Preparation method of super-washable fluoride-free waterproof fabric

Through the improved dyeing and finishing process, combined with NaOH, sodium disulfite and cationic fluorine-free anti-water splashing agent, the problem of waterproof fabric degradation after multiple machine washings is solved, achieving super-wash-resistant waterproofing effect, and avoiding Environmental protection issues of fluorine-containing compounds.

CN118979393APending Publication Date: 2024-11-19NANTONG TEIJIN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411276327.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The waterproof performance of existing waterproof fabrics has dropped sharply after multiple machine washings, making it difficult to meet consumers' demand for durable washing, and the use of fluorine-containing compounds has environmental problems.

Method used

Adopt improved dyeing and finishing processes, including desizing, dyeing, two washings, drying, anti-spraying treatment and shaping and finishing, and enhancement of chemicals such as NaOH, sodium sulfite, chelating agent, cationic fluorine-free anti-spraying agent and other chemicals. The bonding force and cross-linking effect of fabric and water-repellent ensure that the fabric maintains good waterproof performance after 100 machine washes.

Benefits of technology

The ultra-wash-resistant fluorine-free waterproof fabric prepared has a waterproofing level of more than 3 after 100 machine washes, meeting consumers' needs for durable cleaning and waterproof performance, while avoiding the environmental risks of fluorine-containing compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979393A_ABST
    Figure CN118979393A_ABST
Patent Text Reader

Abstract

A preparation method of a super-washable fluoride-free waterproof fabric relates to the technical field of textile dyeing and finishing, and comprises the following steps: S1, desizing; s2, dyeing and washing; s2.1, dyeing is carried out; immersing the desized fabric into the dye liquor for dyeing; s2.2, washing for the first time; naOH, sodium hydrosulfite and a chelating agent are added into the first washing liquid, and the dyed fabric is soaked into the first washing liquid to be washed; s2.3, washing for the second time; an anionic color fixing agent is added into the second washing liquid, and the fabric subjected to primary washing is soaked into the second washing liquid to be washed; s3, drying; the dyed and washed fabric is dried at the temperature of 110-130 DEG C; s4, performing water repellent treatment; adding a pretreating agent, a cationic fluoride-free water-repellent agent, a cross-linking agent, a penetrating agent and organic acid into a water-repellent solution, padding the dried fabric into the water-repellent solution, and then drying at the temperature of 110-130 DEG C; s5, shaping and finishing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile dyeing and finishing, and in particular to a method for preparing a super washable fluorine-free waterproof fabric. Background Art

[0002] The 1930s to 1950s were the initial development period of waterproofing agents, which were mainly based on fluorine-free materials, ordinary or semi-durable waterproofing, and not oil-proof. From the 1950s to the end of the 20th century, waterproofing and oil-proofing entered a rapid development period. The advent of fluorine-containing waterproofing and oil-proofing agents has improved the requirements for clothing performance, and can be expanded to high-performance requirements such as three-proofing, easy decontamination, water repellency, high water pressure resistance, blood resistance, and alcohol resistance. At the beginning of the 21st century, it entered the conversion period of perfluorooctanoic acid replacement targets. Water repellents have also undergone an overall evolution process from 8 carbons to 6 carbons, and after 100 years, they have returned to the original fluorine-free. Water-repellent finishing is one of the important projects of functional finishing of textiles. The most widely used water-repellent finishing agents are fluorinated compounds containing 8 carbon chains or 6 carbon chains. Studies have shown that perfluorooctanoate (PFOA) and perfluorooctane sulfonic acid (PFOS), byproducts produced during the production process of fluorinated compounds, are potentially carcinogenic and difficult to decompose through biological metabolism. They are currently one of the most difficult organic pollutants to degrade. In 2008, the EU officially implemented a restriction that the PFOS content in textiles exported to the EU must be less than 1ug / m 2 , and also proposed the same restriction requirements for PFOA. Subsequently, the US market also proposed corresponding restrictions. Therefore, fluorine-free water-repellent finishing has become an urgent need. The development of ultra-durable water-repellent fabrics based on fluorine-free water-repellent agents has become a new process development direction.

[0003] As people's living standards continue to improve, the functional requirements for clothing fabrics are also getting higher and higher. For water-repellent functional fabrics, people not only pursue their initial water-repellent performance, but also the topic of durable washing is constantly increasing. Due to the accelerated pace of life, consumers usually use machine washing to wash their clothes. Existing waterproof fabrics are usually not resistant to machine washing. After multiple machine washings, the waterproof performance drops sharply and it is difficult to meet application needs. At the same time, due to the current prevalence of green environmental protection, cherishing things, and long-term holding, waterproof functional clothing has basically lost its waterproof performance after multiple washings. Consumers have a considerable mental burden on whether to continue to wear it reluctantly, or choose to recycle or discard it.

