Copper alloy surface Ti-Al-C-based conductive wear-resistant composite coating and preparation method thereof

By using Ti, Al and graphite powder to prepare Ti-Al-C spherical powder and using atmospheric plasma spraying technology, the problems of high cost and deterioration of Ti2AlC phase coating materials are solved, and the conductive wear-resistant composite coating on the surface of copper alloy is realized. Low cost preparation and performance improvement.

CN118979217AActive Publication Date: 2024-11-19ANHUI UNIVERSITY OF TECHNOLOGY

Patent Information

Application Number
CN202411090876.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The preparation of Ti2AlC phase coating materials is costly and prone to high temperature decomposition, resulting in deterioration of performance, limiting its promotion on copper alloy surfaces.

Method used

Ti-Al-C spherical powder is prepared by granulation by Ti, Al and graphite powder, and Ti-Al-C/Cu composite coating is prepared by atmospheric plasma spraying technology, and combined with process regulation to form enhanced phase TiC, TiAl and conductive phase Ti2AlC. , reduce costs and improve wear resistance and conductivity.

Benefits of technology

The conductive and wear-resistant composite coating on the surface of copper alloy is achieved at a low cost, which improves the anti-current wear performance of copper alloy, and has a simple process and a low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979217A_ABST
    Figure CN118979217A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of copper alloy surface wear protection, in particular to a copper alloy surface Ti-Al-C-based conductive wear-resistant composite coating and a preparation method thereof.The preparation method comprises the steps that firstly, raw materials including Ti powder, Al powder and graphite powder are selected, Ti-Al-C powder is prepared in a spray granulation mode, and the powder bonding strength is improved through vacuum sintering; the preparation method comprises the following steps: sintering Ti-Al-C powder and Cu powder, removing a polyvinyl alcohol binder used during granulation, mixing the sintered Ti-Al-C powder and Cu powder through an automatic stirrer to prepare composite coating powder, preparing a coating by using atmospheric plasma spraying equipment, preparing a Ti-Al-C / Cu composite coating with the thickness of 200-300 microns on the surface of a Cu matrix, and carrying out surface sand blasting coarsening and alcohol ultrasonic cleaning on the Cu matrix before spraying. The phase of the coating prepared under the condition comprises a reinforced phase TiC phase and a TiAl phase formed by reaction, a lubricating conductive phase Ti2AlC phase formed by reaction, and unreacted conductive phases such as Ti and Cu, so that low-cost preparation of the conductive wear-resistant composite coating is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper alloy surface wear protection, and in particular to a Ti-Al-C based conductive wear-resistant composite coating on the copper alloy surface and a preparation method thereof. Background Art

[0002] Copper alloys are widely used in brushes, pantograph slides, integrated circuit lead frames, and electromagnetic gun rails due to their excellent electrical conductivity, ductility, and machinability. However, their lack of hardness and wear resistance limits their promotion and application. Surface coating technology is often used to overcome the problems of insufficient hardness and poor wear resistance of copper alloys. 2 As a typical representative of MAX phase, AlC has high hardness, high wear resistance and good oxidation resistance of ceramics, as well as excellent thermal and electrical conductivity and good plasticity of metals, and is considered to be an ideal conductive and wear-resistant coating material. 2 The cost of AlC powder is high, and direct spraying is prone to Ti 2 The high temperature decomposition of AlC phase material leads to Ti 2 The performance of the AlC phase coating material is deteriorated, so direct spraying of Ti 2 AlC phase coating is not economical from an industrial perspective and has limited success.

[0003] In view of the above-mentioned defects, the inventors of the present invention finally obtained the present invention after a long period of research and practice. Summary of the invention

[0004] The purpose of the present invention is to solve the current problem of preparing Ti 2 The cost of AlC powder is high, and direct spraying is prone to Ti 2 The high temperature decomposition of AlC phase material leads to Ti 2 To solve the problem of performance degradation of AlC phase coating materials, a Ti-Al-C based conductive wear-resistant composite coating on the surface of a copper alloy and a preparation method thereof are provided.

