NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material and preparation method thereof
NiMo-LDH/MOF positive electrode material is prepared through two-step hydrothermal reaction of Ni-MOF template, which solves the problems of insufficient agglomeration and electrochemical performance of NiMo-LDH electrode material, and achieves high specific capacitance and good rate performance, which is suitable for super Industrial application of capacitors.
Patent Information
- Application Number
- CN202411326276.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-19
AI Technical Summary
The existing NiMo-LDH electrode materials have problems with agglomeration, insufficient electrochemical performance, complex and high cost in energy storage devices, which limit their application in supercapacitors.
Using Ni-MOF as a template, NiMo-LDH/MOF positive electrode material was prepared through two-step hydrothermal reactions, forming a three-dimensional flower spherical structure composed of thin nanosheets, avoiding the self-stacking of LDHs, increasing the active site and specific surface area, and improving the electrochemical properties.
It achieves high specific capacitance and good rate performance, simplifies the preparation process, reduces costs, and is suitable for mass production and large-scale applications.
Smart Images

Figure CN118983193A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials for energy storage devices, and in particular to a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material and a preparation method thereof. Background Art
[0002] Currently, alkali metal batteries (such as Li + 、Na + Mg 2+ However, they are prone to electrolyte leakage, low power density and high production cost in the process of electronic equipment application, which limits their application scope. Supercapacitors (SCs) have been widely used in the industrial field due to their inherent advantages such as fast charging and discharging capabilities, high power density and long cycle life. In order to meet the high market demand for energy storage devices, low energy density is still a problem that supercapacitors need to overcome, so there is an urgent need to develop high-performance electrode materials for supercapacitors.
[0003] Layered double hydroxides (LDHs) are a typical battery electrode material. This unique two-dimensional layered structure can significantly increase the contact area between the electrode and the electrolyte to promote ion diffusion and electron transfer. In order to increase active sites and promote electrolyte penetration, a reasonable structural design is needed to avoid LDHs self-accumulation.
[0004] The existing methods to improve the electrochemical performance of NiMo-LDH are mainly through doping, coating, structural control and other methods. Wang et al. successfully prepared nanoflower-shaped Ag-NiMo(OH) x The composite material improves the specific surface area and charge transport performance of the electrode material. -2 When the specific capacity is 3548mF cm -2 , but the use of precious metal Ag has a high preparation cost and fails to significantly improve the LDHs agglomeration problem and electrochemical performance; Wang et al. wrapped NiMo-LDH nanosheets on ZIF-67 by hydrothermal treatment, effectively preventing the problem of LDHs agglomeration. At 1A / g, the specific capacitance can reach 1734F / g, but the preparation method of this method is complicated and does not significantly improve the electrochemical performance of LDHs; Liang et al. grew CoNi-MOF nanosheets on carbon cloth, and then further anchored ultrathin NiMo-LDH nanosheets on its surface to form a honeycomb porous heterostructure (NiMo-LDH@CoNi-MOF). This porous heterostructure increases the electrochemically active specific surface area, shortens the charge transfer distance, and has a high specific capacitance at 1mA cm -2 Under these conditions, the specific capacitance can reach 15.6F cm-2 This method not only has complicated preparation steps, but also uses an in-situ growth method, and the amount of electrode material loaded in each step is difficult to control, making it difficult to apply in practice. These problems seriously limit the further practical application of LDHs materials.
