Preparation method of vanadium electrolyte
Through oxalic acid system extraction and electrolytic reduction technology, the problems of high costs and environmental pollution in the production of vanadium electrolyte are solved, and the efficient preparation of vanadium electrolyte and the simplification of wastewater treatment are achieved. It is suitable for a variety of vanadium raw materials.
Patent Information
- Application Number
- CN202411079984.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
AI Technical Summary
The existing vanadium electrolyte production technology has problems such as high cost, environmental pollution and low applicability to high Fe and high Ca vanadium raw materials, especially the complex wastewater treatment and difficulty in reusing the raffinate.
Using the oxalic acid system as the extraction stock solution, vanadium electrolyte is prepared by dissolution reduction, extraction-row extraction and electrolytic reduction steps, avoiding alkaline neutralization and impurity removal steps, simplifying wastewater treatment, and is suitable for high Fe content and low purity pentaoxide. Divana raw material.
It reduces the production cost of vanadium electrolyte, simplifies wastewater treatment, improves the vanadium enrichment effect and the scope of application of raw materials, and reduces environmental pollution.
Smart Images

Figure CN118979260A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of all-vanadium liquid flow batteries, and in particular relates to a method for preparing a vanadium electrolyte. Background Art
[0002] Vanadium electrolyte is one of the key materials for all-vanadium flow batteries. The purity of its raw materials greatly affects the performance of vanadium electrolyte. The existing vanadium electrolyte production technology mainly uses high-purity vanadium pentoxide as raw material. In order to reduce the production cost of vanadium electrolyte and promote the development of the vanadium battery industry, the vanadium battery field adopts the method of purifying low-purity vanadium raw materials such as vanadium-containing leaching solution, ammonium vanadate, and low-purity vanadium pentoxide to prepare high-purity vanadium electrolyte. The existing methods for purifying low-purity vanadium raw materials are relatively mature, mainly including alkaline dissolution-vanadium precipitation method and extraction-strip extraction method.
[0003] The alkali dissolution-vanadium precipitation method generally uses low-purity ammonium vanadate as raw material, and obtains high-purity ammonium vanadate through steps such as adding alkali for re-dissolution, impurity removal, and vanadium precipitation. It is then calcined to obtain high-purity vanadium pentoxide, and then the vanadium electrolyte is obtained through dissolution and reduction steps. This method has a long process and produces a large amount of high-sodium salt and high-ammonia nitrogen wastewater, which has high water treatment costs and causes great environmental pollution.
[0004] The extraction-stripping method is to extract vanadium oxide ions from vanadium-containing solution by using the extractant to select vanadium oxide ions, and then directly obtain an acidic solution of vanadium sulfate by stripping with sulfuric acid solution, and obtain vanadium electrolyte by adjusting the concentration. This method has a short process and low cost, and is widely used in the extraction of vanadium from acidic vanadium-containing mineral leachate. Therefore, in order to further reduce the production cost of vanadium electrolyte, the current research hotspot is to directly prepare high-purity vanadium electrolyte by extraction-stripping using metallurgical grade vanadium products as raw materials.
[0005] Patent document CN114275811A discloses a method for purifying crude vanadium compounds to prepare electrolytes, wherein the method comprises the following steps: reducing and calcining low-purity metallurgical-grade vanadium products into VO2 or vanadium oxysulfate VOSO4; then adding acid to dissolve the vanadium into vanadium oxysulfate or vanadium oxychloride solution; extracting vanadium with an organic extractant, and obtaining VO2-containing electrolytes through stripping. 2+ The solution containing VO 2+ The solution is electrolytically reduced to obtain a vanadium electrolyte with an average valence of 3.5. This method avoids the use of ammonium salts and is simple to treat wastewater. However, due to the use of a sulfuric acid system or a hydrochloric acid system, the heavy metal precipitate of the raffinate needs to be removed by adding a large amount of alkaline substances before it can be reused. At the same time, it may cause an increase in soluble impurities such as K and Na in the raffinate, reducing the solubility of vanadium. In addition, impurities such as Fe and Ca seriously affect the extraction agent's VO 2+ The extraction effect makes this method less applicable to high-Fe and high-Ca vanadium raw materials.
[0006] Therefore, there is an urgent need to develop a method for preparing a vanadium electrolyte with a wide range of raw material applications, simple wastewater treatment, easy recycling of raffinate, and good vanadium enrichment effect. Summary of the invention
[0007] In order to solve the problems existing in the prior art, the present invention provides a method for preparing a vanadium electrolyte. The preparation method of the present invention uses an oxalic acid system as an extraction stock solution, and the raffinate does not need to be neutralized and impurities removed by adding alkali, can be directly reused, and wastewater treatment is simple; the preparation method of the present invention can be used for vanadium pentoxide raw materials with high Fe content and low-purity vanadium pentoxide raw materials including metallurgical vanadium powder and low-purity chemical vanadium powder, which makes the raw material source of the vanadium electrolyte preparation process wide and further reduces the preparation cost.
