Film coating method and equipment for electric shock resistant and laser damage resistant film
By monitoring the gas flow rate in real time and building a temperature solution model in the vacuum reaction chamber, controlling the plasma reaction, the problems of inconsistency and flatness of the film on the surface of the coating substrate are solved, efficient HfO2 oxidation film deposition is achieved, and the performance of the coating is improved. patience.
Patent Information
- Application Number
- CN202411052417.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to control plasma reactions under real-time optimal temperature and pressure conditions, resulting in film inconsistency and flatness on the surface of the coated substrate.
The atomic deposition method is used to monitor the gas flow rate in real time in the vacuum reaction chamber through the supercycle process of ozone and hafnium sources, build a dynamic equilibrium equation and temperature solution model, control the plasma reaction temperature and pressure, and form an HfO2 oxide film.
The uniform deposition and precise thickness control of high aspect ratio structures are achieved, the uniformity and dielectric properties of the coating are improved, and the resistance to electric shock and laser damage is enhanced.
Smart Images

Figure CN118979243A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plasma coating, and in particular relates to a coating method and equipment for a film resistant to electric shock and laser damage. Background Art
[0002] Optical materials and semiconductor materials coating technology have shown broad application prospects in many fields, including optical communications, displays, instruments, storage and sensors, etc. These application fields have put forward higher requirements for improving product performance, reducing costs and environmental protection. With the continuous advancement of science and technology and the continuous changes in market demand, optical coating technology has shown broad application prospects in many fields. In the field of optical communications, optical coating technology can improve the transmission efficiency and signal quality of optical fibers, while reducing the loss and noise of optical fibers. In the field of optical display, it can improve the brightness, contrast and color saturation of displays, while reducing reflection and glare. In the field of optical instruments, optical coating technology can improve the resolution, sensitivity and accuracy of instruments, while reducing reflection and scattering. In addition, in the fields of optical storage, optical sensors, semiconductor sensors, etc., optical material coating technology and semiconductor material coating technology also play an important role, for example, improving read and write speed, storage density, sensitivity, response speed, while reducing bit error rate, noise and interference.
[0003] In recent years, the market for optical coating machines has shown a trend of rapid growth, mainly due to increased demand and technological progress. With the rapid development of industries such as electronic products and communication equipment, the demand for high-performance optical devices and semiconductor devices has gradually increased. Optical coating technology can improve the performance of optical devices, enabling them to have better optical transmission and processing capabilities, so the demand for optical coating machines has also increased accordingly. In addition, with the development of optical materials and devices, the requirements for optical coating technology have become increasingly higher. In recent years, the technological innovation and improvement of optical coating machines have enabled them to have advantages such as higher film uniformity and more precise film control capabilities. As in the prior art, the Chinese patent application document with application number 202211393937.0 discloses a method for preparing an integrated wafer-level hydrogen sulfide gas-sensitive film and a single MEMS hydrogen sulfide gas-sensitive film. Before atomic layer deposition ALD, the method first cleans and dries the wafer MEMS, transfers the MEMS to the ALD reactor, and deposits a ZnO film using diethyl zinc and water as precursors. The number of cycles of ALD ZnO deposition on the MEMS is controlled to obtain ZnO films of different thicknesses. For example, the Chinese patent application document with application number 202410220803.1 discloses a method for preparing a marine anticorrosive film layer, in which the substrate is processed and placed in the reaction chamber of a plasma enhanced atomic layer deposition coating device, and after the reaction chamber is purged with argon, the sample surface is bombarded with oxygen plasma to obtain a sample to be coated; then the ethylmethylamino hafnium pipeline is opened to react with the sample surface obtained in step (1), and the reaction chamber is purged with argon; then the ozone pipeline is opened, the ozone pipeline flow and time are set, and ozone continues to react with the sample surface, and the reaction chamber is purged with argon; the above two steps are cycled to obtain a film with anticorrosive ability. However, none of the above disclosed prior arts discloses how to control the reaction under the control conditions of the real-time optimal temperature and certain pressure conditions during the plasma reaction of the hafnium source and the oxygen plasma to the coated substrate of the optical material or the semiconductor material by pulse bombardment so that the film on the surface of the coated substrate obtained by the reaction has higher consistency and flatness. Summary of the invention
[0004] In view of the above-mentioned defects, the present invention provides a coating method and equipment for a film resistant to electric shock and laser damage.
