Production method of efficient anti-fatigue aluminum alloy cast rod
Through solid solution, aging, super freezing and heat treatment, combined with hydraulic and centrifugal technology, the temperature uneven problem caused by aluminum liquid retention in the production of aluminum alloy casting rods is solved, and the fatigue resistance of aluminum alloy casting rods is significantly improved. Meets the application requirements of high fatigue resistance.
Patent Information
- Application Number
- CN202411076853.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
AI Technical Summary
During the production process of aluminum alloy casting rods, the temperature is uneven due to the retention of aluminum liquid, resulting in different cooling speeds and cooling degrees of casting rods, which are prone to cracks and coarse grains, which affects fatigue resistance and limits their use in aviation, high-speed rail, and new energy sources Applications in other fields.
A series of treatment steps include solution treatment, aging treatment, primary and secondary super-freezing treatment, primary and secondary heat treatment, combined with hydraulic press and centrifugal turntable technology, significantly improve the density of aluminum alloy castings through alternating treatment with extreme cold and high temperatures. and fatigue resistance, avoiding the use of refiners.
The internal densification of aluminum alloy casting rods has been achieved, which significantly improves fatigue resistance, ensures product stability and efficient production, and meets the high requirements in the fields of aviation, high-speed rail, new energy, etc.
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod, and belongs to the technical field of aluminum alloy cast rod production. Background Art
[0002] In the field of aluminum alloy casting rod production, when casting large-diameter or some special aluminum alloy casting rods, due to the process requirements of setting a slower casting speed and higher casting temperature, the aluminum liquid usually stays in the flow channel and mold for a long time, which easily causes uneven temperature of the aluminum alloy melt in the crystallizer, resulting in different cooling speeds and cooling degrees in various parts of the casting rod, resulting in crack tendency, and even eventually cracks inside the casting rod. Moreover, if the aluminum liquid stays for too long, it will also cause grain growth, resulting in structural defects such as coarse grains, which will affect the comprehensive performance of subsequent products.
[0003] It is well known in the industry that the size of the aluminum alloy grains determines the performance of the aluminum alloy to a large extent. The finer the grains, the better the plasticity and toughness of the aluminum alloy material, and the greater the strength. If during the aluminum alloy casting process, it is found that the grains of the cast rod structure are coarse after casting, it is easy to cause serious segregation, which will greatly affect the fatigue resistance of the aluminum alloy, thus limiting its application in aviation, high-speed rail, new energy and other fields.
[0004] A common method in the prior art is to improve some process parameters such as casting speed, casting temperature and cooling water pressure according to different aluminum alloys and rod diameters of aluminum alloy cast rods, and to add refiners to the melt in the flow channel before casting to inhibit grain coarsening and reduce the occurrence of cracks. However, this method has poor stability, and the retention of aluminum liquid will also cause the effect of the refiner to deteriorate.
[0005] Based on this, the present invention is proposed. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a method for producing an efficient fatigue-resistant aluminum alloy cast rod. The specific technical scheme is as follows:
[0007] A method for producing an efficient fatigue-resistant aluminum alloy cast rod comprises the following steps:
[0008] Step S1, melting, alloying, refining, slagging, standing, degassing, and water-cooling casting the aluminum alloy raw materials to obtain an aluminum alloy ingot;
[0009] Step S2, subjecting the aluminum alloy ingot to solution treatment, aging treatment, primary super freezing treatment, primary heat treatment, secondary super freezing treatment, secondary heat treatment, and cooling to room temperature to obtain an aluminum alloy blank;
[0010] Step S3: extruding the aluminum alloy blank to obtain an aluminum alloy cast rod.
[0011] As a further improvement, in step S2, the process of the first-level super freezing treatment is as follows:
[0012] The aluminum alloy ingot is first cold pressed by a hydraulic press with an initial cold pressure of 11.5 bar, and then poured into liquid nitrogen for cooling, and the cooling temperature is controlled at -60°C to -65°C; when the cooling temperature is between -70°C and -80°C, the cold pressure changes periodically, and the cooling time is 30 minutes. Within one cycle, the cold pressure is first increased to 15 bar at a rate of 0.5 bar / min, and then decreased to 12 bar at a rate of 1 bar / min; the pressure head of the hydraulic press is in direct contact with the aluminum alloy ingot and completely covers the aluminum alloy ingot, and the pressure head temperature of the hydraulic press is always maintained at 20 to 25°C.
[0013] As a further improvement, in step S2, a hydraulic press is used for heat treatment, with an initial heat pressure of 1.2 bar, a heat treatment temperature of 130° C., and a heat treatment time of 3 h.