[0008] Specifically, the present invention provides a method for preparing a vanadium electrolyte, the method comprising the following steps:
[0009] (1) Dissolution reduction: Mix a vanadium raw material containing vanadium pentoxide, oxalic acid and water, heat and stir to dissolve and react, and filter after the reaction is completed to obtain a vanadyl oxalate solution;
[0010] (2) Extraction-strip extraction: using an organic extractant to perform one-stage or multi-stage extraction on the vanadyl oxalate solution obtained in step (1) to obtain a vanadium-loaded organic phase and a raffinate, and then using a sulfuric acid solution to perform one-stage or multi-stage stripping on the vanadium-loaded organic phase to obtain an empty organic phase and a vanadyl sulfate solution;
[0011] (3) Circular deoiling: introducing deoiling resin into the vanadyl sulfate solution obtained in step (2) for cyclic deoiling to obtain an oil-free vanadyl sulfate solution;
[0012] (4) Electrolytic reduction: The oil-free vanadyl sulfate solution obtained in step (3) is passed through the cathode of an electrolytic reduction device for electrolytic reduction to obtain a vanadium electrolyte having an average valence of +3.5.
[0013] In one or more embodiments, in step (1), the content of vanadium pentoxide in the vanadium pentoxide-containing raw material is ≥ 95 wt%.
[0014] In one or more embodiments, in step (1), the molar ratio of vanadium pentoxide to oxalic acid is 1:(3.1-3.5).
[0016] In one or more embodiments, in step (1), 30 to 50 g of vanadium raw material containing vanadium pentoxide is added to each liter of water.
[0017] In one or more embodiments, in step (1), the reaction temperature is 50-60°C.
[0018] In one or more embodiments, in step (1), the reaction time is 40 to 60 minutes.
[0019] In one or more embodiments, in step (2), the solute of the organic extractant is an acidic phosphorus-oxygen type extractant; preferably, the acidic phosphorus-oxygen type extractant is di(2-ethylhexyl) phosphate or 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester.
[0020] In one or more embodiments, in step (2), the solvent of the organic extractant is sulfonated kerosene.
[0021] In one or more embodiments, in step (2), the solute content of the organic extractant is 20 wt% to 25 wt%.
[0022] In one or more embodiments, in step (2), the concentration of sulfate in the sulfuric acid solution is 4 to 5.5 mol / L.
[0023] In one or more embodiments, in step (2), the ratio of the total volume of the organic extractant used to the total volume of the vanadyl oxalate solution is 1:(1.5-2.5).
[0024] In one or more embodiments, in step (2), the single-stage extraction time is 5 to 10 minutes.
[0025] In one or more embodiments, in step (2), the extraction temperature is 10 to 30°C.
[0026] In one or more embodiments, in step (2), the number of extraction stages is 3 to 5.
[0027] In one or more embodiments, in step (2), the ratio of the total volume of the sulfuric acid solution used to the total volume of the vanadium-carrying organic phase is 1:(7-9). In one or more embodiments, in step (2), the single-stage stripping time is 5-10 min.
[0028] In one or more embodiments, in step (2), the stripping temperature is 10 to 30°C.
[0029] In one or more embodiments, in step (2), the number of stripping stages is 3 to 5.
[0030] In one or more embodiments, in step (2), the V2O5 concentration in the raffinate is ≤20 g / L.
[0031] In one or more embodiments, in step (2), the vanadium ion concentration of the vanadyl sulfate solution is ≥ 1.0 mol / L.
[0032] In one or more embodiments, in step (3), the degreasing resin is CN-01 resin or ORZ-05 resin.
[0034] In one or more embodiments, in step (3), the cyclic deoiling time is 40 to 60 minutes.
[0035] In one or more embodiments, in step (4), the electrolytic reduction device is a diaphragm type tank or stack electrolytic cell.
[0036] In one or more embodiments, in step (4), the anode plate of the electrolytic reduction device is a titanium plate coated with iridium and tantalum.
[0037] In one or more embodiments, in step (4), the cathode plate of the electrolytic reduction device is a graphite plate.
[0038] In one or more embodiments, in step (4), the anolyte of the electrolytic reduction device is a 25 wt% to 35 wt% sulfuric acid solution.
[0039] In one or more embodiments, in step (4), the diaphragm of the electrolytic reduction device is a perfluorosulfonic acid proton membrane.
[0040] In one or more embodiments, in step (4), the current density of the electrolytic reduction is 80 to 200 mA / cm 2 .
[0041] In one or more embodiments, the method for preparing a vanadium electrolyte provided by the present invention further comprises: using the raffinate obtained in step (2) for dissolving and reducing the vanadium raw material containing vanadium pentoxide in step (1).
[0042] In one or more embodiments, the method for preparing a vanadium electrolyte provided by the present invention further comprises: reusing the unloaded organic phase obtained in step (2) as an organic extractant in step (2).
[0043] The invention provides a vanadium electrolyte prepared by the method of the invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The present invention provides a process flow chart for preparing vanadium electrolyte according to some embodiments of the present invention.
[0045] Figure 2 This is a relationship diagram between the cycle number and energy efficiency of the all-vanadium redox flow battery assembled with the vanadium electrolyte prepared in Example 1 of the present invention.
[0046] Figure 3 This is a relationship diagram between the cycle number and energy efficiency of the all-vanadium redox flow battery assembled with the vanadium electrolyte prepared in Example 2 of the present invention.
[0047] Figure 4 This is a relationship diagram between the cycle number and energy efficiency of the all-vanadium redox flow battery assembled with the vanadium electrolyte prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0048] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in this document. Unless otherwise specified, all technical and scientific terms used in this document have the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definitions in this specification shall prevail.
[0049] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0050] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0051] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0052] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0053] Herein, when describing embodiments or examples, it should be understood that it is not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope defined herein.