[0005] In order to improve the technical defects of the above methods in practical applications, it is urgently necessary to develop a method with low preparation cost and simple process route, which can significantly improve the agglomeration problem of NiMo-LDH materials, enhance the structural stability of LDHs materials, enrich electrochemical active sites, improve the electrochemical performance and stability of NiMo-LDH, break through the common technical bottlenecks and limitations in the preparation process of LDHs materials, and further promote the application of LDHs materials in actual industrial and energy fields. Summary of the invention
[0006] In order to overcome the above technical problems, the purpose of the present invention is to provide a method for preparing a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material. The method uses Ni-MOF as a reaction template and prepares a NiMo-LDH / MOF positive electrode material through an in-situ topological reaction. The positive electrode material presents a three-dimensional flower ball structure composed of thin nanosheets without obvious accumulation phenomenon. This morphology structure can increase the number of active sites. The thin nanosheets are conducive to improving the transfer rate of electrons / ions and promoting OH - Penetrate into the electrode material and improve the electrochemical performance and rate performance of the electrode material through the synergistic effect of the two.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for preparing a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material comprises the following steps:
[0009] Step 1: Take a certain amount of nickel salt and ligand and dissolve them in N,N-dimethylformamide (DMF);
[0010] Stir or ultrasonicate at room temperature to obtain solution A, place solution A in a polytetrafluoroethylene liner for hydrothermal reaction to obtain a product, wash the product with DMF for multiple times, and place it in a vacuum drying oven to obtain Ni-MOF;
[0011] Step 2: Dissolve the Ni-MOF, molybdenum salt and urea in deionized water; disperse them at room temperature to obtain a mixed solution B, transfer them into a polytetrafluoroethylene reactor lining for hydrothermal reaction, wash them with ethanol and water, and dry them to obtain a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material.
[0012] In the above step 1, the molar concentrations of nickel salt and ligand in the obtained solution are controlled to be 0.155-0.225 mol / L and 0.015-0.125 mol / L, respectively. Solution A is placed in a polytetrafluoroethylene liner and reacted under hydrothermal conditions at 140-200° C. for 24-48 hours. The product is washed with DMF several times.
[0013] The nickel salt is one of NiCl2·6H2O, Ni(NO3)2·6H2O, Ni(CH3COO)2·4H2O or NiSO4·6H2O;
[0014] The ligand is one of pyromellitic acid (PA), terephthalic acid (TPA) or tetrafluoroterephthalic acid.
[0015] In the above step 2, the concentrations of Ni-MOF, molybdenum salt and urea in the solution are controlled to be 0.5-3.0 mg / mL, 0.008-0.02 mol / L and 0.122-0.215 mol / L, respectively, and the reaction is carried out at 100-160° C. hydrothermal conditions for 10-16 hours.
[0016] The molybdenum salt is specifically Na2MoO4·2H2O, C 10 H 14 MoO6 (Molybdenum acetylacetonate) or (NH4)6Mo7O 24 One of 4H2O.
[0017] In the above step 1, the concentrations of the nickel salt and the ligand are preferably 0.175 and 0.025 mol / L, respectively, and the reaction temperature and the reaction time are preferably 160° C. and 36 h, respectively.
[0018] In the above step 2, the concentrations of Ni-MOF, molybdenum salt and urea are preferably 1 mg / mL, 0.01 mol / L and 0.125 mol / L, respectively, and the reaction temperature and reaction time are preferably 120° C. and 12 h, respectively.
[0019] In the above preparation method, after the hydrothermal reaction is completed, the preferred drying temperature is 50-60°C.
[0020] In the above step 1, the filling degree in the polytetrafluoroethylene liner is preferably 40-60%.
[0021] A NiMo-LDH / MOF high specific capacitance supercapacitor cathode material, wherein the cathode material adopts a mild solvothermal method to prepare LDHs using Ni-MOF as a template, which not only retains the structural advantages of MOF, but also reduces the internal resistance of the LDHs electrode and accelerates the flow rate of carriers. At the same time, the introduction of transition metal ions increases the number of active sites, thereby promoting the electrochemical kinetic process.
[0022] Nickel ions, molybdenum ions combine with hydroxide ions to form a layered structure, and anions are inserted between the layers to balance the charge;
[0023] The synergistic effect between the easily stacked LDHs and the highly porous MOFs significantly increases the specific surface area of the material;
[0024] The three-dimensional flower-like structure composed of thin nanosheets increases the surface area of the electrode material, shortens the ion / charge transfer distance and is beneficial to the redox kinetics process; in addition, the porous channels and abundant pores in the three-dimensional flower-like structure help to reduce the impedance in the electrochemical process, reduce the resistance of ions and electrons during the transmission process, and accelerate the electrochemical process.