[0004] Chinese patent CN107587346B discloses a fluorine-free water-repellent fabric and a manufacturing method thereof, which can achieve a waterproof level of more than level 3 after 10 or 20 washes. Compared with ordinary waterproof fabrics, this fabric has better washability, but it still cannot meet consumers' expectations for stronger washability of waterproof fabrics.

[0005] Therefore, how to improve the dyeing and finishing process of waterproof fabrics so that the fabrics still have good waterproof performance after multiple machine washings has become a technical problem that needs to be solved urgently. Summary of the invention

[0006] In view of the above technical problems, the present invention provides a method for preparing a super washable fluorine-free waterproof fabric with super washability and a waterproof grade of more than grade 3 after 100 machine washings.

[0007] The technical solution of the present invention is: A method for preparing a super washable fluorine-free waterproof fabric comprises the following steps: S1: Desizing: adding NaOH solution, scouring agent and chelating agent to the tank liquid of the desizing machine to remove the size in the grey cloth; S2: dyeing and washing; S2.1: dyeing: immersing the desized fabric into dyeing solution for dyeing; S2.2: First wash: add NaOH, sodium dithionite and chelating agent to the first washing liquid, immerse the dyed fabric in the first washing liquid for washing, and wash away the floating color on the surface of the fabric; S2.3: Second wash: add anionic color fixing agent to the second wash solution, immerse the fabric after the first wash in the second wash solution for washing, so that the fabric is attached with negative charge; S3: Drying: Drying the dyed and washed fabric at a temperature of 110-130°C; S4: water-repellent treatment: adding a pretreatment agent, a cationic fluorine-free water-repellent agent, a cross-linking agent, a penetrant and an organic acid to the water-repellent solution, dipping the dried fabric into the water-repellent solution, and then drying at a temperature of 110 to 130°C; S5: shaping and finishing: use a shaping machine for heat shaping, and keep the fabric in the oven for 20 to 50 seconds.

[0008] The processing temperatures of step S2.2 and step S2.3 are both 80-90°C.

[0009] In the step S2.2, the dosage of NaOH is 2-4 g / L, the dosage of sodium dithionite is 2-4 g / L, and the dosage of the chelating agent is 1-2 g / L.

[0010] The amount of the anionic color fixing agent used in step S2.3 is 1 to 2 g / L.

[0011] In the S4 step, the dosage of the pretreatment agent is 10-100 g / L, the dosage of the cationic fluorine-free water-repellent agent is 100-120 g / L, the dosage of the cross-linking agent is 10-30 g / L, the dosage of the penetrant is 30-50 g / L, and the dosage of the organic acid is the required dosage for adjusting the pH value of the water-repellent solution to 3.5-4.5.

[0012] The cationic fluorine-free water-repellent agent comprises 40-80 g / L of an acrylic fluorine-free water-repellent agent and 40-80 g / L of a silicone fluorine-free water-repellent agent.

[0013] The processing temperature of step S1 is 80-95°C.

[0014] In the step S1, the concentration of the NaOH solution is 32%, the dosage is 6-10 g / L, the dosage of the scouring agent is 1-3 g / L, and the dosage of the chelating agent is 1-1.8 g / L.

[0015] The setting temperature of the step S5 is not less than 160°C.

[0016] The invention discloses a method for preparing a super washable fluorine-free waterproof fabric. The method improves the dyeing and finishing process of the fabric and performs two washes after dyeing. The first wash process is used to wash away the floating color of the fabric and reduce residues, and the second wash process is used for color fixing treatment and making the fabric attached with negative charge. In the water-repellent treatment, a pretreatment agent is added to enhance the binding force between the fabric and the water-repellent agent, and a cationic water-repellent agent is used to make it firmly adsorbed with the negatively charged fabric, thereby promoting the water-repellent agent to be fully cross-linked and more firmly attached to the fabric. In the subsequent shaping and finishing, the cross-linking effect of the water-repellent agent is further enhanced by controlling the baking time, temperature and other parameters of the oven, so that the prepared fabric has super washability and still has excellent waterproof effect after multiple machine washings.