[0054] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0055] The present invention provides a method for preparing a vanadium electrolyte, the method comprising the following steps:
[0056] (1) Dissolution reduction: Mix a vanadium raw material containing vanadium pentoxide, oxalic acid and water, heat and stir to dissolve and react, and filter after the reaction is completed to obtain a vanadyl oxalate solution;
[0057] (2) Extraction-strip extraction: using an organic extractant to perform one-stage or multi-stage extraction on the vanadyl oxalate solution obtained in step (1) to obtain a vanadium-loaded organic phase and a raffinate, and then using a sulfuric acid solution to perform one-stage or multi-stage stripping on the vanadium-loaded organic phase to obtain an empty organic phase and a vanadyl sulfate solution;
[0058] (3) Circular deoiling: introducing deoiling resin into the vanadyl sulfate solution obtained in step (2) for cyclic deoiling to obtain an oil-free vanadyl sulfate solution;
[0059] (4) Electrolytic reduction: The oil-free vanadyl sulfate solution obtained in step (3) is passed through the cathode of an electrolytic reduction device for electrolytic reduction to obtain a vanadium electrolyte having an average valence of +3.5.
[0060] In step (1) of the present invention, oxalic acid can dissolve the vanadium raw material containing vanadium pentoxide, and can reduce the pentavalent vanadium in the vanadium pentoxide to tetravalent vanadium. Oxalate can also combine with metal ions to obtain precipitation. The specific mechanism is shown below.
[0061] V2O5+3H2C2O4=2VOC2O4+2CO2↑+3H2O
[0062] M n+ +C2O4 2- →M(C2O4) n / 2 ↓
[0063] In the formula, M is Ca, Cu, Ba, Ag, Fe, Ni, Zn, Mn, Al, Cr, Pb, Co, etc.
[0064] After the reaction of oxalic acid and vanadium pentoxide is completed, filtration is performed to obtain a vanadium oxalate solution from which heavy metal precipitation is removed.
[0065] In step (1), the content of vanadium pentoxide in the vanadium pentoxide-containing vanadium raw material may be ≥ 95 wt%, for example, 95 wt%, 96 wt%, 97 wt%, 98 wt%, 99 wt%.
[0066] In step (1), the vanadium raw material containing vanadium pentoxide can be a powdered metallurgical grade vanadium pentoxide with a high impurity content obtained by calcining low-purity ammonium polyvanadate or ammonium metavanadate, or by crushing and grinding vanadium flakes.
[0067] In step (1), the molar ratio of vanadium pentoxide to oxalic acid may be 1:(3.1-3.5), for example, 1:3.1, 1:3.2, 1:3.3, 1:3.4, 1:3.5.
[0068] In step (1), 30 to 50 g of vanadium raw material containing vanadium pentoxide can be added to each liter of water.
[0069] In step (1), the reaction temperature can be 50-60°C, for example, 50°C, 52°C, 54°C, 56°C, 58°C, 60°C.
[0070] In step (1), the reaction time can be 40 to 60 min, for example, 40 min, 45 min, 50 min, 55 min, or 60 min.
[0071] In step (2), the organic extractant contains a solute and a solvent. The solute of the organic extractant can be an acidic phosphorus-oxygen type extractant. Preferably, the acidic phosphorus-oxygen type extractant is di(2-ethylhexyl) phosphate 242767
[0072] (P204) or 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester (P507). In the present invention, the acidic phosphorus oxygen extractant is a compound in which one or two hydroxyl groups in phosphoric acid (H3PO4) are replaced by alkyl or alkoxy groups. The solute content of the organic extractant can be 20wt% to 25wt%, such as 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%. The solvent of the organic extractant can be sulfonated kerosene.
[0073] In step (2), the ratio of the total volume of the organic extractant used to the total volume of the vanadyl oxalate solution is 1:(1.5-2.5), for example, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2, 1:2.1, 1:2.2, 1:2.3, 1:2.4.
[0074] In step (2), the single-stage extraction time can be 5 to 10 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min.
[0075] In step (2), the extraction temperature may be 10-30°C, for example 10°C, 15°C, 20°C, 25°C, 30°C.
[0076] In the present invention, when the extraction is a primary extraction, the vanadium oxalate solution obtained in step (1) is extracted once using an organic extractant. After standing for liquid separation, the organic phase obtained by extraction (referred to as the extracted organic phase) is the vanadium-loaded organic phase, and the inorganic phase obtained by extraction (referred to as the extracted inorganic phase) is the raffinate.
[0077] In some embodiments, when the extraction is a multi-stage extraction and the number of extraction stages is N (N≥2), preferably, the organic extractant is divided into N parts, and the first part of the organic extractant is first used to perform the first-stage extraction on the vanadium oxalate solution obtained in step (1), and after standing and separating the liquids, a first-stage extraction organic phase and a first-stage extraction inorganic phase are obtained; then the Nth part of the organic extractant is used to perform the Nth-stage extraction on the N-1th stage extraction inorganic phase, and after standing and separating the liquids, an Nth-stage extraction organic phase and an Nth-stage extraction inorganic phase are obtained; the first to Nth stage extraction organic phases are combined to obtain a vanadium-carrying organic phase, and the Nth-stage extraction inorganic phase is the raffinate. In these embodiments, the ratio of the total volume of each part of the organic extractant to the volume of the vanadium oxalate solution is preferably 1:(1.5-2.5), and the volumes of each part of the organic extractant can be the same or different, preferably the same.
[0078] In step (2), the number of extraction stages is preferably 3-5, for example 4.
