Preparation method of CrSi resistive film
Through near-infrared femtosecond laser-induced back surface removal and femtosecond laser plasma channel annealing technology, combined with magnetron sputtering and PI passivation layer, the edge roughness and stability of chromium silicon-based resistive films are solved, achieving high accuracy and low The cost preparation improves the performance and production efficiency of the resistive film.
Patent Information
- Application Number
- CN202411077397.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The existing preparation process of chromium silicon-based resistive films has problems such as high edge roughness, poor accuracy and stability, and is complex, expensive, low efficiency, and easy to introduce impurities and pollution, affecting the performance of the resistor.
Near infrared femtosecond laser induced the removal of chromium silicon nickel-molybdenum metal film on the back, and heat treatment was carried out through femtosecond laser plasma channel annealing technology, combining magnetron sputtering and the use of PI passivation layer to simplify the process flow and avoid the large amount of chemical reagents. use.
The edge roughness, accuracy and stability of the CrSi resistive film are reduced, the annealing time is shortened, the production efficiency is improved, environmental pollution and operation risks are reduced, and the resistivity and temperature coefficient of the resistive film are improved.
Smart Images

Figure CN118979223A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of high-precision resistors, and in particular to a method for preparing a CrSi resistor film. Background Art
[0002] With the rapid development of integrated circuit technology and the design of its components tending towards smaller sizes, higher requirements are placed on the resistors in integrated circuits, and high-precision thin-film resistors are gradually coming into people's view. Compared with diffused resistors and ion-implanted resistors, high-precision thin-film resistors are widely used in aerospace, automotive electronics, navigation systems and other fields based on their own excellent characteristics such as high resistivity, low resistance temperature coefficient, high stability, no parasitic effects and low noise. At present, thin-film materials mainly include chromium-silicon thin films, nickel-chromium thin films and carbon thin films. Among them, chromium-silicon resistor alloys have become the most commonly used resistor materials in chip components, hybrid integrated circuits and monolithic integrated circuits due to their moderate resistance range and wide range of applications.
[0003] The patent application with the publication number CN110233016A discloses a method for preparing a diamond-based thin film chip resistor element, which belongs to the field of electronic component manufacturing. The diamond film is deposited on the original carrier by CVD, and then the grinding, polishing, scribing and etching processes are completed in sequence; then a thin film resistor is constructed on the surface of the patterned CVD diamond film, and the resistance of the thin film resistor is adjusted by a heat treatment process; then the electrode is prepared on the surface of the resistor; finally, the original carrier of the CVD diamond film is removed to obtain a diamond-based thin film resistor element with a size and resistivity that meet the requirements. The element of the present invention is based on diamond as a carrier, and has the characteristics of stable chemical properties and high thermal conductivity. In the intermediate process, a laser scribing assisted plasma etching process is used to solve a series of problems such as the difficulty of subsequent processing of the CVD diamond film and the generation of a conductive carbon film after processing, thereby realizing the mass production of CVD diamond film-based thin film chip resistors at a relatively low cost. While reducing the relative cost, the product quality and production efficiency are guaranteed. However, the grinding, polishing and etching processes disclosed in the patent are easy to introduce new impurities, which pollute the film and cause the stability of the thin film resistor to be poor.
[0004] The patent application with the publication number CN103151276A discloses a method for integrating a high-integration power thin-film hybrid integrated circuit. The method integrates chips and chip components on the horizontal surface of the convex base and the two sides of the convex part of the convex tube base, and makes electrical connections through through holes; first, a layer of nickel-chromium alloy resistance film is formed on the ceramic substrate by sputtering or evaporation; then a layer of metal film is formed in the same way; then, the resistance film and the metal film are photolithographically and selectively etched to obtain the required film pattern; after laser resistance adjustment and scribe separation, a horizontal mounting substrate and a vertical mounting substrate are obtained; then the substrate is mounted on the horizontal surface and the vertical surface of the convex tube base, and finally one or more semiconductor chips or chip components are integrated on the substrate by thin-film hybrid integration, and the lead bonding of the semiconductor chip is completed. The selective etching of the resistance film disclosed in the patent is easy to contaminate the resistance film, resulting in poor accuracy and stability of the resistance film.