[0017] The preparation method of the super washable fluorine-free waterproof fabric of the present invention can greatly improve the washability of the waterproof fabric compared with the prior art through the coordinated cooperation of dyeing, waterproofing, finishing and other processes. The waterproof fabric prepared according to the method of the present invention has a waterproof grade of more than 3 after 100 machine washings, which can meet the comprehensive consumer demand for waterproof fabrics that can be washed multiple times to keep clean and hygienic, and can be effectively waterproof and have long-term effective waterproof functionality. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic flow chart of a method for preparing a super washable fluorine-free waterproof fabric of the present invention. Figure 2 It is the experimental data of the waterproof grade of the embodiments and comparative examples of the present invention.

[0019] In the figure: L0-initial state; L10-state after washing 10 times; L20-state after washing 20 times; L30-state after washing 30 times; L40-state after washing 40 times; L50-state after washing 50 times; L100-state after washing 100 times. DETAILED DESCRIPTION

[0020] The following is combined with Figure 1-2 , further illustrating the present invention.

[0021] The invention discloses a method for preparing a super washable fluorine-free waterproof fabric, comprising the following steps: S1: desizing; adding NaOH solution, scouring agent and chelating agent to the tank liquid of a desizing machine for treatment, so as to remove the sizing agent and oil agent in the grey cloth; S2: dyeing and washing; S2.1: dyeing; immersing the desizing fabric into a dyeing solution for dyeing, and adopting different dyeing temperatures according to the type of grey cloth, for example, polyester is usually dyed at 120-135°C, and nylon is usually dyed at 90-110°C; S2.2: first washing; adding NaOH, sodium dithionite and chelating agent to a first washing solution, immersing the dyed fabric into the first washing solution for washing, so as to wash away the floating color on the surface of the fabric and reduce the residue on the surface of the fabric; S2.3: second washing; adding anionic color fixing agent to a second washing solution, and dyeing the fabric after the first washing; The fabric is immersed in the second washing liquid for washing, so that the colorant adheres more firmly and the fabric is attached with negative charge, which is used to enhance the bonding force between the fabric and the water-repellent agent in subsequent processing; S3: Drying: The dyed and washed fabric is dried at a temperature of 110-130°C; S4: Water-repellent treatment: A pretreatment agent, a cationic fluorine-free water-repellent agent, a cross-linking agent, a penetrant and an organic acid are added to the water-repellent solution, the dried fabric is dipped in the water-repellent solution, and then dried at a temperature of 110-130°C; S5: Setting and finishing: A setting machine is used for heat setting, and the width and overfeeding are controlled to ensure the consistency of the width, density and gram weight of the fabric, and the fabric is kept in the oven for 20-50s so that the water-repellent agent can be fully cross-linked, effectively improving the waterproof and durability of the fabric.

[0022] The processing temperatures in step S2.2 and step S2.3 are both 80-90°C.

[0023] In step S2.2, the dosage of NaOH is 2-4 g / L, the dosage of sodium dithionite is 2-4 g / L, and the dosage of the chelating agent is 1-2 g / L.

[0024] The amount of anionic color fixing agent used in step S2.3 is 1-2 g / L.

[0025] In step S4, the dosage of the pretreatment agent is 10-100 g / L, the dosage of the cationic fluorine-free water-repellent agent is 100-120 g / L, the dosage of the cross-linking agent is 10-30 g / L, the dosage of the penetrant is 30-50 g / L, and the dosage of the organic acid is the amount required to adjust the pH value of the water-repellent solution to 3.5-4.5.

[0026] Cationic fluorine-free water repellents include 40-80g / L acrylic fluorine-free water repellents and 40-80g / L silicone fluorine-free water repellents. Acrylic fluorine-free water repellents are mainly used to improve the initial waterproof performance of fabrics, while silicone fluorine-free water repellents are mainly used to improve the waterproof performance of fabrics after multiple washings.

[0027] The processing temperature of step S1 is 80-95°C.

[0028] In step S1, the concentration of NaOH solution is 32%, the dosage is 6-10 g / L, the dosage of scouring agent is 1-3 g / L, and the dosage of chelating agent is 1-1.8 g / L.

[0029] The setting temperature in step S5 is not less than 160°C.