[0079] In step (2), the V2O5 concentration in the raffinate may be ≤20 g / L, for example, 0.01 g / L, 0.1 g / L, 0.2 g / L, 0.5 g / L, 1 g / L, 2 g / L, 4 g / L, 6 g / L, 8 g / L, 10 g / L, 12 g / L, 14 g / L, 16 g / L, 18 g / L, 20 g / L, preferably ≤1 g / L, more preferably ≤0.1 g / L.
[0080] In step (2), the concentration of sulfate in the sulfuric acid solution may be 4 to 5.5 mol / L, for example 4 mol / L,
[0082] 4.3mol / L, 4.6mol / L, 4.9mol / L, 5.2mol / L, 5.5mol / L.
[0083] In step (2), the ratio of the total volume of the sulfuric acid solution used to the total volume of the vanadium-carrying organic phase can be 1:(7-9), for example, 1:7.2, 1:7.4, 1:7.6, 1:7.8, 1:8, 1:8.2, 1:8.4, 1:8.6, 1:8.8.
[0084] In step (2), the single-stage stripping time can be 5 to 10 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min.
[0085] In step (2), the stripping temperature can be 10-30°C, for example, 10°C, 15°C, 20°C, 25°C, 30°C.
[0086] In the present invention, when the stripping is a primary stripping, a sulfuric acid solution is used to strip the vanadium-loaded organic phase once. After standing and separating the liquids, the organic phase obtained by stripping (referred to as the stripping organic phase) is the empty organic phase, and the inorganic phase obtained by stripping (referred to as the stripping inorganic phase) is the vanadium sulfate solution.
[0087] In some embodiments, when the stripping is multi-stage stripping and the stripping stage number is N (N≥2), preferably, the vanadium-carrying organic phase is divided into N parts, and the first part of the vanadium-carrying organic phase is first stripped with a sulfuric acid solution, and after standing and separating, a first stripping organic phase and a first stripping inorganic phase are obtained; then the Nth part of the vanadium-carrying organic phase is stripped with an N-1th stripping inorganic phase, and after standing and separating, an Nth stripping organic phase and an Nth stripping inorganic phase are obtained; the Nth stripping inorganic phase is a vanadium oxysulfate solution, and the first to Nth stripping organic phases are empty organic phases. In these embodiments, the ratio of the volume of the sulfuric acid solution to the total volume of each part of the vanadium-carrying organic phase is preferably 1:(7-9), and the volumes of each part of the vanadium-carrying organic phase may be the same or different, preferably the same.
[0088] In step (2), the number of stripping stages is preferably 3-5, for example 4.
[0089] In step (2), the vanadium ion concentration of the vanadyl sulfate solution is ≥1.0 mol / L, preferably 1.0 to 2.6 mol / L, for example 1.2 mol / L, 1.5 mol / L, 1.7 mol / L, 2 mol / L, 2.2 mol / L, 2.5 mol / L.
[0090] It is understood that in step (2), the empty organic phase may contain a small amount of vanadium, because the empty organic phase can be reused as an organic extractant.
[0091] In step (3), the degreasing resin may be CN-01 resin or ORZ-05 resin.
[0092] In step (3), the cyclic degreasing time can be 40 to 60 minutes, for example, 40 minutes, 45 minutes, 50 minutes, 55 minutes, or 60 minutes.
[0093] In step (4), the electrolytic reduction device can be a diaphragm type tank or stack type electrolytic cell. In some embodiments, the electrolytic reduction device is a diaphragm type tank or stack type electrolytic cell made of corrosion-resistant polymer material.
[0094] In step (4), the anode plate of the electrolytic reduction device can be a titanium plate coated with iridium and tantalum.
[0095] In step (4), the cathode plate of the electrolytic reduction device may be a graphite plate.
[0096] In step (4), the anolyte of the electrolytic reduction device can be a 25wt% to 35wt% sulfuric acid solution, for example, 25wt%, 27wt%, 29wt%, 31wt%, 33wt%, 35wt%.
[0097] In step (4), the diaphragm of the electrolytic reduction device can be a perfluorosulfonic acid proton membrane.
[0098] In step (4), the current density of electrolytic reduction can be 80 to 200 mA / cm 2 , for example 80mA / cm 2 , 100mA / cm 2 , 120mA / cm 2 , 140mA / cm 2 , 160mA / cm 2 , 180mA / cm 2 , 200mA / cm 2 .
[0099] In some embodiments, the method for preparing a vanadium electrolyte of the present invention further comprises: using the raffinate obtained in step (2) for dissolving and reducing the vanadium raw material containing vanadium pentoxide in step (1).
[0100] In some embodiments, the method for preparing a vanadium electrolyte of the present invention further comprises: reusing the unloaded organic phase obtained in step (2) as an organic extractant in step (2).
[0101] The present invention also includes a vanadium electrolyte prepared by the preparation method of the present invention. The vanadium ion concentration of the vanadium electrolyte is preferably 1.6-2 mol / L.
[0102] Compared with the prior art, the present invention has the following beneficial effects:
[0103] 1) The raw material selection and process route design of the preparation method of the present invention do not introduce ammonium salt, thus avoiding the wastewater deammoniation treatment of the traditional process, and the wastewater treatment cost is low;
[0104] 2) The preparation method of the present invention uses an oxalic acid system to replace the strong acid system of the prior art in the extraction stock solution. The heavy metal oxalate produced during the dissolution and reduction directly leaves the system in the form of precipitation, which is beneficial to the recycling of the raffinate. At the same time, the separation of elements such as Fe and Ca is beneficial to improving the enrichment effect of the extractant on vanadium.