[0005] The present invention provides the following technical solution: a coating method for a film resistant to electric shock and laser damage, the method is based on an atomic deposition method and comprises the following steps:
[0006] S1: pre-treating the film-coated substrate, and placing the pre-treated film-coated substrate in a vacuum reaction chamber;
[0007] S2: inputting ozone into the pre-treated surface of the coated substrate in the vacuum reaction chamber;
[0008] S3: inputting a hafnium source into the vacuum reaction chamber, regulating the temperature and pressure in the vacuum reaction chamber, and controlling the reaction temperature in the vacuum reaction chamber with a real-time dynamic optimal temperature to perform a plasma reaction;
[0009] S4: Repeat the steps S2-S3 500 times, and coat the HfO2 oxide film on the surface of the coating substrate to complete the coating.
[0010] As a further limitation of the present invention, the step S1 uses hydrofluoric acid with a mass fraction concentration of 1% to pretreat the coating substrate, so that hydrogen free ends are generated on the surface of the coating substrate.
[0011] As a further limitation of the present invention, the S2 step comprises the following steps:
[0012] S21: Open the nitrogen purge valve first and wait for 0.1s;
[0013] S22: then open the ozone inlet valve to input ozone to the surface pretreated in step S1 for 3 seconds;
[0014] S23: closing the ozone inlet valve, waiting for 2 seconds, and discharging the reaction byproducts and excess unreacted sources;
[0015] S24: close the nitrogen purge valve, wait for 8 seconds, and prepare to introduce the hafnium source while continuing to discharge the by-products.
[0016] As a further limitation of the present invention, the S3 step comprises the following steps:
[0017] S31: Open the hafnium source purge valve and wait for 0.1s;
[0018] S32: Open the hafnium source inlet valve, introduce the hafnium source, and wait for 0.3s; and control the temperature and pressure in the vacuum reaction chamber to control the reaction temperature in the vacuum reaction chamber with real-time dynamic optimal temperature to perform plasma reaction;
[0019] S33: closing the hafnium source inlet valve, waiting for 3 seconds, and discharging the reaction byproducts and excess unreacted source;
[0020] S34: Repeat steps S32-S33 3 times;
[0021] S35: close the hafnium source purge valve, wait for 2.5 seconds, and discharge the by-products.
[0022] As a further limitation of the present invention, the film-coated substrate is an optical material substrate or a semiconductor material substrate.
[0023] As a further limitation of the present invention, the optical material substrate is a square single crystal silicon wafer, and the size of the square single crystal silicon wafer is 125 mm, 150 mm or 156 mm;
[0024] The semiconductor material substrate is a single crystal silicon wafer, and the diameter of the single crystal silicon wafer is 150 mm, 200 mm or 300 mm.
[0025] As a further limitation of the present invention, the hafnium source used in step S3 is CpHf(NMe2)3.
[0026] As a further limitation of the present invention, during the plasma reaction process in step S3, the pressure in the vacuum reaction chamber is controlled to be 130 mPa to 135 mPa.
[0027] As a further limitation of the present invention, the step S2 of controlling the reaction temperature in the reaction chamber with the real-time dynamic optimal temperature to perform a plasma reaction comprises the following steps:
[0028] S321: Using a transverse gas flow rate monitoring sensor and a longitudinal gas flow rate monitoring sensor disposed on the surface of the coating substrate to respectively monitor the transverse x-axis flow rate v of the hafnium source on the surface of the coating substrate in real time x , the flow rate v of the hafnium source in the longitudinal y-axis y ;
[0029] S322: Construct the dynamic balance equation of the flow of hafnium source on the surface of the coating substrate:
[0030]
[0031] Among them, ρ Hf is the gas density of the hafnium source, σ is the gas molecular viscosity of the hafnium source; x is the x-axis position coordinate of the coating substrate, y is the y-axis position coordinate of the ground film substrate; v x is the real-time lateral flow rate of the hafnium source gas obtained by real-time monitoring; v y The real-time longitudinal flow rate of the hafnium source gas is obtained by real-time monitoring;
[0032] S323: Under the condition of the dynamic equilibrium equation of the hafnium source flow on the surface of the coating substrate constructed in step S323, a real-time dynamic optimal temperature solution model for the plasma reaction is constructed:
[0033]
[0034] Wherein, K is the gas thermal conductivity coefficient of the hafnium source, k is the Boltzmann constant, and T(t) is the real-time dynamic temperature in the vacuum reaction chamber;
[0035] S324: The result T obtained by solving the step S323best (t) as a real-time dynamic optimal temperature for controlling the plasma reaction in the reaction chamber.