[0030] Example 1: Use polyester DTY yarn as warp yarn and DTY cool silk cotton as weft yarn to weave grey cloth. Add 6g / L of 32% NaOH solution, 2g / L of scouring agent, and 1g / L of chelating agent to the desizing machine, and perform desizing treatment at 95°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric twice at a washing temperature of 85°C; fill the washing tank with water for one wash, add 2g / L of NaOH, 4g / L of sodium dithionite, and 1g / L of chelating agent to the first wash, immerse the dyed fabric in the first wash to wash, wash away the floating color on the surface of the fabric, and drain the first wash after one wash; fill water again for a second wash, add 1g / L of anionic color fixing agent to the second wash, immerse the fabric after one wash in the second wash to wash, so that the fabric is attached with negative charge. Dry the dyed and washed fabric at 120°C. Add 70g / L of pretreatment agent, 50g / L of acrylic acid-based fluorine-free water-repellent agent, 70g / L of silicone-based fluorine-free water-repellent agent, 25g / L of cross-linking agent, 45g / L of penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 4.1; dip the dried fabric into the water-repellent solution, and then dry it at 120°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 170°C for 25s.

[0031] Comparative Example 1: Use polyester DTY yarn as warp yarn and DTY cool silk cotton as weft yarn to weave grey cloth. Add 6g / L of 32% NaOH solution, 2g / L of scouring agent, and 1g / L of chelating agent to the sizing machine, and perform desizing treatment at 95°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric at 85°C; add 2g / L NaOH, 4g / L sodium dithionite, and 1g / L of chelating agent to the washing solution, and immerse the dyed fabric in the washing solution for washing to remove the floating color on the surface of the fabric. Dry the dyed and washed fabric at 120°C. Add 50g / L acrylic acid-based fluorine-free water-repellent, 70g / L silicone-based fluorine-free water-repellent, 25g / L cross-linking agent, 45g / L penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 4.1, dip the dried fabric into the water-repellent solution, and then dry it at 120°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 170°C for 25s.

[0032] Example 2: Use polyester DTY yarn as warp and weft yarn to weave grey cloth. Add 10g / L of 32% NaOH solution, 1g / L of scouring agent, and 1.5g / L of chelating agent to the desizing machine, and perform desizing at 80°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric twice at a washing temperature of 85°C; fill the washing tank with water for one wash, add 3g / L NaOH, 4g / L sodium dithionite, and 1.5g / L of chelating agent to the first wash, immerse the dyed fabric in the first wash to wash, wash away the floating color on the surface of the fabric, and drain the first wash after one wash; fill water again for a second wash, add 2g / L of anionic color fixing agent to the second wash, immerse the fabric after one wash in the second wash to wash, so that the fabric is attached with negative charge. Dry the dyed and washed fabric at 120°C. Add 10g / L of pretreatment agent, 40g / L of acrylic acid-based fluorine-free water-repellent, 80g / L of silicone-based fluorine-free water-repellent, 30g / L of cross-linking agent, 30g / L of penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 4.5; dip the dried fabric into the water-repellent solution, and then dry it at 120°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 170°C for 42s.

[0033] Comparative Example 2: Use polyester DTY yarn as warp and weft yarn to weave grey cloth. Add 10g / L of 32% NaOH solution, 1g / L of scouring agent, and 1.5g / L of chelating agent to the sizing machine, and perform desizing at 80°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric at 85°C; add 3g / L NaOH, 4g / L sodium dithionite, and 1.5g / L of chelating agent to the washing solution, and immerse the dyed fabric in the washing solution for washing to remove the floating color on the surface of the fabric. Dry the dyed and washed fabric at 120°C. 40g / L acrylic acid-based fluorine-free water-repellent, 80g / L silicone-based fluorine-free water-repellent, 30g / L cross-linking agent, 30g / L penetrant were added to the water-repellent solution, and organic acid was added to adjust the pH value of the water-repellent solution to 4.5. The dried fabric was dipped into the water-repellent solution and then dried at 120°C. A setting machine was used for setting and finishing, and the fabric was kept in an oven at 170°C for 42s.

[0034] Example 3: Use polyester DTY yarn as warp and weft yarn to weave grey cloth. Add 8g / L of 32% NaOH solution, 3g / L of scouring agent, and 1.8g / L of chelating agent to the desizing machine, and perform desizing at 85°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric twice at 85°C; add water to the washing tank for one wash, add 3.5g / L NaOH, 4g / L sodium dithionite, and 1.8g / L of chelating agent to the first wash, immerse the dyed fabric in the first wash to wash, wash away the floating color on the surface of the fabric, and drain the first wash after one wash; then add water for a second wash, add 1g / L of anionic color fixing agent to the second wash, immerse the fabric after one wash in the second wash to wash, so that the fabric is attached with negative charge. Dry the dyed and washed fabric at 120°C. Add 30g / L of pretreatment agent, 75g / L of acrylic acid-based fluorine-free water-repellent agent, 45g / L of silicone-based fluorine-free water-repellent agent, 30g / L of cross-linking agent, 45g / L of penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 3.9; dip the dried fabric into the water-repellent solution, and then dry it at 120°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 165°C for 36s.