[0025] In NiMo-LDH / MOF, Mo is mainly 6+ Existing in the form of, and showing higher activity in redox reactions. High-valence ions usually have stronger electron-accepting ability, which is conducive to the formation of more stable intermediate states in the reaction kinetics, accelerating electron transfer and thus accelerating the reaction rate.
[0026] When the Ni-MOF concentration is 0.5 mg / mL, the nanosheets are unevenly distributed and the sample has obvious accumulation phenomenon;
[0027] When the concentration of Ni-MOF is 1.0 mg / mL, it presents a porous nanoflower structure composed of ordered nanosheets with good dispersion. The smooth surface of the nanosheets has obvious wrinkles, which is conducive to the exposure of more active sites. The porous structure and layered structure are more conducive to electron transfer and electrolyte ion penetration, accelerating the redox kinetics process, thereby improving the specific capacitance of the electrode material.
[0028] When the concentration of Ni-MOF is 2.0-3.0 mg / mL, the layered structure stacking phenomenon is serious, the ordered structure completely disappears, and it appears as a clustered nanoflower structure.
[0029] The invention discloses an application of a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material. When the concentration of Ni-MOF is 1.0 mg / mL, charging and discharging are performed within a voltage window range of 0 to 0.5 V. When the current density is 1 A / g, the specific capacitance is 2500 to 2700 F / g.
[0030] Beneficial effects of the present invention:
[0031] 1. The present invention adopts a two-step hydrothermal reaction and successfully prepares NiMo-LDH / MOF using Ni-MOF as a template. Using Ni-MOF as a template can prevent the self-accumulation of LDHs, expose more active sites, and promote the rapid diffusion of electrolyte ions. In addition, the three-dimensional flower-like structure composed of thin nanosheets shortens the ion / charge transmission distance and is conducive to the redox kinetic process.
[0032] 2. The synergistic effect between the easily stacked LDHs and the highly porous MOFs can significantly increase the specific surface area of the material, and the porous structure of MOFs is not destroyed during the reaction process, which can effectively prevent the volume expansion caused by the redox process from causing structural collapse, thereby improving the stability of the material.
[0033] 3. The preparation method of the present invention has mild reaction conditions, simple method and low cost. The prepared electrode material can achieve high specific capacitance. At 1A / g, the specific capacitance of NiMo-LDH / MOF-1 is 2530F / g and has good rate performance, which is suitable for mass production and large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the SEM image of Example 1.
[0035] Figure 2 These are SEM images of the electrode materials of Comparative Examples 1 to 4.
[0036] Figure 3 This is the EDS mapping diagram of Example 1.
[0037] Figure 4 This is the TEM image of Example 1.
[0038] Figure 5 This is the HRTEM image of Example 1.
[0039] Figure 6 The XRD diagrams of the electrode materials of Examples 1 to 4 and Comparative Examples 1 to 3 are shown.
[0040] Figure 7 FTIR graphs of the electrode materials of Examples 1 to 4 and Comparative Example 1.
[0041] Figure 8 This is the XPS graph of Example 1.
[0042] Fig. 9 The CV graphs at 10 mV / s and the GCD graphs at 1 A / g of the electrode materials of Examples 1 to 4 and Comparative Examples 1 to 3 are shown.
[0043] Fig.10CV graphs of the electrode material of Example 1 at different scan rates and GCD graphs at different current densities.
[0044] Fig.11 Examples 2 to 4 and Comparative Examples 1 to 3 are CV graphs of the electrode materials at different scanning rates and GCD graphs at different current densities, respectively.
[0045] Fig.12 It is a graph showing the specific capacitance retention rate of the electrode materials of Examples 1 to 4 and Comparative Examples 1 to 3 at 1 to 30 A / g.
[0046] Fig.13 The Nyquist plots of the electrode materials of Examples 1 to 4 and Comparative Examples 1 to 3 are shown.
[0047] Fig.14 CV graphs of the asymmetric supercapacitor (NiMo-LDH / MOF-1 / / Active carbon (AC)) prepared in Example 1 at different scan rates.
[0048] Fig.15 This is the GCD diagram of Example 1 under different current densities.