[0005] The preparation methods of chromium silicon resistors mainly include photolithography, corrosion, thermal annealing and other processes. However, the corrosion process, photolithography technology and thermal annealing methods have the problems of complex process, high preparation cost, low preparation efficiency, lack of process flexibility, and environmental pollution. In addition, the edge roughness of the prepared resistor film is large, which affects the accuracy and stability of the thin film resistor. Summary of the invention
[0006] The invention provides a method for preparing a CrSi resistor film. The CrSi resistor film prepared by the method has low edge roughness and high precision and stability of the film resistor.
[0007] The present invention provides a method for preparing a CrSi resistor film, comprising:
[0008] S1, plating a chromium-silicon-nickel-molybdenum metal film on a silicon oxide wafer material substrate;
[0009] S2, using near-infrared femtosecond laser to induce the back removal of the Cr-Si-Ni-Mo metal film in the selected area;
[0010] S3, forming an aluminum-copper alloy electrode on the chromium-silicon-nickel-molybdenum metal film;
[0011] S4, heat treating the chromium-silicon-nickel-molybdenum metal film of step S3 by femtosecond laser plasma channel annealing technology;
[0012] S5. Patterning a PI passivation layer on the heat-treated chromium-silicon-nickel-molybdenum metal film.
[0013] Preferably, a chromium-silicon-nickel-molybdenum metal film is deposited on a silicon oxide wafer substrate in an atmosphere of argon and nitrogen by a magnetron sputtering method.
[0014] Further preferably, the mass fractions of chromium, silicon, nickel and molybdenum are 40-43%, 55%, 1-3% and 1-2% respectively, and during the magnetron sputtering process, the flow ratio of argon gas to nitrogen gas is 300-500:1.
[0015] Further preferably, the thickness of the chromium-silicon-nickel-molybdenum metal film is 10-20 nm.
[0016] Preferably, a near-infrared femtosecond laser is used to induce the back removal of the chromium-silicon-nickel-molybdenum metal film in a selected area by a first device, wherein the first device comprises a femtosecond laser amplifier arranged in the direction of light propagation, an electrically controlled optical shutter, a first λ / 2 wave plate, a polarizer, a 4X beam expander, a second λ / 2 wave plate, an optical parametric amplifier, a dichroic mirror, a CCD camera, a 10x microscope objective lens and an xyz three-dimensional electrically controlled displacement platform;
[0017] The femtosecond laser amplifier is used to generate femtosecond laser pulses, the laser pulse wavelength is 800nm, and the pulse width is 30fs;
[0018] The electrically controlled shutter is used to control the passage and cutoff of femtosecond laser pulses;
[0019] The first λ / 2 wave plate and polarizer are used to adjust the energy of the femtosecond laser pulse, and the polarization direction of the obtained light beam is vertical polarization;
[0020] The 4X beam expander is used to expand the beam diameter of the femtosecond laser pulse;
[0021] The second λ / 2 wave plate is used to adjust the polarization direction of the femtosecond laser pulse from vertical polarization to horizontal polarization;
[0022] The optical parametric amplifier is used to obtain a laser beam with a wavelength of 1064nm;
[0023] The dichroic mirror, CCD camera and 10x microscope objective are used to focus the laser beam to the interface between the silicon oxide substrate and the chromium silicon nickel molybdenum metal film in the selected area to remove the chromium silicon nickel molybdenum metal film in the selected area.
[0024] The present invention obtains a set wavelength light beam through an optical parametric amplifier to obtain a near-infrared femtosecond laser that can completely penetrate a silicon oxide wafer substrate, thereby enabling back etching of a chromium-silicon-nickel-molybdenum metal film.
[0025] Preferably, the laser pulse energy induced by the near-infrared femtosecond laser is 0.2-0.5 μJ, the scanning speed is 2-5 mm / s, and the scanning interval is 1-3 um.
[0026] Preferably, a magnetron sputtering method is used to pattern an aluminum-copper alloy electrode on a hard mask, wherein the hard mask is prepared based on a femtosecond laser filament ablation technique, and the thickness of the aluminum-copper alloy is 1.0-1.2 μm.