[0035] Comparative Example 3: Use polyester DTY yarn as warp and weft yarn to weave grey cloth. Add 8g / L of 32% NaOH solution, 3g / L of scouring agent, and 1.8g / L of chelating agent to the sizing machine, and perform desizing at 85°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric at 85°C; add 3.5g / L NaOH, 4g / L of sodium dithionite, and 1.8g / L of chelating agent to the washing solution, and immerse the dyed fabric in the washing solution for washing to remove the floating color on the surface of the fabric. Dry the dyed and washed fabric at 120°C. 75g / L acrylic acid-based fluorine-free water-repellent, 45g / L silicone-based fluorine-free water-repellent, 30g / L cross-linking agent, 45g / L penetrant were added to the water-repellent solution, and organic acid was added to adjust the pH value of the water-repellent solution to 3.9. The dried fabric was dipped into the water-repellent solution and then dried at 120°C. A setting machine was used for setting and finishing, and the fabric was kept in an oven at 165°C for 36s.

[0036] Example 4: Use polyester DTY yarn as warp and weft yarn to weave grey cloth. Add 6g / L of 32% NaOH solution, 2g / L of scouring agent, and 1g / L of chelating agent to the desizing machine, and perform desizing at 95°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric twice at 80°C; fill the washing tank with water for one wash, add 3g / L of NaOH, 3g / L of sodium dithionite, and 1.5g / L of chelating agent to the first wash, immerse the dyed fabric in the first wash to wash, wash away the floating color on the surface of the fabric, and drain the first wash after one wash; fill water again for a second wash, add 1.5g / L of anionic color fixing agent to the second wash, immerse the fabric after one wash in the second wash to wash, so that the fabric is attached with negative charge. Dry the dyed and washed fabric at 125°C. Add 80g / L of pretreatment agent, 40g / L of acrylic acid-based fluorine-free water-repellent, 80g / L of silicone-based fluorine-free water-repellent, 30g / L of cross-linking agent, 50g / L of penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 4; dip the dried fabric into the water-repellent solution, and then dry it at 125°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 175°C for 40s.

[0037] Comparative Example 4: Use polyester DTY yarn as warp and weft yarn to weave grey cloth. Add 6g / L of 32% NaOH solution, 2g / L of scouring agent, and 1g / L of chelating agent to the desizing machine, and perform desizing at 95°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric at 80°C; add 3g / L NaOH, 3g / L sodium dithionite, and 1.5g / L of chelating agent to the washing solution, and immerse the dyed fabric in the washing solution for washing to remove the floating color on the surface of the fabric. Dry the dyed and washed fabric at 125°C. Add 40g / L acrylic acid-based fluorine-free water-repellent, 80g / L silicone-based fluorine-free water-repellent, 30g / L cross-linking agent, 50g / L penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 4. The dried fabric is dipped into the water-repellent solution and then dried at 125°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 175°C for 40s.

[0038] Example 5: Use polyester DTY yarn as warp and weft yarn to weave grey cloth. Add 6g / L of 32% NaOH solution, 2g / L of scouring agent, and 1g / L of chelating agent to the desizing machine, and perform desizing at 95°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric twice at 80°C; fill the washing tank with water for one wash, add 2g / L of NaOH, 3.5g / L of sodium dithionite, and 1.5g / L of chelating agent to the first wash, immerse the dyed fabric in the first wash to wash, wash away the floating color on the surface of the fabric, and drain the first wash after one wash; fill water again for two washes, add 2g / L of anionic color fixing agent to the second wash, immerse the fabric after one wash in the second wash to wash, so that the fabric is attached with negative charge. Dry the dyed and washed fabric at 130°C. Add 90g / L of pretreatment agent, 45g / L of acrylic acid-based fluorine-free water-repellent agent, 75g / L of silicone-based fluorine-free water-repellent agent, 20g / L of cross-linking agent, 40g / L of penetrant to the water-repellent solution, and add organic acid to compound until the pH value of the water-repellent solution is 4.3; dip the dried fabric into the water-repellent solution, and then dry it at 130°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 175°C for 45s.