[0049] Fig.16 This is the Ragone diagram of Example 1.
[0050] Fig.17 The graph is the specific capacitance retention and coulombic efficiency at 10 A / g. DETAILED DESCRIPTION
[0051] The present invention will be further described in detail below in conjunction with the accompanying drawings.
[0052] Example 1
[0053] In the first step, a certain amount of 0.175 mol / L Ni(NO3)2·6H2O and 0.025 mol / L PA are dissolved in 35 mL of N,N-dimethylformamide (DMF), stirred or ultrasonicated at room temperature for 30 min to obtain solution A, and solution A is placed in a polytetrafluoroethylene-lined reactor, reacted at 160°C for 36 h, and the product is washed with DMF several times and placed in a vacuum drying oven to obtain Ni-MOF.
[0054] In the second step, 1 mg / mL Ni-MOF, 0.01 mol / L Na2MoO4·2H2O, and 0.125 mol / L urea were dissolved in deionized water and dispersed at room temperature for 30 minutes to obtain a mixed solution B, which was transferred into a polytetrafluoroethylene reactor lining and reacted for 12 hours at 120°C. After washing with ethanol and deionized water and drying, NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material was obtained. The sample was named NiMo-LDH / MOF-1.
[0055] Example 2
[0056] The other conditions remained unchanged, the Ni-MOF concentration was changed to 0.5 mg / mL, and the final sample was named NiMo-LDH / MOF-0.5.
[0057] Example 3
[0058] The other conditions remained unchanged, the Ni-MOF concentration was changed to 2.0 mg / mL, and the final sample was named NiMo-LDH / MOF-2.
[0059] Example 4
[0060] The other conditions remained unchanged, the Ni-MOF concentration was changed to 3.0 mg / mL, and the final sample was named NiMo-LDH / MOF-3.
[0061] Comparative Example 1
[0062] A method for preparing a Ni-MOF material is exactly the same as the first step in Example 1.
[0063] Comparative Example 2
[0064] Preparation of NiMo-LDH material: 0.35 mol / L Ni(CH3COO)2·4H2O, 0.005 mol / L (NH4)6Mo7O 24 ·4H2O and 0.13mol / L urea were dissolved in deionized water, and the obtained solution was transferred into a polytetrafluoroethylene reactor lining, and reacted at 120°C for 3h. After washing with ethanol and water, the solution was vacuum dried at 60°C for 12h to obtain NiMo-LDH.
[0065] Comparative Example 3
[0066] Preparation of Mo-MOF materials: 0.01 mol / L imidazole and 0.01 mol / L MoO3 were dissolved in methanol solution (V 甲醇 / V H2O =3 / 2), stirred at room temperature for 12 h, the product was washed three times by centrifugation, and dried to obtain Mo-MOF.
[0067] 1. Morphology and structure characterization analysis
[0068] (I) SEM and TEM analysis
[0069] The microscopic morphology of NiMo-LDH / MOF-1 of Example 1, NiMo-LDH / MOF-0.5 of Example 2, NiMo-LDH / MOF-2 of Example 3, NiMo-LDH / MOF-3 of Example 4, Ni-MOF of Comparative Example 1, NiMo-LDH of Comparative Example 2, and Mo-MOF of Comparative Example 3 were analyzed by scanning electron microscopy (SEM), as shown in FIG. Figure 1-2 . As can be seen from the figure, Ni-MOF, NiMo-LDH / MOF-0.5, NiMo-LDH / MOF-1, NiMo-LDH / MOF-2, and NiMo-LDH / MOF-3 are three-dimensional nanoflower ball structures composed of nanosheets. With the increase of Ni-MOF concentration, the nanosheet layer gradually becomes thicker. When Ni-MOF is 0.5, 2.0, and 3.0 mg / mL, there is an obvious accumulation phenomenon, and the nanoflower ball structure is destroyed. When Ni-MOF is 1.0 mg / mL, it shows a regular nanoflower ball structure. This three-dimensional flower-like structure is conducive to shortening the ion / charge transfer distance and the redox kinetic process. NiMo-LDH mainly presents a loose nanoflower structure, and there is no obvious lamellar structure accumulation phenomenon. Mo-MOF is composed of nanorods of varying lengths and smooth surfaces.