[0036] The present invention also provides a coating device for an electric shock-resistant and laser damage-resistant film using the method described above, characterized in that the device includes a coating substrate pretreatment chamber, a coating substrate conveying robotic arm, a vacuum reaction chamber, a nitrogen purge valve, an ozone inlet valve, a hafnium source purge valve, a hafnium source inlet valve, a lateral gas flow rate monitoring sensor and a longitudinal gas flow rate monitoring sensor arranged on the surface of the coating substrate, and a remote control single-chip microcomputer, wherein the remote control single-chip microcomputer controls the device to execute steps S1-S4 of any of the methods described above.
[0037] The beneficial effects of the present invention are:
[0038] 1. The present invention is based on atomic deposition technology. It first introduces ozone to form a layer of film with oxygen free radicals on the coating surface, then introduces hafnium source CpHf(NMe2)3 after purging with nitrogen, and further reacts with oxygen free radicals on the coating surface under the optimal real-time temperature conditions controlled by PLC to generate a layer of HfO2 film; after repeating 500 times, a HfO2 film of a certain thickness is obtained; the present invention can achieve uniform deposition in high aspect ratio structures and achieve precise thickness control at the atomic level. The present invention is based on atomic deposition technology for film coating. By controlling the introduction time of ozone and hafnium source, the composition ratio of the deposited material in the plasma reaction process can be flexibly adjusted. Through 500 super cycles of each component, the composition control of the film obtained by atomic deposition can be achieved.
[0039] 2. The present invention controls the ozone introduction time and uses nitrogen to purge before and after the ozone introduction to avoid the residue of other impurities on the coating surface, thereby avoiding the generation of impurities other than HfO2 by other impurities and the hafnium source during the plasma reaction. At the same time, the introduction time of the hafnium source is precisely controlled and purged after the reaction, thereby avoiding the interface mismatch that leads to more structural defects at the interface, thereby avoiding the occurrence of defects such as leakage channels that lead to a decrease in the insulation performance of the film when a voltage is applied to the coating substrate material (optical material or semiconductor material), thereby improving the dielectric properties and laser damage resistance of the coating substrate.
[0040] 3. The coating substrate of the present invention can be an optical material substrate or a semiconductor material substrate, which improves the application scope and extensiveness of the coating method.
[0041] 4. The present invention uses a PLC control method to perform real-time optimal temperature control on the plasma reaction process in the vacuum reaction chamber, thereby ensuring a balanced reaction between the hafnium source and the oxygen free radicals of ozone on the surface of the coating substrate material during the plasma reaction. The dynamic equilibrium equation of the hafnium source flow on the coating substrate surface is constructed as follows: Under the limited conditions, the real-time dynamic optimal temperature solution model of plasma reaction is constructed: Then, the optimal real-time temperature of the plasma reaction after the hafnium source enters is solved, which avoids the situation in which the HfO2 film growth rate is too slow or the film becomes loose or the interface molecular structure defects occur due to the temperature being too high or too low during the plasma reaction after the hafnium source enters. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The present invention will be described in more detail below based on embodiments and with reference to the accompanying drawings, wherein:
[0043] Figure 1 A schematic flow chart of a coating method for a film resistant to electric shock and laser damage provided by the present invention;
[0044] Figure 2 This is a schematic diagram of the overall structure of the coating equipment used in the present invention.
[0045] Figure 3 This is a FIB test result diagram of the product after coating by the method provided by the present invention;
[0046] Figure 4 A graph showing the refractive index value of the film layer of the product after coating by the method provided by the present invention at a 1nm emission wave;
[0047] Figure 5 A graph showing the refractive index value of the film layer of the product after coating by the method provided by the present invention under the 550nm emission wave; DETAILED DESCRIPTION
[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] like Figure 1 As shown, the present invention provides a method for coating a film resistant to electric shock and laser damage, the method is based on an atomic deposition method, and comprises the following steps:
[0050] S1: pre-treating the coating substrate, and placing the pre-treated coating substrate in a vacuum reaction chamber;
[0051] S2: Input ozone (O3) into the pre-treated coating substrate surface in the vacuum reaction chamber;
[0052] S3: inputting a hafnium source into the vacuum reaction chamber, regulating the temperature and pressure in the vacuum reaction chamber, and controlling the reaction temperature in the vacuum reaction chamber with a real-time dynamic optimal temperature to perform a plasma reaction;
[0053] S4: Repeat steps S2-S3 500 times to coat a HfO2 oxide film on the surface of the coating substrate to complete the coating.