[0014] As a further improvement, in step S2, the process of the secondary super freezing treatment is as follows:
[0015] The aluminum alloy ingot was cold pressed by a hydraulic press, and the cold pressure was always 13 bar. Then liquid nitrogen was poured into it for cooling. The cooling temperature was controlled at -90°C to -100°C, and the cooling time was 30 minutes.
[0016] As a further improvement, in step S2, the secondary heat treatment process is as follows:
[0017] The aluminum alloy ingot is placed on a centrifugal turntable for centrifugation at a speed of 800 r / min, and then hot air at 150-160° C. is introduced for heating and insulation for 1 hour.
[0018] As a further improvement, in step S1, during the refining process, vacuum degassing is used for refining and degassing.
[0019] As a further improvement, in step S2, the temperature of the solution treatment is 520-560°C, and the solution treatment time is 30-60 minutes.
[0020] As a further improvement, in step S2, the aging treatment temperature is 180-200°C and the time is 1-2 hours.
[0021] As a further improvement, in step S1, the refining and degassing temperature is 730-750°C and the time is 10-20 minutes.
[0022] As a further improvement, in step S1, the aluminum alloy raw material is smelted in a smelting furnace, and when the oxygen content in the smelting furnace is less than 200 ppm, heating is started until the alloy is melted; when the furnace temperature reaches 730-750°C, degassing and refining are carried out, and argon gas is introduced during the refining process.
[0023] Beneficial effects of the present invention:
[0024] 1. The present invention optimizes and improves the aluminum alloy production process, so the process is stable and no refiner needs to be added.
[0025] 2. Through a series of treatments such as solution treatment, aging treatment, primary super freezing treatment, primary heat treatment, secondary super freezing treatment, secondary heat treatment, cooling to room temperature, etc., the casting is finally densified and the fatigue resistance is significantly improved. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0027] Example 1
[0028] Step S1, the aluminum alloy raw material (3 series aluminum alloy, grade 3003) is melted in a melting furnace, and when the oxygen content in the melting furnace is less than 200ppm, heating is started until the alloy is melted; when the furnace temperature reaches 730-740°C, degassing and refining are carried out, and argon gas is introduced during the refining process. The refining and degassing temperature is 730-740°C and the time is 15min; during the refining process, vacuum degassing is used for refining and degassing; and then slag removal, standing, degassing, and water-cooling casting are performed in sequence to obtain an aluminum alloy ingot.
[0029] Step S2, subjecting the aluminum alloy ingot to solution treatment, aging treatment, primary super freezing treatment, primary heat treatment, secondary super freezing treatment, secondary heat treatment, cooling to room temperature, and obtaining an aluminum alloy blank; wherein the temperature of the solution treatment is 520-530°C, and the solution treatment time is 60 minutes. The temperature of the aging treatment is 180°C, and the time is 2 hours. The process of the primary super freezing treatment is as follows:
[0030] The aluminum alloy ingot is first cold pressed by a hydraulic press with an initial cold pressure of 11.5 bar, and then poured into liquid nitrogen for cooling, and the cooling temperature is controlled at -60°C to -65°C; when the cooling temperature is between -70°C and -80°C, the cold pressure changes periodically, and the cooling time is 30 minutes. Within one cycle, the cold pressure is first increased to 15 bar at a rate of 0.5 bar / min, and then decreased to 12 bar at a rate of 1 bar / min; the pressure head of the hydraulic press is in direct contact with the aluminum alloy ingot and completely covers the aluminum alloy ingot, and the pressure head temperature of the hydraulic press is always maintained at 20 to 25°C; wherein, one cycle is 10 minutes.
[0031] The first heat treatment was performed by hot pressing with a hydraulic press, the initial heat pressure was 1.2 bar, the heat treatment temperature was 130°C, and the heat treatment time was 3 h.
[0032] The process of the secondary super freezing treatment is as follows:
[0033] The aluminum alloy ingot was cold pressed by a hydraulic press, and the cold pressure was always 13 bar. Then liquid nitrogen was poured into it for cooling. The cooling temperature was controlled at -90°C to -100°C, and the cooling time was 30 minutes.
[0034] The process of the secondary heat treatment is as follows:
[0035] The aluminum alloy ingot is placed on a centrifugal turntable for centrifugation at a speed of 800 r / min, and then hot air at 150-160° C. is introduced for heating and insulation for 1 hour.
[0036] Step S3: extruding the aluminum alloy blank to obtain an aluminum alloy cast rod.