[0027] Preferably, the chromium-silicon-nickel-molybdenum metal film of step S3 is heat-treated by a second device using a femtosecond laser plasma channel annealing technique, wherein the second device comprises a femtosecond laser amplifier, an electrically controlled optical shutter, a λ / 2 wave plate, a polarization cube beam splitter, a 4X beam expander, a beam shaping system, a scanning galvanometer system, a focusing mirror with a focal length of 20 cm, and a sample stage with a chamber arranged in a light propagation direction;
[0028] The femtosecond laser amplifier is used to generate femtosecond laser pulses, the laser pulse wavelength is 800nm, and the pulse width is 30fs;
[0029] The electrically controlled shutter is used to control the passage and cutoff of femtosecond laser pulses;
[0030] The λ / 2 wave plate and polarization cube beam splitter are used to control the power and polarization state of the femtosecond laser pulse;
[0031] The 4X beam expander is used to expand the diameter of the femtosecond laser pulse;
[0032] The beam shaping system is used to shape the femtosecond laser pulse and realize beam homogenization, so as to ensure that the energy distribution of the femtosecond laser pulse emitted to the chromium-silicon-nickel-molybdenum metal film is uniform;
[0033] The scanning galvanometer system is used to adjust the beam direction of the femtosecond laser pulse so that the femtosecond laser can irradiate a designated area of the chromium-silicon-nickel-molybdenum metal film;
[0034] The focusing mirror is used to focus the femtosecond laser to form a plasma channel, and the plasma channel is located in front of the chromium-silicon-nickel-molybdenum metal film.
[0035] Compared with the annealing disclosed in the prior art, the present invention uses a femtosecond laser to form a plasma above the chromium-silicon-nickel-molybdenum metal film for annealing, and the annealing time is extremely short. In one embodiment, the entire annealing of a 4-inch wafer can be achieved in 10-30 minutes. In summary, the femtosecond laser plasma channel annealing technology provided by the present invention can achieve annealing over a large area and in a very short time.
[0036] Further preferably, the plasma channel is located 0.3-0.5 mm in front of the chromium-silicon-nickel-molybdenum metal film. Since the energy of the femtosecond laser is relatively high, if it is directly focused on the surface of the chromium-silicon-nickel-molybdenum metal film, the surface is easily burned directly. By adjusting the distance between the plasma channel and the chromium-silicon-nickel-molybdenum metal film, the chromium-silicon-nickel-molybdenum metal film is avoided from being overburned, and annealing can be achieved on a larger area of the chromium-silicon-nickel-molybdenum metal film.
[0037] Preferably, the laser pulse energy of the femtosecond laser plasma channel annealing technology is 1.5-2.0 mJ, the scanning speed is 20-50 mm / s, and the scanning spacing is 200-250 um.
[0038] Preferably, a PI passivation layer is spin-coated on the heat-treated chromium-silicon-nickel-molybdenum metal film, the curing temperature is 350° C., the developing solution is cyclopentanone, and the rinsing solution is propylene glycol methyl ether acetate.
[0039] Further preferably, the thickness of the PI passivation layer is 3-20 um.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] The present invention adopts near-infrared light femtosecond laser that can completely penetrate the oxide silicon wafer substrate to induce back-side patterned etching of chromium silicon nickel molybdenum metal film. Since sampling back-side etching is used, the etched chromium silicon nickel molybdenum metal film will not contaminate the unetched chromium silicon nickel molybdenum metal film. Due to the use of femtosecond laser induced back removal technology, the interaction between the laser and the material is completed in an extremely short time, which is much shorter than the time required for thermal diffusion, and will not affect the lattice. Etching can be completed efficiently, effectively reducing the edge roughness of the resistor film and improving the accuracy and stability of the resistor.
[0042] The present invention adopts femtosecond laser plasma channel annealing technology to anneal the chromium silicon nickel molybdenum metal film of S3. Based on the high energy density of the laser, and the controllable spot size and spatial position, the local area of the sample can be uniformly heated in a very short time, achieving rapid annealing, greatly shortening the annealing time, and improving production efficiency. The chromium silicon nickel molybdenum metal film lattice can be precisely controlled by adjusting the various parameters of the femtosecond laser plasma channel annealing technology. The laser annealing process can greatly improve various structural defects in the resistance film, and avoid the presence of structural defects causing changes in the conduction electron density and scattering of carriers. In this way, the film changes from a metastable state to a stable state, and the film performance tends to be stable, thereby improving the resistivity and temperature coefficient of the resistance film.
[0043] The invention is based on the doping of nickel and molybdenum metals, which can cause the electronic structure of the chromium silicon film to change, split the energy level, narrow the band gap, make the electronic structure more stable, improve the stability of the film, and reduce the resistance temperature coefficient of the chromium silicon high resistance film.
