical problems, the technical solution of the present invention is as follows: A wear-resistant steel plate that can be used in high-temperature working conditions has the following chemical composition and mass percentage: C≤0.25%, Si≤0.70%, Mn≤1.60%, P≤0.025%, S≤0.010%, Ni≤1.50%, Cr≤1.40%, Mo≤1.50%, rare earth+Nb≤0.1%, and the balance is Fe and unavoidable impurities.

[0007] The present invention also provides a method for preparing a wear-resistant steel plate that can be used in high-temperature working conditions, comprising: Electric furnace smelting: add molybdenum, nickel, niobium, chromium, manganese, silicon and rare earth silicon in sequence, and the smelting furnace temperature is 1600-1620℃ to obtain molten steel; Pouring: pouring molten steel to obtain slabs; Rolling: The slab is heated, and after being heated, the recrystallization zone rolling and the non-recrystallization zone rolling are performed; Heat treatment: The slab is quenched and tempered after quenching.

[0008] As a preferred embodiment of the method for preparing the wear-resistant steel plate that can be used in high-temperature working conditions of the present invention, the heating temperature of the slab in the rolling process is 790-950°C.

[0009] As a preferred embodiment of the method for preparing the wear-resistant steel plate that can be used in high-temperature working conditions of the present invention, the soaking time in the rolling process is 30 to 50 minutes.

[0010] As a preferred embodiment of the method for preparing the wear-resistant steel plate that can be used in high temperature working conditions described in the present invention, the final rolling temperature of the recrystallization zone rolling in the rolling process is 1000-1100°C, and the final rolling temperature of the non-recrystallization zone rolling is 790-950°C.

[0011] As a preferred solution of the method for preparing the wear-resistant steel plate that can be used in high-temperature working conditions of the present invention, wherein: in the quenching process, the quenching temperature is AC3+ (20-50)°C.

[0012] As a preferred solution of the method for preparing the wear-resistant steel plate that can be used in high temperature working conditions described in the present invention, in the quenching process, when the slab thickness is ≤20mm, the heating time is the plate thickness + 30min; when the thickness is greater than 20mm, the heating time is 2.5 times the plate thickness.

[0013] As a preferred embodiment of the method for preparing the wear-resistant steel plate that can be used in high-temperature working conditions of the present invention, the temperature of the tempering treatment is 400-550°C.

[0014] The beneficial effects of the present invention are: (1) The present invention is designed to add a certain amount of Cr and Mo alloys, and the heating process ensures that the alloy elements are dissolved as much as possible. The heating temperature is controlled at 1200-1250°C, and the pinning effect of Nb carbides is used to refine the grains during the rolling process.

[0015] (2) When the present invention performs the heat treatment process, the AC3 temperature is calculated according to the chemical composition of the steel, and the heating temperature is controlled under the premise of ensuring the solid solution of the alloy to prevent abnormal grain growth. At the same time, conventional wear-resistant steel generally uses low-temperature tempering to eliminate stress. As the tempering temperature increases, the martensite laths recover, the laths merge and disappear, the dislocation density decreases, and the strength and hardness gradually decrease. In order to ensure that the hardness of the steel does not decrease significantly during use, its tempering temperature must be higher than the ambient temperature of use. The tempering temperature designed by the present invention is 400-550℃.

[0016] (3) The wear-resistant steel plate produced by the present invention and applicable to high temperature working conditions can achieve the following performance indicators: tensile strength ≥1100MPa, surface hardness: 370-430HBW, -40℃ impact energy ≥45J, high temperature yield strength ≥600MPa and high temperature hardness ≥300HBW at 300℃, 400℃, 500℃ and 600℃. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0018] Figure 1 and Figure 2 A schematic diagram of the metallographic structure of the wear-resistant steel plate that can be used in high-temperature working conditions provided by the present invention. DETAILED DESCRIPTION

[0019] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific implementation modes and in combination with the accompanying drawings.

[0020] The present application provides a wear-resistant steel plate that can be used in high-temperature working conditions, wherein the microstructure of the steel is lath martensite. The chemical composition and mass percentage of the steel are as follows: C≤0.25%, Si≤0.70%, Mn≤1.60%, P≤0.025%, S≤0.010%, Ni≤1.50%, Cr≤1.40%, Mo≤1.50%, rare earth+Nb≤0.1%, and the balance is Fe and unavoidable impurities.