[0105] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.
[0106] The low-purity vanadium pentoxide in Example 1 of the present invention is obtained by extracting vanadium from waste catalysts of a factory in Sichuan.
[0108] The ammonium polyvanadate product in Example 2 of the present invention is obtained from vanadium extraction from stone coal in a factory in Gansu.
[0109] The metallurgical grade vanadium pentoxide in Example 3 of the present invention is obtained by extracting vanadium from vanadium slag in a factory in Hebei.
[0110] The oxalic acid dihydrate in Examples 1-3 of the present invention was purchased from Shanghai Titan Technology Co., Ltd. with a brand number of CAS6153-56-6.
[0111] In Examples 1-3 of the present invention, the electrolytic reduction device is a diaphragm-type stack single electrolytic cell, the anode plate of the electrolytic reduction device is a titanium plate coated with an iridium-tantalum coating, the cathode plate of the electrolytic reduction device is a graphite plate, the anode liquid of the electrolytic reduction device is a 30wt% sulfuric acid solution, and the diaphragm of the electrolytic reduction device is a perfluorosulfonic acid proton membrane.
[0112] Example 1
[0113] This embodiment refers to Figure 1 The vanadium electrolyte is prepared by the steps of:
[0114] Step 1: Weigh 70g of low-purity vanadium pentoxide (wherein the vanadium pentoxide content is 98.08wt%, and the impurity contents are respectively Al 0.03wt%, As 0.14wt%, Cr 0.02wt%, Ca 0.07wt%, Fe0.01wt%, Mg 0.08wt%, Mo1.13wt%, K 0.20wt%, Na 0.25wt%) and 150g of dihydrated oxalic acid, add them to 2L of water, heat to 50°C under stirring conditions for reaction for 60min, filter after the reaction is completed, and obtain a vanadium oxalate solution with heavy metal precipitation removed;
[0115] Step 2: Using P204 and sulfonated kerosene in a mass ratio of 1:4 as the extractant and 4 mol / L sulfuric acid solution as the stripping agent, perform three-stage extraction and three-stage stripping at 20°C:
[0116] The ratio of the total volume of the extractant used in the three-stage extraction to the volume of the vanadyl oxalate solution was 1:2, and the extractant was divided into three parts;
[0117] The vanadyl oxalate solution prepared in step 1 is subjected to first-stage extraction using the first extractant for 10 minutes, and the solution is allowed to stand for separation to obtain a first-stage extraction organic phase and a first-stage extraction inorganic phase;
[0118] Use the second extractant to perform a second extraction on the first-stage extracted inorganic phase, the extraction time is 10 minutes, and the liquid is allowed to stand to separate, to obtain a second-stage extracted organic phase and a second-stage extracted inorganic phase;
[0119] The third extraction solvent is used to perform a third extraction on the second extraction inorganic phase, the extraction time is 10 minutes, and the liquid is allowed to stand to separate, thereby obtaining a third extraction organic phase and a third extraction inorganic phase;
[0120] The third stage extraction inorganic phase is the raffinate, the V2O5 concentration in the raffinate is 0.04 g / L, and the first to third stage extraction organic phases are combined to obtain the vanadium-loaded organic phase;
[0121] The volume ratio of the stripping agent used in the third-stage stripping to the volume of the vanadium-carrying organic phase is 1:8.
[0122] The vanadium organic phase was divided into three equal parts;
[0123] The first vanadium-loaded organic phase is subjected to first-stage stripping using a stripping agent for 10 minutes, and the phases are allowed to stand for separation to obtain a first-stage stripping organic phase and a first-stage stripping inorganic phase;
[0124] The first-stage stripping inorganic phase is used to perform the second-stage stripping of the second vanadium-loaded organic phase, the stripping time is 10 minutes, and the liquid is allowed to stand for separation to obtain the second-stage stripping organic phase and the second-stage stripping inorganic phase;
[0125] The third vanadium-loaded organic phase is subjected to third-stage stripping using the second-stage stripping inorganic phase, the stripping time is 10 minutes, and the phases are allowed to stand for separation to obtain a third-stage stripping organic phase and a third-stage stripping inorganic phase;
[0126] The organic phases of the first to third stage stripping are empty organic phases, and the inorganic phase of the third stage stripping is a vanadyl sulfate solution, in which the vanadium ion concentration is 1.75 mol / L;
[0127] Step 3: Add CN-01 resin (purchased from Jiangsu Saipuri Separation Technology Co., Ltd.) to the vanadyl sulfate solution obtained in step 2 and circulate to remove oil for 40 minutes to obtain an oil-free vanadyl sulfate solution;
[0128] Step 4: Pass the oil-free vanadyl sulfate solution obtained in step 3 into the cathode of the electrolytic reduction device at 80 mA / cm 2 Electrolytic reduction is carried out to obtain a vanadium electrolyte with an average valence of +3.5.