[0037] In this embodiment, the probability of cracking and peeling on the outer wall of the aluminum alloy billet is 0 (statistics are taken on 100 batches of aluminum alloy billets); the aluminum alloy cast rod finally obtained by the present invention, after precision machining by a precision machining center, has a surface roughness of less than Ra100nm, has excellent optical reflection effect, and also indicates that the grains on the surface and inside of the aluminum alloy cast rod are small and uniform.
[0038] Example 2
[0039] Step S1, the aluminum alloy raw material (3 series aluminum alloy, grade 3003) is melted in a melting furnace, and when the oxygen content in the melting furnace is less than 200ppm, heating is started until the alloy is melted; when the furnace temperature reaches 740-750°C, degassing and refining are carried out, and argon gas is introduced during the refining process. The refining and degassing temperature is 740-750°C and the time is 15min; during the refining process, vacuum degassing is used for refining and degassing; and then slag removal, standing, degassing, and water-cooling casting are performed in sequence to obtain an aluminum alloy ingot.
[0040] Step S2, subjecting the aluminum alloy ingot to solution treatment, aging treatment, primary super freezing treatment, primary heat treatment, secondary super freezing treatment, secondary heat treatment, and cooling to room temperature to obtain an aluminum alloy blank; wherein the temperature of the solution treatment is 530°C and the time of the solution treatment is 40 minutes. The temperature of the aging treatment is 190°C and the time is 1.5 hours. The process of the primary super freezing treatment is as follows:
[0041] The aluminum alloy ingot is first cold pressed by a hydraulic press with an initial cold pressure of 11.5 bar, and then poured into liquid nitrogen for cooling, and the cooling temperature is controlled at -60°C to -65°C; when the cooling temperature is between -70°C and -80°C, the cold pressure changes periodically, and the cooling time is 30 minutes. Within one cycle, the cold pressure is first increased to 15 bar at a rate of 0.5 bar / min, and then decreased to 12 bar at a rate of 1 bar / min; the pressure head of the hydraulic press is in direct contact with the aluminum alloy ingot and completely covers the aluminum alloy ingot, and the pressure head temperature of the hydraulic press is always maintained at 20 to 25°C; wherein, one cycle is 10 minutes.
[0042] The first heat treatment was performed by hot pressing with a hydraulic press, the initial heat pressure was 1.2 bar, the heat treatment temperature was 130°C, and the heat treatment time was 3 h.
[0043] The process of the secondary super freezing treatment is as follows:
[0044] The aluminum alloy ingot was cold pressed by a hydraulic press, and the cold pressure was always 13 bar. Then liquid nitrogen was poured into it for cooling. The cooling temperature was controlled at -90°C to -100°C, and the cooling time was 30 minutes.
[0045] The process of the secondary heat treatment is as follows:
[0046] The aluminum alloy ingot is placed on a centrifugal turntable for centrifugation at a speed of 800 r / min, and then hot air at 150-160° C. is introduced for heating and insulation for 1 hour.
[0047] Step S3: extruding the aluminum alloy blank to obtain an aluminum alloy cast rod.
[0048] In this embodiment, the probability of cracking and peeling of the outer wall of the aluminum alloy blank is 0; the aluminum alloy cast rod finally obtained by the present invention, after precision machining by a precision machining center, can have a surface roughness of less than Ra100nm, with excellent optical reflection effect, which also shows that the grains on the surface and inside of the aluminum alloy cast rod are small and uniform. The room temperature axial loading fatigue test method is in accordance with HB5287 "Axial loading fatigue test method for metal materials", and the result is K Ic =92MPam 1 / 2 .
[0049] Example 3
[0050] Step S1, the aluminum alloy raw material (3 series aluminum alloy, grade 3003) is melted in a melting furnace, and when the oxygen content in the melting furnace is less than 200ppm, heating is started until the alloy is melted; when the furnace temperature reaches 735-745°C, degassing and refining are carried out, and argon gas is introduced during the refining process. The refining and degassing temperature is 7350-745°C, and the time is 15min; during the refining process, vacuum degassing is used for refining and degassing; and then slag removal, standing, degassing, and water-cooling casting are performed in sequence to obtain an aluminum alloy ingot.