[0005] In order to achieve the above object, the present invention discloses a method for preparing a Ti-Al-C based conductive wear-resistant composite coating on a copper alloy surface, comprising the following steps:

[0006] S1, adding Ti powder, Al powder, graphite powder, polyvinyl alcohol and sodium carboxymethyl cellulose into deionized water and stirring to prepare Ti-Al-C powder granulation slurry;

[0007] S2, preparing Ti-Al-C spherical powder from the Ti-Al-C powder granulation slurry obtained in step S1 by spray granulation, and vacuum sintering the slurry to obtain Ti-Al-C powder;

[0008] S3, mechanically mixing the Ti-Al-C powder obtained in step S2 with Cu powder to obtain a Ti-Al-C / Cu composite powder;

[0009] S4, sandblasting roughening and alcohol ultrasonic cleaning of the sprayed surface of the Cu substrate;

[0010] S5, using the Ti-Al-C / Cu composite powder in step S3 to perform atmospheric plasma spraying to obtain a Ti-Al-C / Cu composite thick coating of 200 to 300 μm.

[0011] In the step S1, the molar ratio of Ti powder, Al powder and graphite powder is 2:1:1, the particle size of Ti powder is 5-30 μm, the particle size of Al powder is 3-15 μm, and the particle size of graphite powder is 1-5 μm.

[0012] In the step S1, the mass of deionized water is 1.5 times the mass of the powder, the mass of polyvinyl alcohol is 2.5% of the mass of the powder, and the mass of sodium carboxymethyl cellulose is 0.5% of the mass of the powder.

[0013] In step S2, the vacuum degree during sintering is 1×10 -2 Pa, the heating process is as follows: heat from room temperature to 300°C at 10°C / min, then heat to 610-650°C at 5°C / min, keep warm for 2 hours, and cool with the furnace after the end of the heat preservation.

[0014] In the step S3, the Ti-Al-C composite powder accounts for 40-60% of the total molar ratio, and the Cu powder is a spherical powder of 30-60 μm.

[0015] In step S5, the spraying parameters are as follows: current is 450-500A, power is 30-32kW, main gas flow rate of argon is 30-45L / min, line speed is 450-550mm / s, and spraying distance is 90-110mm.

[0016] The invention also discloses a Ti-Al-C based conductive wear-resistant composite coating on the surface of the copper alloy prepared by the preparation method.

[0017] Compared with the prior art, the invention has the following beneficial effects: the invention selects low-cost Ti, Al and graphite powder, prepares Ti-Al-C spherical powder by granulation, and adopts atmospheric plasma spraying to prepare Ti-Al-C / Cu composite coating, the preparation method is simple, the preparation cost is low, and the reinforcing phase TiC phase and TiAl phase, the lubricating conductive phase TiC phase and ... 2The AlC phase, and unreacted conductive Ti, Cu and other phases are well combined with the matrix, have good wear resistance and conductivity, and realize the low-cost preparation of conductive wear-resistant composite coatings. It can be used as a conductive wear-resistant material on the surface of copper alloy materials to improve the copper alloy's resistance to current-carrying wear. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The powder morphology of the embodiment of the present invention and the comparative example 2;

[0019] Figure 2 This is a cross-sectional morphology diagram of the coating according to an embodiment of the present invention;

[0020] Figure 3 The hardness test results of the embodiment of the present invention and comparative example 3 are shown;

[0021] Figure 4 The conductivity test results of the embodiment of the present invention and comparative example 4 are shown;

[0022] Figure 5 The porosity test results of the embodiment of the present invention and comparative example 5 are shown;

[0023] Figure 6 The hardness test results of the embodiment of the present invention and comparative example 6 are shown;

[0024] Figure 7 The wear marks of current-carrying friction and wear of the embodiment of the present invention and comparative example 1. DETAILED DESCRIPTION

[0025] The above and other technical features and advantages of the present invention are described in more detail below in conjunction with the accompanying drawings.

[0026] Example 1

[0027] S1: Ti powder, Al powder, graphite powder, polyvinyl alcohol, and sodium carboxymethyl cellulose are added to deionized water and stirred to prepare Ti-Al-C powder granulation slurry. The molar ratio of Ti:Al:C is 2:1:1, and the particle size of Ti powder is 5-30 μm, the particle size of Al powder is 3-15 μm, and the particle size of graphite powder is 1-5 μm.

[0028] S2: Prepare Ti-Al-C spherical powder from the Ti-Al-C powder granulation slurry obtained in step S1 by spray granulation, and vacuum sinter the slurry to obtain Ti-Al-C powder. The vacuum degree during sintering is maintained at 1×10 -2 Pa, the heating process is from room temperature to 300°C at 10°C / min, and then to 630°C at 5°C / min, and kept warm for 2 hours. After the end of the heat preservation, the furnace is cooled.

[0029] S3: Mechanically mix the Ti-Al-C powder obtained in S2 with Cu powder, wherein the Ti-Al-C composite powder accounts for 50% of the total molar ratio and the Cu powder is a 30-60 μm spherical powder, thereby obtaining a Ti-Al-C / Cu composite powder.

