Preparation method of gradient pore structure carbon nanofiber electrode material and application of gradient pore structure carbon nanofiber electrode material in flow battery
By regulating the concentration of spinning precursor solution, the carbon nanofiber electrode material with gradient pore structure is solved, and the contradiction between the electrochemical reaction activity and mass transfer performance of the liquid flow battery electrode material is achieved, and the battery performance is improved, especially in Significant improvements in electrolyte utilization and energy efficiency.
Patent Information
- Application Number
- CN202411067661.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
There are contradictions in existing flow battery electrode materials in terms of electrochemical reactivity, conductivity and mass transfer properties, and it is difficult to take into account both electrochemical activation polarization, ohmic polarization and concentration difference polarization, which affects the overall performance of the battery.
By regulating the concentration of spinning precursor solution, a carbon nanofiber electrode material with gradient pore structure is designed to distribute porosity, conductivity and hydrophilicity longitudinally, thereby coordinating different polarization types and degrees during battery operation and improving battery performance.
It effectively improves the utilization rate and energy efficiency of the battery electrolyte, reduces the polarization overpotential, and improves the charging and discharging efficiency and cycle stability of the battery.
Smart Images

Figure HDA0004979819130000011 
Figure HDA0004979819130000012 
Figure HDA0004979819130000021
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery materials and energy storage, and in particular relates to a method for preparing a gradient pore structure carbon nanofiber electrode material and an application thereof in a liquid flow battery. Background Art
[0002] At the forefront of energy technology, efficiently integrating and utilizing clean renewable energy and reducing dependence on fossil fuels such as oil have become core strategies for ensuring energy security, improving the ecological environment, and promoting green and sustainable development. With the rapid advancement of renewable energy technology, large-scale energy storage technology that matches it has gradually become a research hotspot. Among many energy storage technologies, redox flow batteries stand out for their good industrialization potential, scalability, ultra-long cycle life, excellent safety, rapid response capabilities, and huge energy storage capacity, becoming a leader in the field of large-scale long-term energy storage.
[0003] Electrodes are the key places where electrochemical reactions of vanadium batteries occur, and their performance can directly affect the overall performance of the battery. At present, the electrode materials widely used in the market are mainly based on polyacrylonitrile-based carbon fibers. Although this material has the advantages of low cost, high conductivity and good chemical stability, it has contradictions and problems in terms of electrochemical reaction activity, conductivity and mass transfer performance.
[0004] To address this difficulty, the present invention adjusts the concentration of the spinning precursor solution and performs gradient design on the diameter and stacking density of the formed carbon fibers, so that the two sides of the electrode have different properties, and presents a gradient distribution of porosity, conductivity and hydrophilicity in the longitudinal direction. In this way, electrochemical activation polarization, ohmic polarization and concentration polarization are taken into account simultaneously during battery operation, effectively improving the battery electrolyte utilization and energy efficiency, and providing a simple way to build high-performance liquid flow batteries. Summary of the invention
[0005] The purpose of the present invention is to provide a gradient pore structure carbon nanofiber material and apply it to liquid flow battery electrode materials to coordinate the changing polarization type and degree during the battery charging and discharging process, thereby effectively improving the battery performance.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a gradient pore structure carbon nanofiber electrode material comprises the following steps:
[0008] 1) mixing polyacrylonitrile and N,N,-dimethylformamide at different mass ratios to obtain a series of electrospinning precursor solutions of polyacrylonitrile with gradient mass percentage concentrations;
[0009] 2) sucking the electrospinning precursor solutions prepared in step 1) into the electrospinning syringe in equal volumes according to the mass percentage concentration of polyacrylonitrile from high to low, and continuously electrospinning each electrospinning precursor solution using electrospinning technology to obtain the original nanofiber material;
[0010] 3) The original nanofiber material obtained in step 2) is flattened with a corundum plate, placed in a tube furnace for pre-oxidation treatment and carbonization treatment, and then cooled to room temperature to obtain a gradient pore structure carbon nanofiber electrode material.
[0011] Furthermore, in the above preparation method, in step 1), the molecular weight of the polyacrylonitrile is 90,000 to 150,000.