[0051] Step S2, subjecting the aluminum alloy ingot to solution treatment, aging treatment, primary super freezing treatment, primary heat treatment, secondary super freezing treatment, secondary heat treatment, and cooling to room temperature to obtain an aluminum alloy blank; wherein the temperature of the solution treatment is 550°C and the time of the solution treatment is 60 minutes. The temperature of the aging treatment is 190°C and the time is 2 hours. The process of the primary super freezing treatment is as follows:
[0052] The aluminum alloy ingot is first cold pressed by a hydraulic press with an initial cold pressure of 11.5 bar, and then poured into liquid nitrogen for cooling, and the cooling temperature is controlled at -60°C to -65°C; when the cooling temperature is between -70°C and -80°C, the cold pressure changes periodically, and the cooling time is 30 minutes. Within one cycle, the cold pressure is first increased to 15 bar at a rate of 0.5 bar / min, and then decreased to 12 bar at a rate of 1 bar / min; the pressure head of the hydraulic press is in direct contact with the aluminum alloy ingot and completely covers the aluminum alloy ingot, and the pressure head temperature of the hydraulic press is always maintained at 20 to 25°C; wherein, one cycle is 10 minutes.
[0053] The first heat treatment was performed by hot pressing with a hydraulic press, the initial heat pressure was 1.2 bar, the heat treatment temperature was 130°C, and the heat treatment time was 3 h.
[0054] The process of the secondary super freezing treatment is as follows:
[0055] The aluminum alloy ingot was cold pressed by a hydraulic press, and the cold pressure was always 13 bar. Then liquid nitrogen was poured into it for cooling. The cooling temperature was controlled at -90°C to -100°C, and the cooling time was 30 minutes.
[0056] The process of the secondary heat treatment is as follows:
[0057] The aluminum alloy ingot is placed on a centrifugal turntable for centrifugation at a speed of 800 r / min, and then hot air at 150-160° C. is introduced for heating and insulation for 1 hour.
[0058] Step S3: extruding the aluminum alloy blank to obtain an aluminum alloy cast rod.
[0059] In this embodiment, the probability of cracking and peeling of the outer wall of the aluminum alloy blank is zero.
[0060] The aluminum alloy cast rod finally obtained by the present invention can have a surface roughness of less than Ra100nm after precision machining by a precision machining center, and has excellent optical reflection effect, which also shows that the grains on the surface and inside of the aluminum alloy cast rod are fine and uniform.
[0061] Comparative Example 1
[0062] The difference between this example and Example 1 is that the four steps of the primary super freezing treatment, the primary heat treatment, the secondary super freezing treatment, and the secondary heat treatment in step S2 are different, and the rest are the same; in the primary super freezing treatment process of this example, a hydraulic press is not used for cold pressing, the cooling temperature is between -60°C and -100°C, and the cooling time is 30 minutes; the primary heat treatment does not use a hydraulic press for hot pressing, the heat treatment temperature is 130°C, and the heat treatment time is 3 hours; the secondary super freezing treatment does not use a hydraulic press for cold pressing, the cooling temperature is between -90°C and -100°C, and the cooling time is 30 minutes; the secondary heat treatment does not use a centrifugal turntable for centrifugation, and is kept warm for 1 hour in a hot air environment of 150 to 160°C.
[0063] Finally, it was found that the probability of cracking and peeling on the outer wall of the aluminum alloy blank was more than 73%. The outer wall of the aluminum alloy blank needed to be cut before the subsequent process could be carried out. Moreover, the cracking and peeling showed that the alternating treatment of extreme cold and high temperature could make the inside of the aluminum alloy blank, especially the inner core, denser. However, the closer to the outer wall, the tightness of the outer periphery of the aluminum alloy blank decreased due to the excessive stress change, and finally cracking and peeling occurred. Therefore, this part needed to be removed. After flaw detection, it was found that the cutting depth was at least 11cm, and the processing volume was large. The outer wall of the aluminum alloy blank was cut to a processing thickness of 11cm, and then it was precisely processed by a precision machining center, and the surface roughness could reach below Ra100nm.
[0064] Comparative Example 2
[0065] The difference between this example and Example 1 is that in the first-stage super freezing treatment in step S2, when the cooling temperature is between -70°C and -80°C, the cold pressure is kept constant at 13.5 bar, and the rest remain unchanged; the probability of cracking and warping on the outer wall of the aluminum alloy billet finally obtained is 39%±1%.
[0066] Comparative Example 3
[0067] The difference between this example and Example 1 is that in the first-level super freezing treatment in step S2, the pressure head of the hydraulic press is also submerged in liquid nitrogen for cooling, and the rest remains unchanged; the probability of cracking and peeling on the outer wall is 0%, but the outer wall of the aluminum alloy billet needs to be cut and processed, and after the processing thickness reaches at least 5.7cm, it is precisely processed by a precision machining center, and the surface roughness can reach below Ra100nm.