[0030] S4: The sprayed surface of the Cu substrate is roughened by sandblasting and cleaned by alcohol ultrasonic cleaning.

[0031] S5: Atmospheric plasma spraying was performed with a current of 460A, a power of 30kw, a main gas flow rate of argon gas of 45L / min, a linear speed of 500mm / s, and a spraying distance of 100mm to obtain a Ti-Al-C / Cu composite coating.

[0032] Comparative Example 1

[0033] Untreated copper alloy.

[0034] The wear marks of current-carrying friction and wear of the embodiment and comparative example 1 are as follows Figure 7 As shown, the comparative example 1 has a more serious wear condition than the example, which indicates that the anti-current-carrying friction and wear performance of the example is much better than that of the comparative example.

[0035] Comparative Example 2

[0036] S1: Ti powder, Al powder, graphite powder, polyvinyl alcohol, and sodium carboxymethyl cellulose are added to deionized water and stirred to prepare Ti-Al-C powder granulation slurry. The molar ratio of Ti:Al:C is 2:1:1, and the particle size of Ti powder is 5-30 μm, the particle size of Al powder is 3-15 μm, and the particle size of graphite powder is 1-5 μm.

[0037] S2: The Ti—Al—C powder granulation slurry obtained in step S1 is prepared into Ti—Al—C spherical powder by spray granulation.

[0038] S3: Mechanically mix the Ti-Al-C powder obtained in S2 with Cu powder, wherein the Ti-Al-C composite powder accounts for 50% of the total molar ratio and the Cu powder is a 30-60 μm spherical powder, thereby obtaining a Ti-Al-C / Cu composite powder.

[0039] S4: The sprayed surface of the Cu substrate is roughened by sandblasting and cleaned by alcohol ultrasonic cleaning.

[0040] S5: Atmospheric plasma spraying was performed with a current of 460A, a power of 30kw, a main gas flow rate of argon gas of 45L / min, a linear speed of 500mm / s, and a spraying distance of 100mm to obtain a Ti-Al-C / Cu composite coating.

[0041] The powder of Comparative Example 2 was not sintered, and its powder morphology was compared with the powder after sintering in Example 2. Figure 1As shown, the unsintered powder is brittle, resulting in a low proportion of spherical powder and poor fluidity, which leads to low spraying efficiency and poor coating performance.

[0042] Comparative Example 3

[0043] S1: Ti powder, Al powder, graphite powder, polyvinyl alcohol, and sodium carboxymethyl cellulose are added to deionized water and stirred to prepare Ti-Al-C powder granulation slurry. The molar ratio of Ti:Al:C is 2:1:1, and the particle size of Ti powder is 5-30 μm, the particle size of Al powder is 3-15 μm, and the particle size of graphite powder is 1-5 μm.

[0044] S2: Prepare Ti-Al-C spherical powder from the Ti-Al-C powder granulation slurry obtained in step S1 by spray granulation, and vacuum sinter the slurry to obtain Ti-Al-C powder. The vacuum degree during sintering is maintained at 1×10 -2 Pa, the heating process is from room temperature to 300°C at 10°C / min, and then to 630°C at 5°C / min, and kept warm for 2 hours. After the end of the heat preservation, the furnace is cooled.

[0045] S3: Mechanically mix the Ti-Al-C powder obtained in S2 with Cu powder, wherein the Ti-Al-C composite powder accounts for 20% of the total molar ratio, and the Cu powder is a 30-60 μm spherical powder, to obtain a Ti-Al-C / Cu composite powder.

[0046] S4: The sprayed surface of the Cu substrate is roughened by sandblasting and cleaned by alcohol ultrasonic cleaning.

[0047] S5: Atmospheric plasma spraying was performed with a current of 460A, a power of 30kw, a main gas flow rate of argon gas of 45L / min, a linear speed of 500mm / s, and a spraying distance of 100mm to obtain a Ti-Al-C / Cu composite coating.

[0048] The hardness test results of Example 3 and Comparative Example 3 are as follows Figure 3 As shown in the figure, when the Ti-Al-C powder content is insufficient, the hardness of the coating decreases significantly and the wear resistance of the coating is poor.

[0049] Comparative Example 4

[0050] S1: Ti powder, Al powder, graphite powder, polyvinyl alcohol, and sodium carboxymethyl cellulose are added to deionized water and stirred to prepare Ti-Al-C powder granulation slurry. The molar ratio of Ti:Al:C is 2:1:1, and the particle size of Ti powder is 5-30 μm, the particle size of Al powder is 3-15 μm, and the particle size of graphite powder is 1-5 μm.