[0044] Compared with traditional wet etching, photolithography, thermal annealing and other processes, the preparation method provided by the present invention avoids the use of large amounts of chemical reagents, simplifies the preparation process, improves production efficiency, reduces environmental pollution and operational risks, and shows obvious advantages in process efficiency and cost control. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 A flow chart of a method for preparing a CrSi resistor film provided in a specific embodiment of the present invention;
[0046] Figure 2 A structural block diagram of a near-infrared femtosecond laser induced backside removal device provided in a specific embodiment of the present invention;
[0047] Figure 3 A structural block diagram of a femtosecond laser plasma channel annealing device provided in a specific embodiment of the present invention;
[0048] Figure 4 The resistor pattern of the CrSi resistor film provided in the specific embodiment of the present invention;
[0049] Figure 5 A physical picture of a CrSi resistor film provided in a specific embodiment of the present invention;
[0050] Figure 6 A curve diagram showing the change in resistance of a CrSi resistor film with applied temperature provided in a specific embodiment of the present invention. DETAILED DESCRIPTION
[0051] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0052] In order to solve the problem of poor stability and precision of the resistor film disclosed in the prior art, the specific embodiment of the present invention uses femtosecond laser induced back etching of selected areas to avoid the influence of etching residues on the unetched parts. At the same time, the femtosecond laser induced back removal technology is used. Due to the extremely short pulse time, the interaction between the laser and the material is completed in a very short time, which is much shorter than the time required for thermal diffusion, thereby avoiding the influence of heat on the film lattice and making the roughness of the film edge lower. In addition, the present invention uses femtosecond laser to achieve efficient annealing of the film, and can achieve precise control of the crystal structure of the film by adjusting the parameters of the femtosecond laser. In addition, the method provided by the present invention avoids the use of a large amount of chemical reagents, simplifies the preparation process, and improves production efficiency. It provides a process basis for the integrated application of chromium silicon thin film resistors.
[0053] like Figure 1 As shown, a specific embodiment of the present invention provides a method for preparing a CrSi resistor film, comprising:
[0054] S1. A chromium-silicon-nickel-molybdenum metal film is deposited on a silicon oxide wafer substrate.
[0055] In a specific embodiment, the present invention uses magnetron sputtering to plate a chromium-silicon-nickel-molybdenum metal film on a silicon oxide wafer substrate, wherein the mass fractions of chromium, silicon, nickel, and molybdenum are 40%, 55%, 3%, and 2%, respectively. During the sputtering process, the flow ratio of argon and nitrogen is 300-500:1, and the thickness of the prepared chromium-silicon-nickel-molybdenum alloy metal film is 10-20nm.
[0056] S2, using near-infrared femtosecond laser to induce the removal of the chromium-silicon-nickel-molybdenum metal film in the selected area on the back, the specific steps are as follows:
[0057] The specific embodiment of the present invention uses the back side of the first device to remove the chromium-silicon-nickel-molybdenum metal film in the selected area, such as Figure 2 As shown, the first device includes a femtosecond laser amplifier 1, an electrically controlled optical shutter 2, a first λ / 2 wave plate 3, a polarizer 4, a 4X beam expander 5, a second λ / 2 wave plate 6, an optical parametric amplifier 7, a CCD 8, a dichroic mirror 9, a 10x microscope objective 10, and an xyz three-dimensional electrically controlled displacement platform 12. The laser pulse wavelength output by the femtosecond laser amplifier 1 provided in this embodiment is 800nm, and the pulse width is 30fs. The laser pulse passes through the electrically controlled optical shutter 2, the first λ / 2 wave plate 3, the polarizer 4, the 4X beam expander 5, the second λ / 2 wave plate 6, the optical parametric amplifier 7, the dichroic mirror 9, and the 10x microscope objective 10 in sequence, and finally focuses on the interface of the chromium-silicon-nickel-molybdenum alloy metal film 11.