[0012] Furthermore, in the above preparation method, in step 1), the mixing conditions are: magnetic stirring at 80° C. for 6 hours.
[0013] Furthermore, in the above preparation method, in step 1), in the series of electrospinning precursor solutions of polyacrylonitrile with gradient mass percentage concentrations, the mass percentage concentration of polyacrylonitrile is 8% to 20%, and the concentration difference between adjacent mass percentage concentrations of polyacrylonitrile is 3% to 5%.
[0014] Furthermore, in the above-mentioned preparation method, in step 2), the process conditions of the electrospinning technology are as follows: the stainless steel nozzle model is G15~G22; the collector is a stainless steel roller, and the roller speed is 50~150r / min; the voltage between the nozzle and the roller is 18~22kV; the distance between the nozzle and the roller is 10~15cm; the spinning temperature is 25℃~30℃; the spinning humidity is 30%~50%RH; the push speed is 10~50μL / min; 8mL~20mL of each mass percentage concentration of polyacrylonitrile solution is spun.
[0015] Furthermore, in the above preparation method, in step 3), the conditions for the pre-oxidation treatment are: in an air atmosphere, heating to 180°C at a heating rate of 2°C / min, keeping warm for 10 minutes, then heating to 290°C at a heating rate of 1°C / min, and keeping warm for 60 minutes.
[0016] Furthermore, in the above preparation method, in step 3), the conditions of the carbonization treatment are: in a nitrogen or argon atmosphere, a heating rate of 5°C / min, and keeping at 1000°C for 120min.
[0017] Application of the gradient pore structure carbon nanofiber electrode material obtained by any of the preparation methods described above in liquid flow batteries.
[0018] Furthermore, in the above application, when assembling the liquid flow battery, the side of the gradient pore structure carbon nanofiber electrode material with a small fiber diameter and a large packing density is in contact with the diaphragm as an activation enhancement zone, and the side with a large fiber diameter and a small packing density is in contact with the current collector as a mass transfer enhancement zone.
[0019] Furthermore, in the above application, the flow battery includes an all-vanadium flow battery, a zinc-bromine flow battery, an iron-chromium flow battery and an organic flow battery.
[0020] The advantages and beneficial effects of the present invention are:
[0021] 1. The present invention utilizes a simple and controllable electrospinning technology. By simply changing the PAN concentration in the precursor solution, carbon nanofibers of different diameters and a three-dimensional network structure with similar porosity and pore size formed by overlapping each other can be obtained. Moreover, as the concentration of the PAN solution increases, the diameter of the carbon nanofibers gradually increases.
[0022] 2. By continuously electrospinning in descending order according to the PAN concentration, an integrated carbon nanofiber porous material with a longitudinal gradient distribution of fiber diameter and pore structure can be obtained. The preparation method is universal and easy to control.
[0023] 3. The present invention applies the gradient pore structure carbon nanofiber material to the positive and negative electrode materials of the liquid flow battery. According to the different structural properties of the two sides of the electrode material, the side with a small fiber diameter and a large stacking density is in contact with the diaphragm as an activation enhancement zone; the side with a large fiber diameter and a small stacking density is in contact with the current collector as a mass transfer enhancement zone. This can simultaneously take into account the activation polarization, ohmic polarization and concentration polarization of the battery during the charge and discharge process, thereby effectively reducing the polarization overpotential of the battery and improving the battery efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 These are scanning electron microscope photographs of the CG10-ECNFs (a1, a2, a3) with a small diameter and a large packing density in the gradient pore structure carbon nanofiber electrode material prepared in Example 1, the blank carbon nanofiber electrode material 14-ECNFs (b1, b2, b3) in the control example, and the CG18-ECNFs (c1, c2, c3) with a large diameter and a small packing density in the gradient pore structure carbon nanofiber electrode material.
[0025] Figure 2 It is the cyclic voltammetry curve of the upper and lower surfaces (CG10-ECNFs, CG18-ECNFs) of the blank carbon nanofiber electrode material 14-ECNFs and the gradient pore structure carbon nanofiber electrode material CG-ECNFs prepared in Example 1 in vanadium electrolyte.