[0070] Transmission electron microscopy (TEM), high resolution transmission electron microscopy (HRTEM) and energy spectrum (EDX mapping) were used to analyze the microstructure and element distribution of NiMo-LDH / MOF-1 in Example 1, as shown in the figure. Figure 3 to Figure 5 .from Figure 3 It can be seen that the Ni, Mo, and O elements are evenly distributed in Example 1. Figure 4 It can be clearly seen that the flower ball structure is composed of some irregular nanosheets. Figure 5 It can be seen that the HRTEM image of Example 1 shows interlayer spacings of 0.198, 0.206, and 0.229 nm, respectively, which correspond to the (018), (012), and (015) crystal planes of NiMo-LDH. The results prove the presence of a clear NiMo-LDH crystal structure in the sample.
[0071] (ii) XRD and FTIR analysis
[0072] The crystal structures of NiMo-LDH / MOF-1 of Example 1, NiMo-LDH / MOF-0.5 of Example 2, NiMo-LDH / MOF-2 of Example 3, NiMo-LDH / MOF-3 of Example 4, Ni-MOF of Comparative Example 1, NiMo-LDH of Comparative Example 2, and Mo-MOF of Comparative Example 3 were analyzed by X-ray diffraction (XRD), as shown in FIG. Figure 6-7 .from Figure 6 From the XRD diagram of (a), it can be seen that the Ni-MOF of Comparative Example 1 has obvious characteristic peaks, indicating that the increase of Ni 2+ The ratio of PA linker helps to improve the crystallinity of MOF. In addition, Examples 1 to 4 and Comparative Examples 2 to 3 were carefully compared with Ni(OH)2 standard cards (ICCD No. 38-0715). Examples 1 to 4 have obvious diffraction peaks at 2θ of about 12.8°, 26.0°, 33.5°, 36.2°, and 48.1°, respectively, corresponding to the (003), (006), (012), (015), and (110) crystal planes of NiMo-LDH. Figure 6 (b) It can be seen that the NiMo-LDH of Comparative Example 2 has obvious characteristic peaks at 2θ of about 10.4°, 27.8°, 34.2°, and 60.5°, corresponding to the (003), (006), (012), and (110) crystal planes. At the same time, the sharp peak of Mo-MOF of Comparative Example 3 at 26.6° corresponds to the (011) crystal plane of monoclinic MoO2 (ICCD No. 32-0671). The above results show that Examples 1 to 4 and Comparative Examples 1 to 3 were successfully prepared.
[0073] At the same time, FTIR tests were performed on Examples 1 to 4 and Comparative Example 1. Figure 7 As shown, at 3483.5cm -1 The broad peak at is related to the OH stretching vibration of -OH, which is due to the stretching vibration of water molecules and -OH groups between the LDHs layers. These -OH groups help to balance the positive charges within the skeleton layer (Ni 2+ and Mo 6+ ). At about 2167.3, 1383.5cm -1 The peaks at 1653.3 and 1299.2 cm -1 The peak at 660.5 cm may be related to C=C and CO stretching vibration. -1 The peaks appearing at are mainly related to the vibration and stretching vibration of MO, MOM and OMO bonds. These results further indicate that Examples 1 to 4 and Comparative Example 1 were successfully prepared.