[0039] Comparative Example 5: Use polyester DTY yarn as warp and weft yarn to weave grey cloth. Add 6g / L of 32% NaOH solution, 2g / L of scouring agent, and 1g / L of chelating agent to the sizing machine, and perform desizing at 95°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric at 80°C; add 2g / L NaOH, 3.5g / L of sodium dithionite, and 1.5g / L of chelating agent to the washing solution, and immerse the dyed fabric in the washing solution for washing to remove the floating color on the surface of the fabric. Dry the dyed and washed fabric at 130°C. 45g / L acrylic acid-based fluorine-free water-repellent, 75g / L silicone-based fluorine-free water-repellent, 20g / L cross-linking agent, 40g / L penetrant were added to the water-repellent solution, and organic acid was added to adjust the pH value of the water-repellent solution to 4.3. The dried fabric was dipped into the water-repellent solution and then dried at 130°C. A setting machine was used for setting and finishing, and the fabric was kept in an oven at 175°C for 45s.

[0040] Example 6: Use polyester DTY yarn as warp and weft yarn to weave grey cloth. Add 10g / L of 32% NaOH solution, 1g / L of scouring agent, and 1.5g / L of chelating agent to the desizing machine, and perform desizing at 80°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric twice at a washing temperature of 85°C; fill the washing tank with water for one wash, add 3g / L NaOH, 4g / L sodium dithionite, and 2g / L of chelating agent to the first wash, immerse the dyed fabric in the first wash to wash, wash away the floating color on the surface of the fabric, and drain the first wash after one wash; fill water again for a second wash, add 1.5g / L of anionic color fixing agent to the second wash, immerse the fabric after one wash in the second wash to wash, so that the fabric is attached with negative charge. Dry the dyed and washed fabric at 130°C. Add 100g / L pretreatment agent, 60g / L acrylic acid-based fluorine-free water-repellent agent, 50g / L silicone-based fluorine-free water-repellent agent, 25g / L cross-linking agent, 45g / L penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 4; dip the dried fabric into the water-repellent solution, and then dry it at 130°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 170°C for 20s.

[0041] Comparative Example 6: Use polyester DTY yarn as warp and weft yarn to weave grey cloth. Add 10g / L of 32% NaOH solution, 1g / L of scouring agent, and 1.5g / L of chelating agent to the sizing machine, and perform desizing at 80°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric at 85°C; add 3g / L NaOH, 4g / L sodium dithionite, and 2g / L of chelating agent to the washing solution, and immerse the dyed fabric in the washing solution for washing to remove the floating color on the surface of the fabric. Dry the dyed and washed fabric at 130°C. 60g / L acrylic acid-based fluorine-free water-repellent, 50g / L silicone-based fluorine-free water-repellent, 25g / L cross-linking agent, 45g / L penetrant were added to the water-repellent solution, and organic acid was added to adjust the pH value of the water-repellent solution to 4. The dried fabric was dipped into the water-repellent solution and then dried at 130°C. A setting machine was used for setting and finishing, and the fabric was kept in an oven at 170°C for 20s.

[0042] Example 7: Use DTY cool silk cotton as warp yarn and T400 silk as weft yarn to weave grey cloth. Add 10g / L of 32% NaOH solution, 1g / L of scouring agent, and 1.5g / L of chelating agent to the sizing machine tank liquid, and perform desizing treatment at 80°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing liquid for dyeing. Wash the dyed fabric twice at a washing temperature of 85°C; fill the washing tank with water for one wash, add 2g / L NaOH, 4g / L sodium dithionite, and 2g / L of chelating agent to the first wash liquid, immerse the dyed fabric in the first wash liquid for washing, wash away the floating color on the surface of the fabric, and drain the first wash liquid after one wash; fill water again for a second wash, add 1g / L of anionic color fixing agent to the second wash liquid, immerse the fabric after one wash in the second wash liquid for washing, so that the fabric is attached with negative charge. The dyed and washed fabrics were dried at 120°C. 20g / L of pretreatment agent, 80g / L of acrylic acid-based fluorine-free water-repellent, 40g / L of silicone-based fluorine-free water-repellent, 15g / L of cross-linking agent, 35g / L of penetrant were added to the anti-splash water solution, and organic acid was added to compound the pH value of the anti-splash water solution to 3.5; the dried fabric was dipped in the anti-splash water solution, and then dried at 120°C. A setting machine was used for setting and finishing, and the fabric was kept in an oven at 170°C for 35s.