[0058] Among them, the electrically controlled light gate 2 provided in this embodiment is used to control the passage and cutoff of the light path, the first λ / 2 wave plate 3 and the polarizer 4 adjust the energy of the single pulse of the femtosecond laser, and the polarization direction of the obtained light beam is vertical polarization. The optical parametric amplifier 7 is used to obtain a laser light beam with a wavelength of 1064nm to achieve complete transmission through the silicon oxide wafer substrate. The second λ / 2 wave plate 6 adjusts the light beam from vertical polarization to horizontal polarization, and the light beam is divided into two light beams by a dichroic mirror. The laser beam is focused on the interface between the silicon oxide wafer substrate and the chromium-silicon-nickel-molybdenum metal film in the selected area through the CCD and the 10x microscope objective lens to remove the chromium-silicon-nickel-molybdenum metal film in the selected area. During the processing, the laser pulse energy is set to 0.2-0.5μJ, the scanning speed is set to 2-5mm / s, and the scanning spacing is set to 3um.
[0059] S3. A specific embodiment of the present invention forms an aluminum-copper alloy electrode on a chromium-silicon-nickel-molybdenum metal film.
[0060] In a specific embodiment, the magnetron sputtering aluminum-copper alloy electrode is prepared by using a hard mask, wherein the hard mask is prepared based on femtosecond laser filament ablation technology, and the thickness of the aluminum-copper alloy is 1.0-1.2 μm.
[0061] S4, heat treating the chromium-silicon-nickel-molybdenum metal film of step S3 by femtosecond laser plasma channel annealing technology, the specific steps are:
[0062] The specific embodiment of the present invention uses the second device to heat treat the chromium-silicon-nickel-molybdenum metal film in step S3, such as Figure 3 As shown, the second device includes a femtosecond laser amplifier 1, an electrically controlled optical shutter 2, a λ / 2 wave plate 3, a polarization cube beam splitter 4, a 4X beam expander 5, a beam shaping system 6, a scanning galvanometer system 7, a focusing mirror 8 with a focal length of 20 cm, and a sample stage 10 with a chamber. The laser pulse wavelength output by the femtosecond laser amplifier 1 is 800nm, and the pulse width is 30fs. The laser pulse passes through the electrically controlled optical shutter 2, the λ / 2 wave plate 3, the polarization cube beam splitter 4, the 4X beam expander 5, the beam shaping system 6, the scanning galvanometer system 7, and the focusing mirror 8 with a focal length of 20 cm in sequence, and finally focuses on the surface of the chromium-silicon-nickel-molybdenum metal film 9 to form a plasma channel, and the film surface is fine-tuned to be located 0.3mm behind the plasma channel. The λ / 2 wave plate 3 and the polarization cube beam splitter 4 control the laser power and polarization state. The beam shaping system 6 is used to shape the initial beam and realize beam homogenization to ensure uniform energy distribution of the outgoing laser. During the processing, the sample is kept in a nitrogen atmosphere. The laser pulse energy is set to 1.5-2.0mJ, the scanning speed is set to 5-40mm / s, and the scanning spacing is set to 100um.
[0063] S5. Patterning a PI passivation layer on the heat-treated chromium-silicon-nickel-molybdenum metal film.
[0064] In a specific embodiment, the thickness of the PI layer provided in this embodiment is 3-20 um, the curing temperature is 350° C., the developing solution is cyclopentanone, and the rinsing solution is propylene glycol methyl ether acetate.
[0065] In a specific embodiment, this embodiment provides a method for preparing a CrSi resistor film, comprising:
[0066] Step 1: Place the silicon oxide wafer substrate material in the acetone organic tank and ethanol organic tank of the acid-base cleaning machine (Suzhou Xinsi Electronic Technology Co., Ltd.) in turn for ultrasonic cleaning, then place it in a deionized water tank for quick rinse to remove pollutants on the surface of the substrate, and finally place it in a vertical wafer spin dryer (Wuxi Quanyi Technology Co., Ltd.) for spin drying.
[0067] Step 2: Place the cleaned silicon oxide wafer substrate into the pre-evacuation chamber of a fully automatic magnetron sputtering coating machine (Beijing Chuangshi Weina Technology Co., Ltd.), introduce argon gas into the pre-evacuation chamber, and use RF sputtering to perform RF cleaning on the device for 5 minutes to further reduce surface impurity contamination. After the RF cleaning is completed, the sample is transferred to the sputtering chamber by a manipulator, and the chamber is evacuated by a combination of a mechanical pump and a molecular pump. After the chamber is evacuated to the background vacuum (8.0×10-4Pa), argon and nitrogen are introduced into the chamber, and the flow rate of argon and nitrogen is controlled by a mass flow meter to a ratio of 300-500:1, and chromium, silicon, nickel, and molybdenum metal thin films are plated using DC magnetron sputtering technology.