[0074] (III) XPS analysis
[0075] The surface composition and valence state of NiMo-LDH / MOF-1 of Example 1 were analyzed by X-ray photoelectron spectroscopy (XPS). Figure 8 As shown in (a), it shows that NiMo-LDH / MOF-1 of Example 1 contains Ni, Mo and O elements. This result is consistent with the EDXmapping analysis result. Figure 8 As shown in (b), the Ni 2p fine spectrum of NiMo-LDH / MOF-1 has two main peaks at 855.69 and 873.33 eV, which are respectively related to the Ni 2p 3 / 2 and Ni 2p 1 / 2 Consistently, there are two satellite peaks at 861.55 and 879.41 eV. The peaks at 855.64 and 873.14 eV are attributed to the Ni-O bonds of Ni-MOF, and the peaks at 857.49 and 874.95 are attributed to the Ni-OH bonds in the hydroxide. Figure 8 In (c), the fine spectrum binding energy of Mo 3d has two peaks at 232.16 and 235.25 eV, corresponding to Mo 3d 3 / 2 and Mo 3d 5 / 2 The binding energy difference between the two peaks is about 3 eV, indicating that the Mo element in NiMo-LDH / MOF-1 is mainly in the form of Mo 6+ exists in the form of. Figure 8 (d) It can be seen that O 1s can be fitted into two peaks. The peak at 530.93 eV can be attributed to the MO bond in the metal oxide or hydroxide, while the peak at 531.60 eV is attributed to the water molecules adsorbed on the sample surface.
[0076] 2. Electrochemical performance test
[0077] Figures 9 to 11 The electrochemical performance diagrams (cyclic voltammetry (cyclic voltammetry, CV), galvanostatic charge / discharge (constant current charge and discharge, GCD) and electrochemical impedance spectroscopy (electrochemical impedance, EIS)) of the samples of NiMo-LDH / MOF-1 of Example 1, NiMo-LDH / MOF-0.5 of Example 2, NiMo-LDH / MOF-2 of Example 3, NiMo-LDH / MOF-3 of Example 4, Ni-MOF of Comparative Example 1, NiMo-LDH of Comparative Example 2, and Mo-MOF of Comparative Example 3 were tested by a three-electrode device at room temperature.
[0078] Fig. 9(a) is a CV comparison diagram of the embodiment and the comparative example under the voltage window of 0-0.60V (vs Hg / HgO). It can be seen from the figure that different samples have obvious oxidation / reduction peaks, indicating that reversible redox reactions occur on the electrode surface, reflecting the pseudocapacitive characteristics of the samples. Compared with other comparative examples, NiMo-LDH / MOF-1 has a larger CV integral area, indicating that it has higher charge storage capacity and electrochemical reaction activity. In addition, the potential difference between the redox peaks of NiMo-LDH / MOF-1 is smaller than that of other samples, indicating that it has better conductivity and better reversibility. Fig. 9 As shown in (b), at 1 A / g, the specific capacitances of Examples 1 to 4 and Comparative Examples 1 to 3 are 2516, 1524, 2103.3, 1646, 1484, 1003.8 and 373.8 F / g, respectively. The CV and GCD curves of Examples 1 to 4 and Comparative Examples 1 to 3 at different scan rates and current densities are shown in Figure 10-11 As shown. All GCD diagrams show near symmetry and charge-discharge platforms, further demonstrating good reversibility and fast Faraday redox reactions. The specific capacitance of NiMo-LDH / MOF-1 is much greater than that of the comparative example, which indicates that the regular flower ball-like morphology helps to produce more concentrated active sites, further increasing the contact area between the electrolyte and the electrode. From the CV diagram, it can be seen that with the increase in scan rate, the effect of polarization causes the oxidation peak to move upward to a higher potential, while the reduction peak moves downward to a lower potential. The CV integrated area increases with the increase in scan rate, indicating that the charge storage mechanism has changed, gradually shifting towards intercalation and surface redox pseudocapacitance, and this change helps to improve the rate capability. In addition, at a current density of 1 to 30 A / g, the specific capacitance retention rates of Examples 1 to 4 and Comparative Examples 1 to 3 are 45.31, 48.84, 41.65, 52.13, 51.35, 50.81 and 28.89%, respectively. Fig.12 ), indicating that the NiMo-LDH / MOF-1 of Example 1 also has good charge and discharge capabilities.
[0079] EIS spectrum ( Fig.13 ) provides information about charge transfer pathways, phase transitions, and electrode conductivity. In the low-frequency range, the EIS curve of the NiMo-LDH / MOF-1 electrode of Example 1 is relatively steep, indicating that it has a good electron migration rate. In the high-frequency region, the Rs of Examples 1 to 4 and Comparative Examples 1 to 3 are 0.66, 0.84, 0.76, 0.85, 0.73, 0.74, and 0.58, respectively. Example 1 has a smaller Rs value, indicating that the resistance between its electrode and the electrolyte is the smallest, which is conducive to electrolyte ion diffusion.