[0051] S2: Prepare Ti-Al-C spherical powder from the Ti-Al-C powder granulation slurry obtained in step S1 by spray granulation, and vacuum sinter the slurry to obtain Ti-Al-C powder. The vacuum degree during sintering is maintained at 1×10 -2 Pa, the heating process is from room temperature to 300°C at 10°C / min, and then to 630°C at 5°C / min, and kept warm for 2 hours. After the end of the heat preservation, the furnace is cooled.

[0052] S3: Mechanically mix the Ti-Al-C powder obtained in S2 with Cu powder, wherein the Ti-Al-C composite powder accounts for 80% of the total molar ratio and the Cu powder is a 30-60 μm spherical powder, thereby obtaining a Ti-Al-C / Cu composite powder.

[0053] S4: The sprayed surface of the Cu substrate is roughened by sandblasting and cleaned by alcohol ultrasonic cleaning.

[0054] S5: Atmospheric plasma spraying was performed with a current of 460A, a power of 30kw, a main gas flow rate of argon gas of 45L / min, a linear speed of 500mm / s, and a spraying distance of 100mm to obtain a Ti-Al-C / Cu composite coating.

[0055] The conductivity test results of Example 4 and Comparative Example 4 are as follows Figure 4 As shown, when the Ti-Al-C powder content is too high, the ceramic phase by-product content is high, resulting in a decrease in the electrical conductivity of the coating, affecting the coating's conductive properties and resistance to current-carrying friction and wear.

[0056] Comparative Example 5

[0057] S1: Ti powder, Al powder, graphite powder, polyvinyl alcohol, and sodium carboxymethyl cellulose are added to deionized water and stirred to prepare Ti-Al-C powder granulation slurry. The molar ratio of Ti:Al:C is 2:1:1, and the particle size of Ti powder is 5-30 μm, the particle size of Al powder is 3-15 μm, and the particle size of graphite powder is 1-5 μm.

[0058] S2: Prepare Ti-Al-C spherical powder from the Ti-Al-C powder granulation slurry obtained in step S1 by spray granulation, and vacuum sinter the slurry to obtain Ti-Al-C powder. The vacuum degree during sintering is maintained at 1×10 -2 Pa, the heating process is from room temperature to 300°C at 10°C / min, and then to 630°C at 5°C / min, and kept warm for 2 hours. After the end of the heat preservation, the furnace is cooled.

[0059] S3: Mechanically mix the Ti-Al-C powder obtained in S2 with Cu powder, wherein the Ti-Al-C composite powder accounts for 50% of the total molar ratio and the Cu powder is a 30-60 μm spherical powder, thereby obtaining a Ti-Al-C / Cu composite powder.

[0060] S4: The sprayed surface of the Cu substrate is roughened by sandblasting and cleaned by alcohol ultrasonic cleaning.

[0061] S5: Atmospheric plasma spraying was performed with a current of 460A, a power of 25kw, a main gas flow rate of argon gas of 45L / min, a line speed of 500mm / s, and a spraying distance of 100mm to obtain a Ti-Al-C / Cu composite coating.

[0062] The porosity test results of Example 5 and Comparative Example 5 are as follows Figure 5 As shown, when the spraying power is low, the powder melting is poor and the coating porosity is high, which affects the coating's electrical conductivity and resistance to current-carrying friction and wear.

[0063] Comparative Example 6

[0064] S1: Ti powder, Al powder, graphite powder, polyvinyl alcohol, and sodium carboxymethyl cellulose are added to deionized water and stirred to prepare Ti-Al-C powder granulation slurry. The molar ratio of Ti:Al:C is 2:1:1, and the particle size of Ti powder is 5-30 μm, the particle size of Al powder is 3-15 μm, and the particle size of graphite powder is 1-5 μm.

[0065] S2: Prepare Ti-Al-C spherical powder from the Ti-Al-C powder granulation slurry obtained in step S1 by spray granulation, and vacuum sinter the slurry to obtain Ti-Al-C powder. The vacuum degree during sintering is maintained at 1×10 -2 Pa, the heating process is from room temperature to 300°C at 10°C / min, and then to 630°C at 5°C / min, and kept warm for 2 hours. After the end of the heat preservation, the furnace is cooled.