[0054] The present invention adopts the atomic deposition method to super-circulate the introduction of ozone and hafnium source, thereby coating the surface of the coating substrate with the advantages of high shape retention, high film quality, good surface uniformity, precise thickness control, and no porosity.
[0055] As another preferred embodiment of the present invention, in order to enable the ozone to form oxygen free radicals on the surface of the coated substrate material during the ozone introduction process, and then facilitate the plasma reaction with the hafnium source introduced subsequently, the coated substrate material needs to be activated. In step S1, the coated substrate is pretreated with hydrofluoric acid with a mass fraction concentration of 1%, so that hydrogen free ends are generated on the surface of the coated substrate. Then, when ozone is introduced, the ozone can easily combine with H· generated by the coating substrate material being activated by hydrofluoric acid acidification, and then adhere to the surface of the coated substrate to form oxygen free radicals.
[0056] As another preferred embodiment of the present invention, step S2 includes the following steps:
[0057] S21: Open the nitrogen purge valve first and wait for 0.1s;
[0058] S22: Then open the ozone inlet valve to input ozone (O3) to the surface pretreated in step S1 for 3 seconds;
[0059] S23: Close the ozone inlet valve, wait for 2 seconds, and discharge the reaction by-products and excess unreacted sources;
[0060] S24: Close the nitrogen purge valve, wait for 8 seconds, and prepare to introduce the hafnium source while continuing to discharge the by-products.
[0061] By controlling the ozone introduction time and further controlling the ozone shut-off time after the ozone introduction through the above-mentioned steps S21-S22, it is beneficial to discharge the reaction by-products and excess unreacted sources, and then further controlling the nitrogen purge time by PLC to further discharge the undischarged ozone to avoid other impurities on the surface of the coating substrate reacting with the subsequent hafnium source; by controlling the ozone introduction time and further purging with nitrogen, it is also avoided that the defects such as interface mismatch and dangling bonds introduced by the difference in interface characteristics between the components in the super-cycle process of the prior art through atomic deposition method are avoided, which leads to the phenomenon of degradation of film performance.
[0062] As another preferred embodiment of the present invention, in order to accurately control the amount of the hafnium source component introduced during the super-cycle process of introducing ozone and hafnium source in atomic deposition, it is necessary to control the hafnium source introduction valve and closing time. Therefore, as another preferred embodiment of the present invention, step S3 includes the following steps:
[0063] S31: Open the hafnium source purge valve and wait for 0.1s;
[0064] S32: Open the hafnium source inlet valve, introduce the hafnium source, and wait for 0.3s; and control the temperature and pressure in the vacuum reaction chamber to control the reaction temperature in the vacuum reaction chamber with the real-time dynamic optimal temperature to perform plasma reaction;
[0065] S33: close the hafnium source inlet valve, wait for 3 seconds, and discharge the reaction byproducts and excess unreacted source;
[0066] S34: Repeat steps S32-S33 3 times;
[0067] S35: Close the hafnium source purge valve, wait 2.5 seconds, and discharge the by-products.
[0068] Preferably, the hafnium source used in step S3 is CpHf(NMe2)3.
[0069] By controlling the time of introduction and purge of the hafnium source, the amount of the hafnium source introduced can be effectively controlled, and the thin film product produced on the surface of the coated substrate can be accurately controlled to be HfO2. After the hafnium source is introduced for plasma reaction, it is purged to ensure that the hafnium source will not produce other reaction impurities with other substances in the vacuum reaction chamber before the next introduction of ozone, causing defects on the coating surface.
[0070] Preferably, the film-coated substrate is an optical material substrate or a semiconductor material substrate.
[0071] The coating substrate of the present invention can be an optical material substrate or a semiconductor material substrate. The optical material substrate is a square single crystal silicon wafer. The size of the square single crystal silicon wafer is 125 mm, 150 mm or 156 mm.