[0129] Example 2
[0130] This embodiment refers to Figure 1 The vanadium electrolyte is prepared by the steps of:
[0131] Step 1: calcining the ammonium polyvanadate product at 500° C. for 3 h to obtain metallurgical grade vanadium pentoxide (wherein the vanadium pentoxide content is 98.52 wt%, and the impurity contents are respectively Al 0.13 wt%, As 0.003 wt%, Cr 0.01 wt%, Ca 0.05 wt%, Fe 0.22 wt%, Mg 0.02 wt%, Mo 0.04 wt%, K 0.08 wt%, and Na 1.01 wt%), weighing 80 g of metallurgical grade vanadium pentoxide and 180 g of oxalic acid dihydrate, adding them to 2 L of water, heating to 55° C. under stirring conditions for reaction for 50 min, filtering after the reaction is completed, and obtaining a vanadium oxalate solution with heavy metal precipitation removed;
[0132] Step 2: Using P204 and sulfonated kerosene in a mass ratio of 1:3 as the extractant and 4.5 mol / L sulfuric acid solution as the stripping agent, four-stage extraction and four-stage stripping were performed at 20°C:
[0133] The ratio of the total volume of the extractant used in the four-stage extraction to the volume of the vanadyl oxalate solution is 1:2, and the extractant is divided into four parts;
[0134] The first extraction agent is used to perform the first extraction on the vanadyl oxalate solution obtained in step 1, the extraction time is 7 minutes, and the solution is allowed to stand for separation to obtain a first extraction organic phase and a first extraction inorganic phase;
[0135] The inorganic phase of the first extraction was subjected to a second extraction using the second extractant, and the extraction time was 242767
[0136] 7min, stand and separate the liquids to obtain the second-stage extraction organic phase and the second-stage extraction inorganic phase;
[0137] The second-stage extracted inorganic phase is subjected to a third-stage extraction using a third portion of an extractant, the extraction time is 7 minutes, and the liquid is allowed to stand for separation to obtain a third-stage extracted organic phase and a third-stage extracted inorganic phase;
[0138] The third-stage extraction inorganic phase is subjected to a fourth-stage extraction using a fourth portion of an extractant, the extraction time is 7 minutes, and the liquid is allowed to stand for separation to obtain a fourth-stage extraction organic phase and a fourth-stage extraction inorganic phase;
[0139] The fourth stage extraction inorganic phase is the raffinate, the V2O5 concentration in the raffinate is 0.03 g / L, and the first to fourth stage extraction organic phases are combined to obtain the vanadium-loaded organic phase;
[0140] The ratio of the volume of the stripping agent used in the four-stage stripping to the volume of the vanadium-carrying organic phase is 1:8, and the vanadium-carrying organic phase is divided into four equal parts;
[0141] The first vanadium-loaded organic phase is subjected to first-stage stripping using a stripping agent for 7 minutes, and the phases are allowed to stand for separation to obtain a first-stage stripping organic phase and a first-stage stripping inorganic phase;
[0142] The first-stage stripping inorganic phase is used to perform the second-stage stripping of the second vanadium-loaded organic phase, the stripping time is 7 minutes, and the liquid is allowed to stand to separate, to obtain the second-stage stripping organic phase and the second-stage stripping inorganic phase;
[0143] The third vanadium-loaded organic phase is subjected to third-stage stripping using the second-stage stripping inorganic phase, the stripping time is 7 minutes, and the liquid is allowed to stand for separation to obtain a third-stage stripping organic phase and a third-stage stripping inorganic phase;
[0144] The fourth stage stripping of the vanadium-loaded organic phase was performed using the third stage stripping inorganic phase, the stripping time was 7 minutes, and the liquid was allowed to stand for separation to obtain a fourth stage stripping organic phase and a fourth stage stripping inorganic phase;
[0145] The organic phases of the first to fourth stage stripping are empty organic phases, and the inorganic phase of the fourth stage stripping is a vanadium oxysulfate solution, in which the vanadium ion concentration is 2.03 mol / L;
[0146] Step 3: passing ORZ-05 resin (purchased from Jiangsu Saipuri Separation Technology Co., Ltd.) into the vanadyl sulfate solution obtained in step 2 for 50 minutes of circulation to remove oil, thereby obtaining an oil-free vanadyl sulfate solution;
[0147] Step 4: Pass the oil-free vanadyl sulfate solution obtained in step 3 into the cathode of the electrolytic reduction device at 150 mA / cm 2 Electrolytic reduction is carried out to obtain a vanadium electrolyte with an average valence of +3.5.