[0026] Figure 3 The three groups of vanadium batteries assembled in Example 2 are charge and discharge curves at different current densities (a), energy efficiency diagram (b), voltage efficiency and coulomb efficiency diagram (c), capacity decay curve diagram (d) and cycle stability diagram (e). DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings and embodiments.
[0028] Example 1
[0029] (I) Comparative example - blank carbon nanofiber electrode material
[0030] The preparation method comprises the following steps:
[0031] 1) Preparation of blank electrospinning precursor solution
[0032] The dried polyacrylonitrile (PAN) powder with a molecular weight of 150,000 was dissolved in N,N,-dimethylformamide (DMF) solution and magnetically stirred at 80°C for 6 hours until completely dissolved to obtain a blank PAN / DMF electrospinning precursor solution with a polyacrylonitrile (PAN) mass percentage concentration of 14 wt%.
[0033] 2) Preparation of original blank polyacrylonitrile nanofiber material by electrospinning
[0034] The blank PAN / DMF electrospinning precursor solution was sucked into the syringe of the electrospinning equipment, and the original blank polyacrylonitrile nanofiber material was obtained by electrospinning technology. Electrospinning conditions: the stainless steel nozzle model is G20, the collector is a stainless steel roller, the roller speed is 100r / min; the voltage between the nozzle and the roller is 20kV; the distance between the nozzle and the roller is 12cm; the spinning temperature is 25℃; the spinning humidity is 30%RH; the push speed is 30μL / min, and 24mL of the precursor solution is spun.
[0035] 3) Preparation of blank carbon nanofiber electrode materials by pre-oxidation and carbonization
[0036] The obtained original blank polyacrylonitrile nanofiber material was flattened with a corundum plate and placed in a tubular furnace for pre-oxidation treatment, i.e., in an air atmosphere, the temperature was increased to 180°C at a heating rate of 2°C / min, and kept warm for 10 minutes, and then the temperature was increased to 290°C at a heating rate of 1°C / min, and kept warm for 60 minutes; then a carbonization treatment was carried out, i.e., in a N2 atmosphere, the temperature was increased at a rate of 5°C / min, and kept warm at 1000°C for 120 minutes, and then cooled to room temperature to obtain a blank carbon nanofiber electrode material 14-ECNFs.
[0037] like Figure 1 As shown in b1-b3, the diameter of the blank carbon nanofiber electrode material obtained is about 160nm and the surface is smooth. (II) Highly active PAN concentration gradient carbon nanofiber electrode material
[0038] The preparation method comprises the following steps:
[0039] 1) Preparation of electrospinning precursor solution
[0040] The dried polyacrylonitrile (PAN) powder with a molecular weight of 150,000 was dissolved in N,N,-dimethylformamide (DMF) in different mass proportions and magnetically stirred at 80°C for 6 hours until completely dissolved to obtain PAN / DMF electrospinning precursor solutions with polyacrylonitrile (PAN) mass percentage concentrations of 10wt%, 14wt%, and 18wt%, respectively.
[0041] 2) Preparation of original gradient pore structure nanofiber materials by continuous electrospinning
[0042] 18wt%, 14wt%, 10wt% PAN / DMF electrospinning precursor solutions were sucked into the syringe of the electrospinning equipment in turn, and the electrospinning technology was used to continuously electrospin to obtain the original fiber material. Electrospinning conditions: The stainless steel nozzle model is G20, the collector is a stainless steel roller, and the roller speed is 100r / min; the voltage between the nozzle and the roller is 20kV; the distance between the nozzle and the roller is 12cm; the spinning temperature is 25℃; the spinning humidity is 30%RH; the push speed is 30μL / min, and 18wt%, 14wt%, 10wt% PAN / DMF electrospinning precursor solutions are each continuously electrospun 8mL.