[0072] The semiconductor material substrate is a single crystal silicon wafer, and the diameter of the single crystal silicon wafer is 150 mm (6-inch wafer), 200 mm (8-inch wafer) or 300 mm (12-inch wafer).
[0073] Furthermore, in order to ensure that the plasma reaction in the vacuum reaction chamber is precisely controlled in a super cycle during the super cycle process, thereby improving the consistency and flatness of the coating, as another preferred embodiment of the present invention, the pressure in the vacuum reaction chamber is controlled to be 130mPa~135mPa during the plasma reaction process in step S3.
[0074] Atomic layer deposition (ALD) is an emerging chemical deposition technology with great advantages in coating quality and coating efficiency. ALD is greatly affected by temperature, so it is very important to analyze and study the influence of its parameters on the uniformity of temperature distribution. Therefore, it is necessary to perform real-time optimal control of the temperature of ozone and hafnium sources during the plasma reaction on the surface of the coating substrate. As another preferred embodiment of the present invention, the plasma reaction in the reaction chamber is controlled by real-time dynamic optimal temperature in step S2, which includes the following steps:
[0075] S321: Using a transverse gas flow rate monitoring sensor and a longitudinal gas flow rate monitoring sensor disposed on the surface of the coating substrate to respectively monitor the transverse x-axis flow rate v of the hafnium source on the surface of the coating substrate in real time x , the flow rate v of the hafnium source in the longitudinal y-axis y ;
[0076] S322: Construct the dynamic balance equation of the flow of hafnium source on the surface of the coating substrate:
[0077]
[0078] Among them, ρ Hf is the gas density of the hafnium source, σ is the gas molecular viscosity of the hafnium source; x is the x-axis position coordinate of the coating substrate, y is the y-axis position coordinate of the film substrate; v x is the real-time lateral flow rate of the hafnium source gas obtained by real-time monitoring of the lateral gas flow rate monitoring sensor; v y The real-time longitudinal flow rate of the hafnium source gas is obtained by real-time monitoring of the longitudinal gas flow rate monitoring sensor;
[0079] S323: Under the condition of the dynamic equilibrium equation of the hafnium source flow on the surface of the coating substrate constructed in step S323, a real-time dynamic optimal temperature solution model for the plasma reaction is constructed:
[0080]
[0081] Where, K is the gas thermal conductivity of the hafnium source, k is the Boltzmann constant, T(t) is the real-time dynamic temperature in the vacuum reaction chamber (an unknown number to be solved); C Hf is the specific heat capacity of the hafnium source gas;
[0082] S324: The result T obtained by solving the step S323 best (t) is used as the real-time dynamic optimal temperature for controlling the plasma reaction in the reaction chamber.
[0083] Through the above process, the PLC can accurately control the plasma reaction process after the hafnium source enters the vacuum reaction chamber in real time. The coating substrate temperature is coated at the optimal real-time temperature, and a HfO2 film with good consistency, flatness and uniformity without interface molecular structure defects is produced on the surface of the coating substrate; it avoids the situation that there may be a trace of physical adsorption in the atomic deposition process when the temperature is low without real-time optimal temperature control, which makes the deposition rate higher than the ideal saturated chemical adsorption level, and then leads to the occurrence of looser defects in the film under this condition. It also avoids the desorption of some precursors in the chemical adsorption state at high temperatures, thereby avoiding the growth rate of the film being lower than the ideal saturated chemical adsorption level under this situation.
[0084] The present invention also provides a coating device for a film resistant to electric shock and laser damage using the above method, the device comprising a coating substrate pretreatment chamber (used to be controlled by a remote-controlled single-chip computer to execute step S1 to pretreat the coating substrate), a coating substrate conveying robot arm (used to convey the coating substrate into a vacuum reaction chamber), a vacuum reaction chamber (used to provide a reaction space for ozone and hafnium source gas to perform plasma reaction on the surface of the coating substrate), a nitrogen purge valve arranged on the vacuum reaction chamber (used to purge residual ozone, so it is also called an ozone purge valve, for Figure 2 O3 purge valve in), ozone inlet valve (for Figure 2 O3 dose valve in the Figure 2 Hfpurge valve in the middle), hafnium source inlet valve (for Figure 2 The Hfdose valve in the coating substrate, the lateral gas flow rate monitoring sensor and the longitudinal gas flow rate monitoring sensor arranged on the surface of the coating substrate, and the remote control microcontroller control device execute the steps S1-S4 of the above method. Figure 2 The figure is a schematic diagram of the overall structure of the coating equipment used in the present invention.