[0021] The present application also provides a method for preparing a wear-resistant steel plate that can be used in high temperature working conditions, the method specifically comprising the following steps: Step S101: electric furnace smelting: add ferromolybdenum, nickel plate, ferroniobium, low carbon chromium, ferromanganese, ferrosilicon and rare earth ferrosilicon in sequence, and the smelting temperature is 1600-1620°C to obtain molten steel, and the chemical composition of the obtained molten steel is as follows by weight percentage: C≤0.25%, Si≤0.70%, Mn≤1.60%, P≤0.025%, S≤0.010%, Ni≤1.50%, Cr≤1.40%, Mo≤1.50%, rare earth+Nb≤0.1%, and the balance is Fe and unavoidable impurities.

[0022] Step S102: Pouring: pouring molten steel to obtain a slab with a thickness of 220-460 mm.

[0023] Step S101: rolling: heating the slab to 1180-1250°C, soaking time 30-50 minutes, and then performing recrystallization zone rolling and non-recrystallization zone rolling. The final rolling temperature of the recrystallization zone rolling is 1000-1100°C, and the final rolling temperature of the non-recrystallization zone rolling is 790-950°C.

[0024] Step S101: Heat treatment: The slab is quenched at a temperature of AC3+(20-50)°C. When the slab thickness is ≤20mm, the heating time is the slab thickness+30min; when the thickness is >20mm, the heating time is 2.5 times the slab thickness. After quenching, tempering is performed at a temperature of 400-550°C.

[0025] The technical solution of this application is described below through specific embodiments: According to the chemical composition requirements of the steel in this application and in combination with the preparation process, wear-resistant steels of different specifications are prepared. The specific composition is shown in Table 1.

[0026]

[0027] Table 1 The smelted steel billet is used according to the method to produce heat-resistant and wear-resistant steel plates by using the method of controlled rolling air cooling + offline heat treatment, which is specifically implemented as follows: Example 1: The molten steel smelted according to the composition of Example 1 in Table 1 was subjected to vacuum degassing and then continuously cast. The continuous casting billet thickness was 220 mm. The billet was heated to a furnace temperature of 1200°C, kept warm for 180 minutes, and then taken out of the furnace for austenite recrystallization rolling and non-recrystallization zone rolling. The final rolling temperature of the recrystallization zone was 1030°C, and the final rolling temperature of the non-recrystallization zone was 840°C. The final rolling thickness of the steel plate was 30 mm. After rolling, it was air-cooled to room temperature, and then offline quenching and tempering were performed. The quenching temperature was 910°C, the heating time was 40 minutes; the tempering temperature was 450°C, and the tempering time was 50 minutes.

[0028] Example 2: The molten steel smelted according to the composition of Example 2 in Table 1 was subjected to vacuum degassing and then continuously cast. The thickness of the continuous casting billet was 320 mm. The billet was heated to a furnace temperature of 1150°C, kept warm for 220 minutes, and then taken out of the furnace for austenite recrystallization rolling and non-recrystallization zone rolling. The final rolling temperature of the recrystallization zone was 1010°C, and the final rolling temperature of the non-recrystallization zone was 840°C. The final rolling thickness of the steel plate was 40 mm. After rolling, it was air-cooled to room temperature, and then offline quenching and tempering were performed. Then offline quenching and tempering were performed. Quenching temperature was 910°C, heating time was 40 minutes; tempering temperature was 500°C, and tempering time was 50 minutes.

[0029] Example 3: The molten steel smelted according to the composition of Example 3 in Table 1 was subjected to vacuum degassing and then continuously cast. The thickness of the continuous casting billet was 370 mm. The billet was heated to a furnace temperature of 1250°C, kept warm for 220 minutes, and then taken out of the furnace for austenite recrystallization rolling and non-recrystallization zone rolling. The final rolling temperature of the recrystallization zone was 1040°C, and the final rolling temperature of the non-recrystallization zone was 850°C. The final rolling thickness of the steel plate was 60 mm. After rolling, it was air-cooled to room temperature and then offline quenching and tempering were performed. Then offline quenching and tempering were performed. Then offline quenching and tempering were performed. Quenching temperature was 900°C, heating time was 45 minutes; tempering temperature was 500°C, and tempering time was 55 minutes.

[0030] Example 4: The molten steel smelted according to the composition of Example 4 in Table 1 was subjected to vacuum degassing and then continuously cast. The thickness of the continuous casting billet was 460 mm. The billet was heated to a furnace temperature of 1200°C, kept warm for 200 minutes, and then taken out of the furnace for austenite recrystallization rolling and non-recrystallization zone rolling. The final rolling temperature of the recrystallization zone was 1020°C, and the final rolling temperature of the non-recrystallization zone was 860°C. The final rolling thickness of the steel plate was 100 mm. After rolling, it was air-cooled to room temperature and then offline quenching and tempering were performed. Then offline quenching and tempering were performed. Then offline quenching and tempering were performed. Quenching temperature was 900°C, heating time was 40 minutes; tempering temperature was 550°C, and tempering time was 45 minutes.