[0066] S3: Mechanically mix the Ti-Al-C powder obtained in S2 with Cu powder, wherein the Ti-Al-C composite powder accounts for 50% of the total molar ratio and the Cu powder is a 30-60 μm spherical powder, thereby obtaining a Ti-Al-C / Cu composite powder.

[0067] S4: The sprayed surface of the Cu substrate is roughened by sandblasting and cleaned by alcohol ultrasonic cleaning.

[0068] S5: Atmospheric plasma spraying was performed with a current of 460A, a power of 35kw, a main gas flow rate of argon gas of 45L / min, a line speed of 500mm / s, and a spraying distance of 100mm to obtain a Ti-Al-C / Cu composite coating.

[0069] The hardness test results of Example 6 and Comparative Example 6 are as follows Figure 6 As shown, when the spraying power is high, more oxides are produced in the coating, which affects the hardness of the coating and causes the coating's resistance to current-carrying friction and wear to decrease.

[0070] The above description is only a preferred embodiment of the present invention, which is only illustrative and not restrictive of the present invention. Those skilled in the art understand that many changes, modifications, and even equivalences may be made to the present invention within the spirit and scope defined by the claims of the present invention, but all of them will fall within the scope of protection of the present invention.

Claims

1. A method for preparing a Ti-Al-C based conductive wear-resistant composite coating on a copper alloy surface, characterized in that: The following steps are involved: S1, adding Ti powder, Al powder, graphite powder, polyvinyl alcohol and sodium carboxymethyl cellulose into deionized water and stirring to prepare Ti-Al-C powder granulation slurry; S2, preparing Ti-Al-C spherical powder from the Ti-Al-C powder granulation slurry obtained in step S1 by spray granulation, and vacuum sintering the slurry to obtain Ti-Al-C powder; S3, mechanically mixing the Ti-Al-C powder obtained in step S2 with Cu powder to obtain a Ti-Al-C / Cu composite powder; S4, sandblasting roughening and alcohol ultrasonic cleaning of the sprayed surface of the Cu substrate; S5, using the Ti-Al-C / Cu composite powder in step S3 to perform atmospheric plasma spraying to obtain a Ti-Al-C / Cu composite thick coating of 200 to 300 μm.

2. The method for preparing a Ti-Al-C based conductive wear-resistant composite coating on a copper alloy surface as claimed in claim 1, characterized in that: In the step S1, the molar ratio of Ti powder, Al powder and graphite powder is 2:1:1, the particle size of Ti powder is 5-30 μm, the particle size of Al powder is 3-15 μm, and the particle size of graphite powder is 1-5 μm.

3. The method for preparing a Ti-Al-C based conductive wear-resistant composite coating on a copper alloy surface as claimed in claim 1, characterized in that: In the step S1, the mass of deionized water is 1.5 times the mass of the powder, the mass of polyvinyl alcohol is 2.5% of the mass of the powder, and the mass of sodium carboxymethyl cellulose is 0.5% of the mass of the powder.

4. The method for preparing a Ti-Al-C based conductive wear-resistant composite coating on a copper alloy surface as claimed in claim 1, characterized in that: In step S2, the vacuum degree during sintering is 1×10 -2 Pa, the heating process is as follows: heat from room temperature to 300°C at 10°C / min, then heat to 610-650°C at 5°C / min, keep warm for 2 hours, and cool with the furnace after the end of the heat preservation.

5. The method for preparing a Ti-Al-C based conductive wear-resistant composite coating on a copper alloy surface as claimed in claim 1, characterized in that: In the step S3, the Ti-Al-C composite powder accounts for 40-60% of the total molar ratio, and the Cu powder is a 30-60 μm spherical powder.

6. The method for preparing a Ti-Al-C based conductive wear-resistant composite coating on a copper alloy surface as claimed in claim 1, characterized in that: In step S5, the spraying parameters are as follows: current is 450-500A, power is 30-32kW, main gas flow rate of argon is 30-45L / min, line speed is 450-550mm / s, and spraying distance is 90-110mm.

7. A Ti-Al-C based conductive wear-resistant composite coating on the surface of a copper alloy prepared by the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Method for synthesizing spherical MAX-phase powder material with main phase being Ti2AlC

    CN106032324A

  • Method for preparing Ti-Al-C-based composite coating through plasma spraying

    CN115491629A

  • High-performance composite coating as well as preparation method and application thereof

    CN116180070A

Cited By

  • Ti-Al-C phase reinforced NiCrAlY composite coating as well as preparation method and application of Ti-Al-C phase reinforced NiCrAlY composite coating

    CN119506763A