[0085] Test Example 1
[0086] In order to verify the coating effect of the present invention, the product coated by the above method was subjected to FIB test. The test results are as follows: Figure 3As shown, the thickness of the irregular surface film layer on the surface of the coated substrate is between 111.3 and 126.2, and the step coverage rate reaches more than 85%.
[0087] Test Example 2
[0088] The JAWoollam M2000D spectral ellipsometer was used to measure the refractive index of the film after the product was coated by the above method. Figure 4 This is the test result of the emitted light wave of 1nm. Figure 5 This is the test result when the emitted light wave is 550nm, such as Figure 4-Figure 5 As shown, the uniformity of the coated substrate over an 8-inch area reaches ±1.4%.
[0089] Test Example 3
[0090] In addition, ex situ measurements were performed after coating using a JA Woollam M2000D spectroscopic ellipsometer to determine the final thickness and dielectric function in the spectral range of 1.25-6.5 eV.
[0091] Through the step S321-S324 method of the present invention, the real-time reaction temperature in the vacuum reaction chamber is subjected to PLC optimal real-time temperature control. During the coating process of the coating substrate, the growth rate (GPC) of the HfO2 film is 0.1 nm / cycle, which is closest to the ideal saturated adsorption rate. The HfO2 film at this temperature is the most uniform and dense, the surface RMS of the HfO2 film is less than 0.4 nm, the element O / Hf component ratio is 1.987, and the film components at different depths are uniform. The relative dielectric constant of the HfO2 film grown at this temperature is the largest, reaching 24.5. The corresponding HfO2 / coating substrate material interface state density is the smallest, 1.64×10 12 e / (V·cm 2 ).
[0092] It should be noted that the serial numbers of the above embodiments of the present invention are only for description and do not represent the advantages and disadvantages of the embodiments. And the terms "including", "comprising" or any other variants thereof in this article are intended to cover non-exclusive inclusion, so that a process, device, article or method including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, device, article or method. In the absence of further restrictions, an element defined by the sentence "including a ..." does not exclude the presence of other identical elements in the process, device, article or method including the element.
[0093] Through the description of the above implementation methods, those skilled in the art can clearly understand that the above-mentioned embodiment methods can be implemented by means of software plus a necessary general hardware platform, and of course by hardware, but in many cases the former is a better implementation method. Based on such an understanding, the technical solution of the present invention is essentially or the part that contributes to the prior art can be embodied in the form of a software product, which is stored in a storage medium (such as ROM / RAM, magnetic disk, optical disk) as described above, and includes a number of instructions for a terminal device (which can be a mobile phone, a computer, a server, or a network device, etc.) to execute the methods described in each embodiment of the present invention.
[0094] In particular, according to the embodiments provided by the present invention, the facial recognition smart door lock security management method provided by the present invention can be implemented as a computer software program. For example, a computer program product provided by the present invention includes a computer program carried on a computer-readable medium, and the computer program contains program code for executing the method shown in the flowchart. In such an embodiment, the computer program can be downloaded and installed from the network through a communication device, or installed from a storage device, or installed from a ROM. When the computer program is executed by a processing device, the above functions defined in the method of the embodiment of the present disclosure are executed.
[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for coating a film resistant to electric shock and laser damage, the method being based on an atomic deposition method and characterized in that: The following steps are involved: S1: pre-treating the film-coated substrate, and placing the pre-treated film-coated substrate in a vacuum reaction chamber; S2: inputting ozone into the pre-treated surface of the coated substrate in the vacuum reaction chamber; S3: inputting a hafnium source into the vacuum reaction chamber, regulating the temperature and pressure in the vacuum reaction chamber, and controlling the reaction temperature in the vacuum reaction chamber with a real-time dynamic optimal temperature to perform a plasma reaction; S4: Repeat the steps S2-S3 500 times, and coat the HfO2 oxide film on the surface of the coating substrate to complete the coating.
2. The coating method of the electric shock and laser damage resistant film according to claim 1, characterized in that: In the step S1, hydrofluoric acid with a mass fraction concentration of 1% is used to pretreat the coating substrate, so that hydrogen free ends are generated on the surface of the coating substrate.