[0043] 3) Preparation of highly active PAN concentration gradient carbon nanofiber electrode materials by pre-oxidation and carbonization
[0044] The obtained original gradient pore structure nanofiber material was flattened with a corundum plate and placed in a tubular furnace for pre-oxidation treatment, i.e., in an air atmosphere, the temperature was increased to 180°C at a heating rate of 2°C / min, and kept warm for 10 minutes, and then the temperature was increased to 290°C at a heating rate of 1°C / min, and kept warm for 60 minutes; then a carbonization treatment was carried out, i.e., in a N2 atmosphere, the heating rate was 5°C / min, and the temperature was kept at 1000°C for 120 minutes, and then cooled to room temperature to obtain a gradient pore structure carbon nanofiber electrode material, of which the upper and lower surfaces were named CG10-ECNFs and CG18-ECNFs, respectively.
[0045] like Figure 1As shown in a1-a3 and c1-c3, the diameter of the CG10-ECNFs fiber on the upper surface of the obtained gradient pore structure carbon nanofiber electrode material is about 130nm, the diameter of the CG18-ECNFs fiber on the lower surface is about 290nm, and the fiber surface is smooth.
[0046] Example 2 Electrochemical performance test of gradient pore structure carbon nanofiber electrode material
[0047] 1) Cyclic voltammetry test
[0048] Method: A three-electrode system was used, with 1 cm prepared in Example 1. 2 The upper and lower surfaces of blank carbon nanofiber electrode material 14-ECNFs and gradient pore structure carbon nanofiber electrode material were in contact with the electrolyte as working electrode, saturated glycan common electrode as reference electrode, platinum sheet as counter electrode, 0.1M VOSO4+2.0M H2SO4 as electrolyte, and the electrochemical properties of the electrodes were investigated by cyclic voltammetry with a scan rate of 5mV / s.
[0049] like Figure 2 As shown, 14-ECNFs, CG10-ECNFs and CG18-ECNFs electrodes all showed V 2+ / V 3+ and VO 2+ / VO2 + However, compared with 14-ECNFs, the CV graphs measured on CG10-ECNFs and CG18-ECNFs electrodes have larger peak currents and smaller peak potential differences, which may be attributed to the larger specific surface area of CG10-ECNFs electrode materials and the better electrolyte permeability of CG18-ECNFs electrode materials. It is worth noting that the potential difference between the oxidation peak and the reduction peak on CG18-ECNFs (when the thicker side of CG-ECNFs fibers is in direct contact with the electrolyte) and CG10-ECNFs (that is, the thinner side of CG10-ECNFs fibers is in direct contact with the electrolyte) is basically the same, while the peak current on CG18-ECNFs is larger. This enhancement of the reversibility of the electrochemically active agent may be due to the gradient distribution of the pores from large to small inside the electrode, which is more conducive to the penetration of the electrolyte, increases the effective reaction area, and improves the electrochemical reaction activity.
[0050] 2) Single battery charge and discharge test
[0051] Method: 4 cm prepared in Example 1 2Blank carbon nanofiber electrode materials and gradient pore structure carbon nanofiber electrode materials are used as positive and negative electrodes. When CG10-ECNFs and CG18-ECNFs are assembled into batteries, the electrodes are in contact with the current collector (liquid inlet side) on one side and the separator on the other side; Nafion212 is an ion exchange membrane, 1.65MV 3+ / V 4+ +3.0M H2SO4 is the electrolyte, the volume of the positive and negative electrolytes are 20mL and 10mL respectively, and a single cell is assembled for charge and discharge tests. The charge and discharge cut-off voltages are 1.75V and 1.0V respectively, and the current density is 100mA / cm 2 ~400mA / cm 2 , and the charge and discharge cycles were repeated 3 times at each current density. The corresponding charge and discharge curves at different current densities are shown in Figure 3 As shown in (a), the battery efficiency is Figure 3 As shown in (bc), the capacity comparison is Figure 3 In addition, the vanadium battery assembled with CG-ECNFs as positive and negative electrodes was tested for 500 cycles of stability, and the corresponding battery efficiency attenuation is shown in Figure 3 As shown in e.