[0068] Comparative Example 4
[0069] The difference between this example and Example 1 is that in the secondary heat treatment in step S2, the aluminum alloy ingot is not subjected to centrifugal treatment, but the same process as the primary heat treatment is adopted, and the rest remains unchanged; the probability of cracking on the outer wall of the aluminum alloy billet finally obtained is 22%±1%, and there is no peeling phenomenon.
[0070] In the above embodiments, the present invention optimizes and improves the 3 series aluminum alloys with poor toughness and fatigue resistance, and adopts the alternating treatment of extreme cold of nearly 100°C below zero and overheating of more than 100°C. The stress changes generated inside the aluminum alloy castings will cause microscopic deformation of the castings, and the stress changes are drastic. By using the drastic stress changes, under the constraint of external heavy pressure, most of the microscopic defects are compacted to achieve the densification effect of the castings, effectively improve the nucleation position of the precipitation phase, and the crystallization and strengthening effect of the precipitation phase are better, further improving the fatigue resistance; in addition, in the case of extreme cold liquid nitrogen, the upper end of the ingot is in contact with the pressure head of the hydraulic press and maintained at room temperature. The stress generated by this huge temperature difference can further compact the microscopic defects of the ingots to achieve the densification effect of the castings. The aluminum alloy cast rod obtained by the present invention can meet the high fatigue resistance requirements in the fields of aviation, high-speed rail, new energy, etc., and has high application value.
[0071] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod, characterized in that The following steps are involved: Step S1, melting, alloying, refining, slagging, standing, degassing, and water-cooling casting the aluminum alloy raw materials to obtain an aluminum alloy ingot; Step S2, subjecting the aluminum alloy ingot to solution treatment, aging treatment, primary super freezing treatment, primary heat treatment, secondary super freezing treatment, secondary heat treatment, and cooling to room temperature to obtain an aluminum alloy blank; Step S3: extruding the aluminum alloy blank to obtain an aluminum alloy cast rod.
2. The method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod according to claim 1, characterized in that: In step S2, the process of the first-level super freezing treatment is as follows: The aluminum alloy ingot is first cold pressed by a hydraulic press with an initial cold pressure of 11.5 bar, and then poured into liquid nitrogen for cooling, and the cooling temperature is controlled at -60°C to -65°C; when the cooling temperature is between -70°C and -80°C, the cold pressure changes periodically, and the cooling time is 30 to 50 minutes. Within one cycle, the cold pressure is first increased to 15 bar at a rate of 0.5 bar / min, and then decreased to 12 bar at a rate of 1 bar / min; the pressure head of the hydraulic press is in direct contact with the aluminum alloy ingot and completely covers the aluminum alloy ingot, and the pressure head temperature of the hydraulic press is always maintained at 20 to 25°C.
3. The method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod according to claim 1, characterized in that: In step S2, a heat treatment is performed using a hydraulic press, with an initial heat pressure of 1.2 bar, a heat treatment temperature of 130° C., and a heat treatment time of 3 h.
4. The method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod according to claim 1, characterized in that: In step S2, the process of the secondary super freezing treatment is as follows: The aluminum alloy ingot was cold pressed by a hydraulic press, and the cold pressure was always 13 bar. Then liquid nitrogen was poured into it for cooling. The cooling temperature was controlled at -90°C to -100°C, and the cooling time was 30 minutes.
5. The method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod according to claim 1, characterized in that: In step S2, the process of the secondary heat treatment is as follows: The aluminum alloy ingot is placed on a centrifugal turntable for centrifugation at a speed of 800 r / min, and then hot air at 150-160° C. is introduced for heating and insulation for 1 hour.
6. The method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod according to claim 1, characterized in that: In step S1, during the refining process, vacuum degassing is used to perform refining and degassing.
7. The method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod according to claim 1, characterized in that: In step S2, the temperature of the solution treatment is 520-560°C, and the time of the solution treatment is 30-60 minutes.
8. The method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod according to claim 1, characterized in that: In step S2, the aging treatment is performed at a temperature of 180 to 200°C for 1 to 2 hours.
9. The method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod according to claim 6, characterized in that: In step S1, the refining and degassing temperature is 730-750°C and the time is 10-20 minutes.
10. The method for producing a high-efficiency fatigue-resistant aluminum alloy cast rod according to claim 1, characterized in that: In step S1, the aluminum alloy raw material is melted in a melting furnace, and when the oxygen content in the melting furnace is less than 200 ppm, heating is started until the alloy is melted; when the furnace temperature reaches 730-750°C, degassing and refining are carried out, and argon gas is introduced during the refining process.
Citation Information
Cited By
Method for preparing aluminum alloy component through additive-deep cold forging coupling forming technology
CN120921015A