3. The coating method of the electric shock and laser damage resistant film according to claim 1, characterized in that: The S2 step includes the following steps: S21: Open the nitrogen purge valve first and wait for 0.1s; S22: then open the ozone inlet valve to input ozone to the surface pretreated in step S1 for 3 seconds; S23: closing the ozone inlet valve, waiting for 2 seconds, and discharging the reaction byproducts and excess unreacted sources; S24: close the nitrogen purge valve, wait for 8 seconds, and prepare to introduce the hafnium source while continuing to discharge the by-products.
4. The coating method of the electric shock and laser damage resistant film according to claim 1, characterized in that: The S3 step includes the following steps: S31: Open the hafnium source purge valve and wait for 0.1s; S32: Open the hafnium source inlet valve, introduce the hafnium source, and wait for 0.3s; and control the temperature and pressure in the vacuum reaction chamber to control the reaction temperature in the vacuum reaction chamber with real-time dynamic optimal temperature to perform plasma reaction; S33: closing the hafnium source inlet valve, waiting for 3 seconds, and discharging the reaction byproducts and excess unreacted source; S34: Repeat steps S32-S33 3 times; S35: close the hafnium source purge valve, wait for 2.5 seconds, and discharge the by-products.
5. The coating method of the electric shock and laser damage resistant film according to claim 1, characterized in that: The film-coated substrate is an optical material substrate or a semiconductor material substrate.
6. The coating method of the electric shock and laser damage resistant film according to claim 3, characterized in that: The optical material substrate is a square single crystal silicon wafer, and the size of the square single crystal silicon wafer is 125 mm, 150 mm or 156 mm; The semiconductor material substrate is a single crystal silicon wafer, and the diameter of the single crystal silicon wafer is 150 mm, 200 mm or 300 mm.
7. The coating method of the electric shock and laser damage resistant film according to claim 1, characterized in that: The hafnium source used in the step S3 is CpHf(NMe2)3.
8. The coating method of the electric shock and laser damage resistant film according to claim 1, characterized in that: During the plasma reaction in step S3, the pressure in the vacuum reaction chamber is controlled to be 130 mPa to 135 mPa.
9. The method for coating a film resistant to electric shock and laser damage according to claim 4, characterized in that: The step S2 in which the reaction temperature in the reaction chamber is controlled by the real-time dynamic optimal temperature to perform a plasma reaction comprises the following steps: S321: Using a transverse gas flow rate monitoring sensor and a longitudinal gas flow rate monitoring sensor disposed on the surface of the coating substrate to respectively monitor the transverse x-axis flow rate v of the hafnium source on the surface of the coating substrate in real time x , the flow rate v of the hafnium source in the longitudinal y-axis y ; S322: Construct the dynamic balance equation of the flow of hafnium source on the surface of the coating substrate: Among them, ρ Hf is the gas density of the hafnium source, ρ is the gas molecular viscosity of the hafnium source; x is the x-axis position coordinate of the coating substrate, y is the y-axis position coordinate of the ground film substrate; v x is the real-time lateral flow rate of the hafnium source gas obtained by real-time monitoring; v y The real-time longitudinal flow rate of the hafnium source gas is obtained by real-time monitoring; S323: Under the condition of the dynamic equilibrium equation of the hafnium source flow on the surface of the coating substrate constructed in step S323, a real-time dynamic optimal temperature solution model for the plasma reaction is constructed: Wherein, K is the gas thermal conductivity coefficient of the hafnium source, k is the Boltzmann constant, and T(t) is the real-time dynamic temperature in the vacuum reaction chamber; C Hf is the specific heat capacity of the hafnium source gas; S324: The result T obtained by solving the step S323 best (t) as a real-time dynamic optimal temperature for controlling the plasma reaction in the reaction chamber.
10. A coating device for a film resistant to electric shock and laser damage using the method according to any one of claims 1 to 9, characterized in that: The equipment includes a coating substrate pretreatment chamber, a coating substrate conveying robot arm, a vacuum reaction chamber, a nitrogen purge valve, an ozone inlet valve, a hafnium source purge valve, a hafnium source inlet valve, a lateral gas flow rate monitoring sensor and a longitudinal gas flow rate monitoring sensor arranged on the surface of the coating substrate, and a remote control single chip microcomputer, wherein the remote control single chip microcomputer controls the equipment to perform steps S1-S4 of any method described in claims 1-9.