[0052] The results show that the CG18-ECNFs battery group, whose larger diameter side is in contact with the current collector, shows higher charge-discharge capacity and energy efficiency at all current densities. As the current density increases, the energy efficiency of the 14-ECNFs and CG10-ECNFs batteries differs more from that of the 14-ECNFs and CG10-ECNFs batteries, indicating that the CG18-ECNFs battery group has better rate performance. This is due to the fact that the electrode material has a larger porosity and pore size in the mass transfer control area, i.e., the liquid inlet side of the current collector, which is more conducive to the penetration of the electrolyte, thereby increasing the effective area of the electrode, improving the active surface area of the electrode while taking into account the mass transfer performance, so that it can maintain a relatively rapid reactant supply rate at a higher current density. At a current density of 200 mA cm -2 Under the condition of , the battery assembled with CG18-ECNFs showed the highest VE (82.73%) and the highest EE (79.38%), which further verified the effectiveness of this gradient pore structure electrode material in improving battery performance. In addition, the battery assembled with CG18-ECNFs showed less energy efficiency decay after 500 cycles ( Figure 3 e), indicating that it has good cycle stability.
Claims
1. A method for preparing a gradient pore structure carbon nanofiber electrode material, characterized in that: The steps include: 1) mixing polyacrylonitrile and N,N,-dimethylformamide at different mass ratios to obtain a series of electrospinning precursor solutions of polyacrylonitrile with gradient mass percentage concentrations; 2) sucking the electrospinning precursor solutions prepared in step 1) into the electrospinning syringe in equal volumes according to the mass percentage concentration of polyacrylonitrile from high to low, and continuously electrospinning each electrospinning precursor solution using electrospinning technology to obtain the original nanofiber material; 3) The original nanofiber material obtained in step 2) is flattened with a corundum plate, placed in a tube furnace for pre-oxidation treatment and carbonization treatment, and then cooled to room temperature to obtain a gradient pore structure carbon nanofiber electrode material.
2. The preparation method according to claim 1, characterized in that: In step 1), the molecular weight of the polyacrylonitrile is 90,000 to 150,000.
3. The preparation method according to claim 1, characterized in that: In step 1), the mixing conditions are: magnetic stirring at 80° C. for 6 h.
4. The preparation method according to claim 1, characterized in that: In step 1), in the electrospinning precursor solution of a series of gradient mass percentage concentrations of polyacrylonitrile, the mass percentage concentration of polyacrylonitrile is 8% to 20%, and the concentration difference between adjacent mass percentage concentrations of polyacrylonitrile is 3% to 5%.
5. The preparation method according to claim 1, characterized in that: In step 2), the process conditions of the electrospinning technology are as follows: the stainless steel nozzle model is G15~G22; the wire collector is a stainless steel roller, and the roller speed is 50~150r / min; the voltage between the nozzle and the roller is 18~22kV; the distance between the nozzle and the roller is 10~15cm; the spinning temperature is 25℃~30℃; the spinning humidity is 30%~50%RH; the push speed is 10~50μL / min; 8mL~20mL of each mass percentage concentration of polyacrylonitrile solution is spun.
6. The preparation method according to claim 1, characterized in that: In step 3), the pre-oxidation treatment conditions are: in an air atmosphere, heating to 180°C at a heating rate of 2°C / min, keeping warm for 10 minutes, then heating to 290°C at a heating rate of 1°C / min, keeping warm for 60 minutes.
7. The preparation method according to claim 1, characterized in that: In step 3), the carbonization treatment conditions are: in a nitrogen or argon atmosphere, a heating rate of 5°C / min, and keeping at 1000°C for 120 min.
8. Use of the gradient pore structure carbon nanofiber electrode material obtained by the preparation method according to any one of claims 1 to 7 in liquid flow batteries.
9. The use according to claim 8, characterized in that: When assembling the liquid flow battery, the side of the gradient pore structure carbon nanofiber electrode material with a small fiber diameter and a large packing density is in contact with the diaphragm as an activation enhancement zone, and the side with a large fiber diameter and a small packing density is in contact with the current collector as a mass transfer enhancement zone.
10. The use according to claim 8, characterized in that: The flow batteries include all-vanadium flow batteries, zinc-bromine flow batteries, iron-chromium flow batteries and organic flow batteries.