[0080] 3. Asymmetric supercapacitor
[0081] Figure 14 to Figure 17 The charge storage performance of the asymmetric supercapacitor. In order to evaluate the practical application potential of the material, a NiMo-LDH / MOF-1 / / AC asymmetric supercapacitor was constructed using the NiMo-LDH / MOF-1 of Example 1 as the positive electrode, AC (Active carbon) as the negative electrode, and 6M KOH solution as the electrolyte. Fig.14 The CV curves of supercapacitors under different voltage windows are shown in Figure 2. The CV curves show an approximate rectangle and redox peaks, indicating that its capacitance behavior is a combination of double-layer capacitance and redox reaction. Fig.15 As shown, the NiMo-LDH / MOF-1 / / AC device presents an almost symmetrical GCD contour curve, indicating that it has good electrochemical reversibility and excellent stability. According to the specific capacitance formula, at different current densities, the specific capacitance of the NiMo-LDH / MOF-1 / / AC asymmetric supercapacitor is 164.9, 127.1, 107, 93.7, 86.7, 76.4 and 72.6 F / g (1, 2, 4, 6, 8, 10, 15 A / g), and the retention rate reaches 44.03% (1-15 A / g), indicating its good rate performance. Ragone diagram ( Fig.16 ) shows the relationship between energy and power density. The NiMo-LDH / MOF-1 / / AC asymmetric supercapacitor has a maximum energy density of 58.62Wh / kg at a power density of 800W / kg, and an energy density of 30.83Wh / kg at a maximum power density of 6400W / kg, further demonstrating its good energy storage capacity. Cyclic stability is an important indicator for measuring the performance of supercapacitors. After 9000 cycles at a current density of 10A / g, the device retained a capacitance of 83.8% and had a Coulombic efficiency of 100% throughout the process, indicating that it has good cycling performance ( Fig.17 ).
[0082] In summary, a three-dimensional flower-shaped NiMo-LDH / MOF-1 composed of thin nanosheets was prepared by a two-step hydrothermal method. The thin nanosheet structure enables it to expose more active sites, and the multi-metal synergistic effect and abundant unsaturated coordinated metal sites provide abundant electron transfer paths. This study shows that adding highly active metal nodes is an effective strategy to improve the conductivity, cycle stability and increase active sites of LDHs materials.
[0083] The present invention belongs to the technical field of electrode materials for energy storage devices. The present invention uses MOFs as a template and prepares NiMo-LDH through an in-situ reaction, which can not only effectively avoid LDHs self-accumulation, but also the larger specific surface area of MOFs can effectively improve the ability to adsorb ions from the electrolyte, and through the synergistic effect between the two, a high specific capacitance is achieved. The preparation of NiMo-LDH / MOF material specifically includes the following steps: first, using Ni(NO3)2·6H2O and PA as raw materials to prepare a flower ball-shaped Ni-MOF template, and then using Na2MoO4·2H2O and urea as raw materials to prepare NiMo-LDH / MOF. The present invention has simple steps and low cost. The prepared NiMo-LDH / MOF electrode with a flower-like structure composed of two-dimensional nanosheets has excellent electrochemical properties. At a current density of 1A / g, the specific capacitance can reach 2530F / g. The assembled NiMo-LDH / MOF-1 / / AC asymmetric supercapacitor has a power density of 800W / kg and an energy density of 58.62Wh / kg. As a supercapacitor positive electrode material, it has great application potential.
Claims
1. A method for preparing a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material, It is characterized in that The steps include: Step 1: Take a certain amount of nickel salt and ligand and dissolve them in N,N-dimethylformamide (DMF); Stir or ultrasonicate at room temperature to obtain solution A, place solution A in a polytetrafluoroethylene liner for hydrothermal reaction to obtain a product, wash the product with DMF for multiple times, and place it in a vacuum drying oven to obtain Ni-MOF; Step 2: Dissolve the Ni-MOF, molybdenum salt and urea in deionized water; disperse them at room temperature to obtain a mixed solution B, transfer them into a polytetrafluoroethylene reactor lining for hydrothermal reaction, wash them with ethanol and water, and dry them to obtain a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material.