[0031] Example 5: The molten steel smelted according to the composition of Example 5 in Table 1 was subjected to vacuum degassing and then continuously cast. The thickness of the continuous casting billet was 320 mm. The billet was heated to a furnace temperature of 1250°C, kept warm for 200 minutes, and then taken out of the furnace for austenite recrystallization rolling and non-recrystallization zone rolling. The final rolling temperature of the recrystallization zone was 1030°C, and the final rolling temperature of the non-recrystallization zone was 825°C. The final rolling thickness of the steel plate was 40 mm. After rolling, it was air-cooled to room temperature and then offline quenching and tempering were performed. Then offline quenching and tempering were performed. Then offline quenching and tempering were performed. Quenching temperature was 900°C, heating time was 45 minutes; tempering temperature was 500°C, and tempering time was 50 minutes.

[0032] The mechanical properties of the steel plate in the embodiment were tested, wherein the room temperature strength and high temperature strength were tested according to the room temperature tensile test method for metal materials in GB / T228.1 and GB / T228.2; the low temperature impact toughness was measured according to the Charpy pendulum impact test method for metal materials in GB / T 229; the hardness was measured according to the Brinell hardness test for metal materials in GB / T 231.1 Part 1: Test method; the wear test was carried out on a high temperature friction and wear testing machine with a wear time of 15 min. The results are shown in Table 2.

[0033]

[0034] Table 2 It can be seen from the above table that the wear-resistant steel plate prepared by the present invention for high temperature working conditions has a Brinell hardness of more than 400 HB, a yield strength of more than 1100 MPa, an impact energy of more than 40 J at -40 °C, a yield strength of ≥ 600 MPa, a surface hardness of ≥ 300 HBW, and a wear rate of ≤ 1.60 × 10 -4 mm 3 / N·m, and the high temperature wear resistance is better than HiTemp. It can be seen that the wear-resistant steel plate for high temperature working conditions prepared by the present invention not only has high strength, hardness and good low temperature toughness, but also has excellent high temperature strength and high temperature wear resistance.

[0035] In addition to the above embodiments, the present invention may also have other implementation modes; any technical solutions formed by equivalent replacement or equivalent transformation shall fall within the protection scope required by the present invention.

Claims

1. A wear-resistant steel plate that can be used in high temperature working conditions, characterized in that: Its chemical composition and mass percentage are as follows: C≤0.25%, Si≤0.70%, Mn≤1.60%, P≤0.025%, S≤0.010%, Ni≤1.50%, Cr≤1.40%, Mo≤1.50%, rare earth+Nb≤0.1%, and the balance is Fe and unavoidable impurities.

2. A method for preparing a wear-resistant steel plate that can be used in high temperature working conditions based on claim 1, characterized in that: include: Electric furnace smelting: add molybdenum, nickel, niobium, chromium, manganese, silicon and rare earth silicon in sequence, and the smelting furnace temperature is 1600-1620℃ to obtain molten steel; Pouring: pouring molten steel to obtain slabs; Rolling: The slab is heated, and after being heated, the recrystallization zone rolling and the non-recrystallization zone rolling are performed; Heat treatment: The slab is quenched and tempered after quenching.

3. The method for preparing the wear-resistant steel plate that can be used in high temperature working conditions according to claim 2, characterized in that: The heating temperature of the slab in the rolling process is 790-950°C.

4. The method for preparing the wear-resistant steel plate that can be used in high temperature working conditions according to claim 2, characterized in that: The soaking time in the rolling process is 30 to 50 minutes.

5. The method for preparing the wear-resistant steel plate that can be used in high temperature working conditions according to claim 2, characterized in that: In the rolling process, the final rolling temperature of the recrystallization zone rolling is 1000-1100° C., and the final rolling temperature of the non-recrystallization zone rolling is 790-950° C.

6. The method for preparing the wear-resistant steel plate that can be used in high temperature working conditions according to claim 2, characterized in that: In the quenching process, the quenching temperature is AC3+ (20-50)°C.

7. The method for preparing the wear-resistant steel plate that can be used in high temperature working conditions according to claim 2, characterized in that: In the quenching process, when the slab thickness is ≤20 mm, the heating time is the slab thickness+30 min; when the thickness is greater than 20 mm, the heating time is 2.5 times the slab thickness.

8. The method for preparing the wear-resistant steel plate that can be used in high temperature working conditions according to claim 2, characterized in that: The temperature of the tempering treatment is 400-550°C.

Citation Information

Cited By

  • Corrosion-resistant wear-resistant steel and manufacturing method thereof

    CN119710468A