[0043] Comparative Example 7: Use DTY cool silk cotton as warp yarn and T400 silk as weft yarn to weave grey cloth. Add 10g / L of 32% NaOH solution, 1g / L of scouring agent, and 1.5g / L of chelating agent to the sizing machine, and perform desizing at 80°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric at 85°C; add 2g / L NaOH, 4g / L sodium dithionite, and 2g / L of chelating agent to the washing solution, and immerse the dyed fabric in the washing solution for washing to remove the floating color on the surface of the fabric. Dry the dyed and washed fabric at 120°C. 80g / L acrylic acid-based fluorine-free water-repellent, 40g / L silicone-based fluorine-free water-repellent, 15g / L cross-linking agent, 35g / L penetrant were added to the water-repellent solution, and organic acid was added to adjust the pH value of the water-repellent solution to 3.5. The dried fabric was dipped into the water-repellent solution and then dried at 120°C. A setting machine was used for setting and finishing, and the fabric was kept in an oven at 170°C for 35s.

[0044] Example 8: Use DTY cool silk cotton as warp and weft yarn to weave grey cloth. Add 8g / L of 32% NaOH solution, 3g / L of scouring agent, and 1.8g / L of chelating agent to the desizing machine, and perform desizing at 85°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric twice at 90°C; fill the washing tank with water for one wash, add 2g / L of NaOH, 2g / L of sodium dithionite, and 1.2g / L of chelating agent to the first wash, immerse the dyed fabric in the first wash to wash, wash away the floating color on the surface of the fabric, and drain the first wash after one wash; fill water again for two washes, add 1.5g / L of anionic color fixing agent to the second wash, immerse the fabric after one wash in the second wash to wash, so that the fabric is attached with negative charge. Dry the dyed and washed fabric at 125°C. Add 60g / L pretreatment agent, 40g / L acrylic acid-based fluorine-free water-repellent agent, 60g / L silicone-based fluorine-free water-repellent agent, 10g / L cross-linking agent, 40g / L penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 4.2; dip the dried fabric into the water-repellent solution, and then dry it at 125°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 175°C for 30s.

[0045] Comparative Example 8: Use DTY cool silk cotton as warp and weft yarn to weave grey cloth. Add 8g / L of 32% NaOH solution, 3g / L of scouring agent, and 1.8g / L of chelating agent to the sizing machine, and perform desizing at 85°C to remove the sizing and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric at 90°C; add 2g / L NaOH, 2g / L of sodium dithionite, and 1.2g / L of chelating agent to the washing solution, and immerse the dyed fabric in the washing solution for washing to remove the floating color on the surface of the fabric. Dry the dyed and washed fabric at 125°C. Add 40g / L acrylic acid-based fluorine-free water-repellent, 60g / L silicone-based fluorine-free water-repellent, 10g / L cross-linking agent, 40g / L penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 4.2, dip the dried fabric into the water-repellent solution, and then dry it at 125°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 175°C for 30s.

[0046] Example 9: Use DTY yarn as warp yarn and PTT yarn as weft yarn to weave grey cloth. Add 6g / L of 32% NaOH solution, 2g / L of scouring agent, and 1g / L of chelating agent to the desizing machine, and perform desizing treatment at 95°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric twice at 90°C; fill the washing tank with water for one wash, add 2g / L of NaOH, 3g / L of sodium dithionite, and 1g / L of chelating agent to the first wash, immerse the dyed fabric in the first wash to wash, wash away the floating color on the surface of the fabric, and drain the first wash after one wash; fill water again for two washes, add 1g / L of anionic color fixing agent to the second wash, immerse the fabric after one wash in the second wash to wash, so that the fabric is attached with negative charge. Dry the dyed and washed fabric at 110°C. Add 40g / L pretreatment agent, 50g / L acrylic acid-based fluorine-free water-repellent agent, 70g / L silicone-based fluorine-free water-repellent agent, 15g / L cross-linking agent, 35g / L penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 4; dip the dried fabric into the water-repellent solution, and then dry it at 110°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 160°C for 50s.

[0047] Comparative Example 9: Use DTY yarn as warp yarn and PTT yarn as weft yarn to weave grey cloth. Add 6g / L of 32% NaOH solution, 2g / L of scouring agent, and 1g / L of chelating agent to the sizing machine, and perform desizing treatment at 95°C to remove the sizing agent and oil in the grey cloth. Immerse the desized fabric in dyeing solution for dyeing. Wash the dyed fabric at 90°C; add 2g / L NaOH, 3g / L sodium dithionite, and 1g / L of chelating agent to the washing solution, and immerse the dyed fabric in the washing solution for washing to remove the floating color on the surface of the fabric. Dry the dyed and washed fabric at 110°C. Add 50g / L acrylic acid-based fluorine-free water-repellent, 70g / L silicone-based fluorine-free water-repellent, 15g / L cross-linking agent, 35g / L penetrant to the water-repellent solution, and add organic acid to mix until the pH value of the water-repellent solution is 4. The dried fabric is dipped into the water-repellent solution and then dried at 110°C. Use a setting machine for setting and finishing, and keep the fabric in an oven at 160°C for 50s.