[0068] Step 3: Place the chromium silicon nickel molybdenum metal film on the xyz three-dimensional electric control displacement platform 12, use near-infrared femtosecond laser to induce the back removal of the chromium silicon nickel molybdenum alloy metal film, focus the laser spot on the interface between the silicon oxide substrate and the chromium silicon nickel molybdenum alloy metal film by adjusting the Z-axis platform and the coaxial CCD camera, optimize the laser processing parameters, and remove the chromium silicon nickel molybdenum alloy metal film by controlling the programmed movement of the two-dimensional electric control displacement platform. The processing process is monitored in real time by the CCD coaxial camera. During the processing, the laser pulse energy is set to 0.2-0.5μJ, the scanning speed is set to 2-5mm / s, and the scanning spacing is set to 3um.
[0069] Step 4: Place the hard mask prepared by femtosecond laser filament ablation technology on the surface of the prepared sample, and use DC magnetron sputtering technology to plate patterned aluminum-copper alloy electrodes, with the thickness of the aluminum-copper alloy being 1.0-1.2 μm.
[0070] Step 5: Place the above sample on a sample stage with a chamber, with nitrogen as the protective gas in the chamber, and use femtosecond laser plasma channel annealing to treat the chromium-silicon-nickel-molybdenum alloy metal film. Fine-tune the film surface to be 0.3mm behind the plasma channel, and write a Visual Studio program to control the deflection of the lens in the scanning galvanometer system, uniformly heat the local area of the sample, and achieve rapid annealing. During the processing, ensure that the sample is in a nitrogen atmosphere, the laser pulse energy is set to 1.5-2.0mJ, the scanning speed is set to 20-50mm / s, and the scanning spacing is set to 200-250um.
[0071] Step 6: Spin a PI passivation layer on the sample surface using a coating developer (Ningbo Runhua Quanxin Microelectronics Co., Ltd.), set the speed to 1500-4000rpm / s, bake on a 110℃ hot plate for 240s after spin coating, expose and develop the sample, the exposure dose is 100-300mJ / cm2, and cure in a computer oxygen-free oven (Hefei Zhenping Electronic Technology Co., Ltd.), the curing temperature is 350 degrees Celsius, and the oxygen concentration during the curing process is less than 100ppm. Polyimide (PI, polyimide) is often used as a protective layer together with the passivation layer material PAssivation (PA, usually a silicon-containing material) in semiconductor manufacturing due to its good electrical properties, chemical resistance, mechanical and thermodynamic stability, to improve the reliability of the device.
[0072] like Figure 4 and 5 As shown, the resistor layout and physical picture of the CrSi resistor film prepared in this embodiment.
[0073] Figure 6 The curve showing the change of the sheet resistance of the CrSi resistor film prepared in this embodiment with the applied temperature shows that the resistivity thereof is better than 20 ppm / °C.
Claims
1. A method for preparing a CrSi resistor film, characterized in that: include: S1, coating a chromium-silicon-nickel-molybdenum metal film on an oxide silicon wafer substrate; S2, using near-infrared femtosecond laser to induce the back removal of the Cr-Si-Ni-Mo metal film in the selected area; S3, forming an aluminum-copper alloy electrode on the chromium-silicon-nickel-molybdenum metal film; S4, heat treating the chromium-silicon-nickel-molybdenum metal film of step S3 by femtosecond laser plasma channel annealing technology; S5. Patterning a PI passivation layer on the heat-treated chromium-silicon-nickel-molybdenum metal film.
2. The method for preparing the CrSi resistor film according to claim 1, characterized in that: A chromium-silicon-nickel-molybdenum metal film is deposited on a silicon oxide wafer substrate in an argon and nitrogen atmosphere by magnetron sputtering.
3. The method for preparing the CrSi resistor film according to claim 2, characterized in that: The mass fractions of chromium, silicon, nickel and molybdenum are 40-43%, 55%, 1-3% and 1-2% respectively. During the magnetron sputtering process, the flow ratio of argon gas to nitrogen gas is 300-500:
1.