[0148] Example 3
[0149] This embodiment refers to Figure 1 The vanadium electrolyte is prepared by the steps of:
[0150] Step 1: Weigh 100g of metallurgical grade vanadium pentoxide (wherein the vanadium pentoxide content is 97.94wt%, and the impurity contents are Al 0.02wt%, As 0.002wt%, Cr 0.05wt%, Ca0.01wt%, Fe 0.05wt%, Mg0.008wt%, Mo 0.06wt%, K 0.20wt%, Na 0.25wt%)
[0152] and 237 g of oxalic acid dihydrate, added to 2 L of water, heated to 60 ° C with stirring for 40 min, and filtered after the reaction was completed to obtain a vanadyl oxalate solution with heavy metal precipitation removed;
[0153] Step 2: Using P507 and sulfonated kerosene in a mass ratio of 1:3 as the extractant and 5 mol / L sulfuric acid solution as the stripping agent, five-stage extraction and five-stage stripping were performed at 30°C:
[0154] The ratio of the total volume of the extractant used in the five-stage extraction to the volume of the vanadyl oxalate solution is 1:2, and the extractant is divided into five equal parts;
[0155] Using the first extractant to perform a first-stage extraction on the vanadyl oxalate solution obtained in step 1, the extraction time is 5 minutes, and the solution is allowed to stand for separation to obtain a first-stage extraction organic phase and a first-stage extraction inorganic phase;
[0156] Use the second extractant to perform a second extraction on the first-stage extracted inorganic phase, the extraction time is 5 minutes, and the liquid is allowed to stand to separate, to obtain a second-stage extracted organic phase and a second-stage extracted inorganic phase;
[0157] The third extraction solvent is used to perform a third extraction on the second extraction inorganic phase, the extraction time is 5 minutes, and the liquid is allowed to stand to separate, thereby obtaining a third extraction organic phase and a third extraction inorganic phase;
[0158] The third-stage extraction inorganic phase is subjected to a fourth-stage extraction using a fourth portion of an extractant, the extraction time is 5 minutes, and the liquid is allowed to stand for separation to obtain a fourth-stage extraction organic phase and a fourth-stage extraction inorganic phase;
[0159] The fifth extraction solvent is used to perform a fifth extraction on the fourth extraction inorganic phase, the extraction time is 5 minutes, and the liquid is allowed to stand to separate, thereby obtaining a fifth extraction organic phase and a fifth extraction inorganic phase;
[0160] The fifth stage extraction inorganic phase is the raffinate, the V2O5 concentration in the raffinate is 0.07 g / L, and the first to fifth stage extraction organic phases are combined to obtain the vanadium-loaded organic phase;
[0161] The ratio of the volume of the stripping agent used in the five-stage stripping to the volume of the vanadium-carrying organic phase is 1:8, and the vanadium-carrying organic phase is divided into five equal parts;
[0162] The first vanadium-loaded organic phase is subjected to first-stage stripping using a stripping agent for 5 minutes, and the phases are allowed to stand for separation to obtain a first-stage stripping organic phase and a first-stage stripping inorganic phase;
[0163] The first-stage stripping inorganic phase is used to perform the second-stage stripping of the second vanadium-loaded organic phase, the stripping time is 5 minutes, and the liquid is allowed to stand for separation to obtain the second-stage stripping organic phase and the second-stage stripping inorganic phase;
[0164] The third stage stripping of the vanadium-loaded organic phase is performed using the second stage stripping inorganic phase, the stripping time is 5 minutes, and the liquid is allowed to stand for separation to obtain a third stage stripping organic phase and a third stage stripping inorganic phase;
[0165] The fourth stage stripping of the vanadium-loaded organic phase was performed using the third stage stripping inorganic phase, the stripping time was 5 minutes, and the liquid was allowed to stand for separation to obtain a fourth stage stripping organic phase and a fourth stage stripping inorganic phase;
[0166] The fifth step of stripping the fifth vanadium-loaded organic phase is performed with the fourth step stripping inorganic phase, the stripping time is 5 minutes, and the phases are allowed to stand for separation to obtain a fifth step stripping organic phase and a fifth step stripping inorganic phase;
[0167] The organic phases of the first to fifth stage stripping are empty organic phases, and the inorganic phase of the fifth stage stripping is a vanadyl sulfate solution, in which the vanadium ion concentration is 2.52 mol / L;
[0168] Step 3: passing ORZ-05 resin (purchased from Jiangsu Saipuri Separation Technology Co., Ltd.) into the vanadyl sulfate solution obtained in step 2 for 60 minutes of circulation to remove oil, thereby obtaining an oil-free vanadyl sulfate solution;
[0169] Step 4: Pass the oil-free vanadyl sulfate solution obtained in step 3 into the cathode of the electrolytic reduction device at 200 mA / cm 2 Electrolytic reduction is carried out to obtain a vanadium electrolyte with an average valence of +3.5.
[0170] Test Case
[0171] Impurity element content test: The impurity element content of the vanadium electrolyte prepared in Examples 1-3 was analyzed using an inductively coupled plasma spectrometer. The test results are shown in Table 1.
[0172] Table 1: Impurity element content of vanadium electrolyte prepared in Examples 1-3
[0173]
[0174] Note: ND in the table means not detected
[0175] Assemble all-vanadium flow battery: adjust the vanadium ion concentration of the vanadium electrolyte prepared in Example 1-3 to 1.7 mol / L and the sulfate concentration to 4.3 mol / L by adding sulfuric acid and water to obtain a standard concentration vanadium electrolyte, and inject 100 mL of the standard concentration vanadium electrolyte into the all-vanadium flow battery, wherein the effective area of the positive electrode and the negative electrode is 48 cm 2 , the membrane is a perfluorosulfonic acid proton membrane.
[0176] Energy efficiency test: at 150mA / cm 2 The battery's operating conditions and energy efficiency were tested during 50 cycles of constant current charge and discharge at a current density of 1.34 W. Figure 2-Figure 4The energy efficiency test results of the all-vanadium redox flow battery assembled with the vanadium electrolyte prepared in Examples 1-3 are shown in Table 2. The energy efficiency test results of the all-vanadium redox flow battery assembled with the vanadium electrolyte prepared in Example 1 are shown in Table 2. Figure 2 As shown, the energy efficiency test results of the all-vanadium redox flow battery assembled with the vanadium electrolyte prepared in Example 2 are as follows Figure 3 As shown, the energy efficiency test results of the all-vanadium redox flow battery assembled with the vanadium electrolyte prepared in Example 3 are as follows Figure 4 shown.
[0177] Table 2: Energy efficiency of all-vanadium redox flow batteries assembled with vanadium electrolytes prepared in Examples 1-3
[0178] Example 1 Example 2 Example 3 Energy efficiency of the 10th cycle / % 83.42 84.17 84.63 Energy efficiency at the 20th cycle / % 82.84 81.74 83.37 Energy efficiency at the 30th cycle / % 82.67 83.13 82.92 Energy efficiency at the 40th cycle / % 82.51 82.86 82.81 Energy efficiency at the 50th cycle / % 82.29 82.49 82.47
[0179] It can be seen from Table 1 that the vanadium electrolytes prepared in Examples 1-3 meet the standards for first-class vanadium electrolytes in GB / T_37204-2018_Electrolyte for All-Vanadium Liquid Flow Batteries.