[0048] See attached Figure 2 The waterproof levels of the fabrics made in the embodiments of the present invention in the initial state L0, the state L10 after washing 10 times, the state L20 after washing 20 times, the state L30 after washing 30 times, the state L40 after washing 40 times, the state L50 after washing 50 times, and the state L100 after washing 100 times are all above 3, and have excellent wash resistance and long-term effective waterproof performance.

[0049] Regarding the contents disclosed in the present invention, there are still the following points to be explained: (1) The embodiments disclosed in the present invention are only examples, and the technical solutions implemented by other equivalent alternative technical means shall fall within the protection scope of the present invention; (2) In the absence of conflict, the technical features disclosed in the present invention may be combined with each other to obtain new embodiments; The above are only specific implementation methods disclosed in the present invention, but the protection scope of the present invention is not limited thereto. Technical solutions obtained after modifications and transformations of certain technical features by those skilled in the art based on the contents disclosed in the present invention should all be within the protection scope of the present invention.

Claims

1. A method for preparing a super washable fluorine-free waterproof fabric, characterized in that: The following steps are involved: S1: Desizing: NaOH solution, scouring agent and chelating agent are added to the tank liquid of the desizing machine to remove the size in the grey cloth; S2: dyeing and washing; S2.1: dyeing: immersing the desized fabric into dyeing solution for dyeing; S2.2: First wash: add NaOH, sodium dithionite and chelating agent to the first washing liquid, immerse the dyed fabric in the first washing liquid for washing, and wash away the floating color on the surface of the fabric; S2.3: Second wash: add anionic color fixing agent to the second wash solution, immerse the fabric after the first wash in the second wash solution for washing, so that the fabric is attached with negative charge; S3: Drying: Drying the dyed and washed fabric at a temperature of 110 to 130°C; S4: Water-repellent treatment; Add a pretreatment agent, a cationic fluorine-free water-repellent agent, a cross-linking agent, a penetrant and an organic acid into the water-repellent solution, dip the dried fabric into the water-repellent solution, and then dry it at a temperature of 110 to 130° C.; S5: shaping and finishing: use a shaping machine for heat shaping, and keep the fabric in the oven for 20 to 50 seconds.

2. The method for preparing a super washable fluorine-free waterproof fabric according to claim 1, characterized in that: The processing temperatures of step S2.2 and step S2.3 are both 80-90°C.

3. The method for preparing a super washable fluorine-free waterproof fabric according to claim 1, characterized in that: In the step S2.2, the dosage of NaOH is 2-4 g / L, the dosage of sodium dithionite is 2-4 g / L, and the dosage of the chelating agent is 1-2 g / L.

4. The method for preparing a super washable fluorine-free waterproof fabric according to claim 1, characterized in that: The amount of the anionic color fixing agent used in step S2.3 is 1 to 2 g / L.

5. The method for preparing a super washable fluorine-free waterproof fabric according to claim 1, characterized in that: In the S4 step, the dosage of the pretreatment agent is 10-100 g / L, the dosage of the cationic fluorine-free water-repellent agent is 100-120 g / L, the dosage of the cross-linking agent is 10-30 g / L, the dosage of the penetrant is 30-50 g / L, and the dosage of the organic acid is the required dosage for adjusting the pH value of the water-repellent solution to 3.5-4.

5.

6. The method for preparing a super washable fluorine-free waterproof fabric according to claim 5, characterized in that: The cationic fluorine-free water-repellent agent comprises 40-80 g / L of an acrylic fluorine-free water-repellent agent and 40-80 g / L of a silicone fluorine-free water-repellent agent.

7. The method for preparing a super washable fluorine-free waterproof fabric according to claim 1, characterized in that: The processing temperature of step S1 is 80-95°C.

8. The method for preparing a super washable fluorine-free waterproof fabric according to claim 1, characterized in that: In the step S1, the concentration of the NaOH solution is 32%, the dosage is 6-10 g / L, the dosage of the scouring agent is 1-3 g / L, and the dosage of the chelating agent is 1-1.8 g / L.