4. The method for preparing the CrSi resistor film according to claim 1, characterized in that: Removing the chromium-silicon-nickel-molybdenum metal film in the selected area from the back by a first device using a near-infrared femtosecond laser to induce the back removal, wherein the first device includes a femtosecond laser amplifier arranged in the direction of light propagation, an electrically controlled optical shutter, a first λ / 2 wave plate, a polarizer, a 4X beam expander, a second λ / 2 wave plate, an optical parametric amplifier, a dichroic mirror, a CCD camera, a 10x microscope objective lens, and an xyz three-dimensional electrically controlled displacement platform; The femtosecond laser amplifier is used to generate femtosecond laser pulses, the laser pulse wavelength is 800nm, and the pulse width is 30fs; The electrically controlled shutter is used to control the passage and cutoff of femtosecond laser pulses; The first λ / 2 wave plate and polarizer are used to adjust the energy of the femtosecond laser pulse, and the polarization direction of the obtained light beam is vertical polarization; The 4X beam expander is used to expand the beam diameter of the femtosecond laser pulse; The second λ / 2 wave plate is used to adjust the polarization direction of the femtosecond laser pulse from vertical polarization to horizontal polarization; The optical parametric amplifier is used to obtain a laser beam with a wavelength of 1064nm; The dichroic mirror, CCD camera and 10x microscope objective are used to focus the laser beam to the interface between the silicon oxide substrate and the chromium silicon nickel molybdenum metal film in the selected area to remove the chromium silicon nickel molybdenum metal film in the selected area.
5. The method for preparing the CrSi resistor film according to claim 1, characterized in that: The laser pulse energy induced by the near-infrared femtosecond laser is 0.2-0.5 μJ, the scanning speed is 2-5 mm / s, and the scanning interval is 1-3 um.
6. The method for preparing the CrSi resistor film according to claim 1, characterized in that: The aluminum-copper alloy electrode is prepared by using a hard mask, wherein the hard mask is prepared based on femtosecond laser filament ablation technology, and the thickness of the aluminum-copper alloy is 1.0-1.2μm.
7. The method for preparing a CrSi resistor film according to claim 1, characterized in that: The chromium-silicon-nickel-molybdenum metal film of step S3 is heat-treated by a second device using a femtosecond laser plasma channel annealing technology, wherein the second device includes a femtosecond laser amplifier, an electrically controlled optical shutter, a λ / 2 wave plate, a polarization cube beam splitter, a 4X beam expander, a beam shaping system, a scanning galvanometer system, a focusing mirror with a focal length of 20 cm, and a sample stage with a chamber arranged in a light propagation direction; The femtosecond laser amplifier is used to generate femtosecond laser pulses, the laser pulse wavelength is 800nm, and the pulse width is 30fs; The electrically controlled shutter is used to control the passage and cutoff of femtosecond laser pulses; The λ / 2 wave plate and polarization cube beam splitter are used to control the power and polarization state of the femtosecond laser pulse; The 4X beam expander is used to expand the diameter of the femtosecond laser pulse; The beam shaping system is used to shape the femtosecond laser pulse and realize beam homogenization, so as to ensure that the energy distribution of the femtosecond laser pulse emitted to the chromium-silicon-nickel-molybdenum metal film is uniform; The scanning galvanometer system is used to adjust the beam direction of the femtosecond laser pulse so that the femtosecond laser can irradiate a designated area of the chromium-silicon-nickel-molybdenum metal film; The focusing mirror is used to focus the femtosecond laser to form a plasma channel, and the plasma channel is located in front of the chromium-silicon-nickel-molybdenum metal film.
8. The method for preparing the CrSi resistor film according to claim 7, characterized in that: The plasma channel is located 0.3-0.5 mm in front of the chromium-silicon-nickel-molybdenum metal film.
9. The method for preparing a CrSi resistor film according to claim 1, characterized in that: The laser pulse energy of the femtosecond laser plasma channel annealing technology is 1.5-2.0 mJ, the scanning speed is 20-50 mm / s, and the scanning spacing is 200-250 um.
Citation Information
Patent Citations
Method for improving moisture and heat resistance of Cr-Si high resistance film resistor based on electro-catalytic property
CN104485190A
Method of utilizing laser plasma thin filaments to prepare metal multifunctional surface
CN106141438A
Preparation method of nickel-chromium-silicon film low in resistance temperature coefficient
CN106435478A
Process for preparing resistive films
GB1112756A
Method for the protection against corrosion of a steel part made of austentic or semi-austentic steel during the production of sulfuric acid
US20040238375A1
Cited By
Thin film resistor and method of forming the same
TWI909992B