2. The method for preparing a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material according to claim 1, It is characterized in that In the above step 1, the molar concentrations of nickel salt and ligand in the obtained solution are controlled to be 0.155-0.225 mol / L and 0.015-0.125 mol / L, respectively. Solution A is placed in a polytetrafluoroethylene liner and reacted under hydrothermal conditions at 140-200° C. for 24-48 hours. The product is washed with DMF several times.
3. The method for preparing a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material according to claim 1, It is characterized in that The nickel salt is NiCl 2 6H 2 O.Ni(NO 3 ) 2 6H 2 O.Ni(CH 3 COO 2 ·4H 2 O or NiSO 4 6H 2 One of O; The ligand is one of pyromellitic acid (PA), terephthalic acid (TPA) or tetrafluoroterephthalic acid.
4. The method for preparing a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material according to claim 1, It is characterized in that In the above step 2, the concentrations of Ni-MOF, molybdenum salt and urea in the solution are controlled to be 0.5-3.0 mg / mL, 0.008-0.02 mol / L and 0.122-0.215 mol / L, respectively, and the reaction is carried out at 100-160° C. hydrothermal conditions for 10-16 hours.
5. The method for preparing a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material according to claim 1, It is characterized in that The molybdenum salt is specifically Na 2 MoO 4 ·2H 2 O.C 10 H 14 MoO 6 (Molybdenum acetylacetonate) or (NH 4 ) 6 Mo 7 O 24 ·4H 2 One of O.
6. The method for preparing a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material according to claim 1, It is characterized in that In the above preparation method, after the hydrothermal reaction is completed, the drying temperature is 50-60°C.
7. The method for preparing a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material according to claim 1, It is characterized in that In the above step 1, the filling degree in the polytetrafluoroethylene liner is preferably 40-60%.
8. A NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material prepared by the method according to any one of claims 1 to 7, It is characterized in that Nickel ions, molybdenum ions combine with hydroxide ions to form a layered structure, and anions are inserted between the layers to balance the charge; The synergistic effect between the easily stacked LDHs and the highly porous MOFs significantly increases the specific surface area of the material; The three-dimensional flower-like structure composed of thin nanosheets increases the surface area of the electrode material, shortens the ion / charge transmission distance and is conducive to the redox kinetic process; in addition, the porous channels and abundant pores in the three-dimensional flower-like structure help to reduce the impedance of the electrochemical process, reduce the resistance of ions and electrons in the transmission process, and accelerate the electrochemical process; The Mo element in NiMo-LDH / MOF is Mo 6+ In NiMo-LDH / MOF, Mo element exists in the form of Mo 6+ exists in the form of.
9. The NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material according to claim 8, It is characterized in that When the Ni-MOF concentration is 0.5 mg / mL, the nanosheets are unevenly distributed and the sample has obvious accumulation phenomenon; When the concentration of Ni-MOF is 1.0 mg / mL, it presents a porous nanoflower structure composed of ordered nanosheets with good dispersion. The smooth surface of the nanosheets has obvious wrinkles, which is conducive to the exposure of more active sites. The porous structure and layered structure are more conducive to electron transfer and electrolyte ion penetration, accelerating the redox kinetics process, thereby improving the specific capacitance of the electrode material. When the concentration of Ni-MOF is 2.0-3.0 mg / mL, the layered structure stacking phenomenon is serious, the ordered structure completely disappears, and it appears as a clustered nanoflower structure.
10. Application of a NiMo-LDH / MOF high specific capacitance supercapacitor positive electrode material prepared by the method according to any one of claims 1 to 7, It is characterized in that When the concentration of Ni-MOF is 1.0 mg / mL, charging and discharging are carried out in the voltage window range of 0 to 0.5 V, and the specific capacitance is 2500 to 2700 F / g at a current density of 1 A / g.