[0180] From Table 2 and Figure 2 It can be seen that the energy efficiency of the all-vanadium redox flow battery assembled with the vanadium electrolyte prepared in Example 1 is normal after 50 cycles, and the average energy efficiency of 50 cycles is 83.0%. Figure 3 It can be seen that the energy efficiency of the all-vanadium redox flow battery assembled with the vanadium electrolyte prepared in Example 2 is normal after 50 cycles, and the average energy efficiency of 50 cycles is 83.3%. Figure 4 It can be seen that the energy efficiency of the all-vanadium redox flow battery assembled with the vanadium electrolyte prepared in Example 2 is normal after 50 cycles, and the energy efficiency of the 50 cycles is 83.4% on average.
Claims
1. A method for preparing a vanadium electrolyte, characterized in that: The method comprises the following steps: (1) Dissolution reduction: Mix a vanadium raw material containing vanadium pentoxide, oxalic acid and water, heat and stir to dissolve and react, and filter after the reaction is completed to obtain a vanadyl oxalate solution; (2) Extraction-strip extraction: using an organic extractant to perform one-stage or multi-stage extraction on the vanadyl oxalate solution obtained in step (1) to obtain a vanadium-loaded organic phase and a raffinate, and then using a sulfuric acid solution to perform one-stage or multi-stage stripping on the vanadium-loaded organic phase to obtain an empty organic phase and a vanadyl sulfate solution; (3) Circular deoiling: introducing deoiling resin into the vanadyl sulfate solution obtained in step (2) for cyclic deoiling to obtain an oil-free vanadyl sulfate solution; (4) Electrolytic reduction: The oil-free vanadyl sulfate solution obtained in step (3) is passed through the cathode of an electrolytic reduction device for electrolytic reduction to obtain a vanadium electrolyte having an average valence of +3.
5.
2. The method according to claim 1, characterized in that The method includes one or more of the following features: In step (1), the content of vanadium pentoxide in the vanadium pentoxide-containing raw material is ≥ 95wt%; In step (1), the molar ratio of vanadium pentoxide to oxalic acid is 1:(3.1-3.5); In step (1), 30 to 50 g of vanadium raw material containing vanadium pentoxide is added to each liter of water; In step (1), the reaction temperature is 50-60°C; In step (1), the reaction time is 40 to 60 minutes.
3. The method according to claim 1, characterized in that The method includes one or more of the following features: In step (2), the solute of the organic extractant is an acidic phosphorus-oxygen type extractant; preferably, the acidic phosphorus-oxygen type extractant is di(2-ethylhexyl) phosphate or 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester; In step (2), the solvent of the organic extractant is sulfonated kerosene; In step (2), the solute content of the organic extractant is 20 wt% to 25 wt%; In step (2), the concentration of sulfate in the sulfuric acid solution is 4 to 5.5 mol / L.
4. The method according to claim 1, characterized in that The method comprises one of the following or Multiple features: In step (2), the ratio of the total volume of the organic extractant used to the total volume of the vanadyl oxalate solution is 1:(1.5-2.5); In step (2), the single-stage extraction time is 5 to 10 minutes; In step (2), the extraction temperature is 10 to 30° C.; In step (2), the number of extraction stages is 3 to 5; In step (2), the ratio of the total volume of the sulfuric acid solution used to the total volume of the vanadium-carrying organic phase is 1:(7-9); In step (2), the single-stage stripping time is 5 to 10 minutes; In step (2), the stripping temperature is 10 to 30° C.; In step (2), the number of stripping stages is 3 to 5.
5. The method according to claim 1, characterized in that In step (2), the concentration of V2O5 in the raffinate is ≤20 g / L; and / or In step (2), the vanadium ion concentration of the vanadyl sulfate solution is ≥1.0 mol / L.
6. The method according to claim 1, characterized in that In step (3), the degreasing resin is CN-01 resin or ORZ-05 resin; and / or In step (3), the cyclic degreasing time is 40 to 60 minutes.
7. The method according to claim 1, characterized in that The method includes one or more of the following features: In step (4), the electrolytic reduction device is a diaphragm type tank or stack electrolytic cell; In step (4), the anode plate of the electrolytic reduction device is a titanium plate coated with iridium and tantalum; In step (4), the cathode plate of the electrolytic reduction device is a graphite plate; In step (4), the anolyte of the electrolytic reduction device is a 25wt% to 35wt% sulfuric acid solution; In step (4), the diaphragm of the electrolytic reduction device is a perfluorosulfonic acid proton membrane; In step (4), the current density of the electrolytic reduction is 80 to 200 mA / cm 2 .
8. The method according to claim 1, characterized in that The method further comprises: using the raffinate obtained in step (2) to dissolve and reduce the vanadium raw material containing vanadium pentoxide in step (1).
9. The method according to claim 1, characterized in that The method further comprises: reusing the unloaded organic phase obtained in step (2) as the organic extractant in step (2).
10. A vanadium electrolyte, characterized in that: The vanadium electrolyte is prepared by the method according to any one of claims 1 to 9.
Citation Information
Cited By
Method for preparing vanadium electrolyte by sodium polyvanadate extraction method