Preparation method of solar cell and solar cell
By combining laser bombardment and alkaline solution etching techniques, the problem of etching uniformity in the non-metallic contact area of solar cells has been solved, thereby improving etching uniformity and cell performance.
Patent Information
- Application Number
- CN202411040559.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
In existing technologies, it is difficult to guarantee the etching uniformity of solar cells in the non-metallic contact area, which affects cell performance.
Laser bombardment is used to improve the surface roughness of the non-metallic contact area and form a first silicon oxide layer on it. Combined with alkaline solution etching, a patterned mask is formed to cover the metallic contact area, ensuring etching uniformity.
By combining laser bombardment and alkaline solution etching, the etching uniformity of the non-metallic contact area is improved, parasitic absorption is reduced, and the short-circuit current and overall performance of the solar cell are enhanced.
Smart Images

Figure CN118983369A_ABST
Abstract
Description
Technical Field
[0001] The present application mainly relates to the field of photovoltaic technology, and in particular to a method for preparing a solar cell and a solar cell. Background Art
[0002] TOPcon cells use a tunneling layer and a doped polysilicon layer to form a passivation contact, which can effectively reduce surface recombination and metal contact recombination. The thicker doped polysilicon layer at the metal contact and the thinner doped polysilicon layer at the non-metallic contact area can avoid contact between the electrode and the silicon substrate and reduce parasitic absorption. When thinning the doped polysilicon layer at the non-metallic contact area, how to improve etching uniformity is one of the important research directions in this field. Summary of the invention
[0003] The technical problem to be solved by the present application is to provide a method for preparing a solar cell and a solar cell. The method for preparing a solar cell can improve the etching uniformity of a doped polysilicon layer at a non-metallic contact area.
[0004] To solve the above technical problems, the present application provides a method for preparing a solar cell, comprising: providing a silicon substrate; sequentially forming a tunneling layer and a doped polysilicon layer on the front and / or back side of the silicon substrate, the doped polysilicon layer comprising adjacent metal contact areas and non-metal contact areas; forming a mask on a side of the doped polysilicon layer away from the silicon substrate, the mask covering the metal contact areas and exposing the non-metal contact areas; bombarding the non-metal contact areas with a laser; etching the non-metal contact areas after laser bombardment with an alkaline solution; and forming electrodes in the metal contact areas, the electrodes being electrically connected to the doped polysilicon layer.
[0005] In one embodiment of the present application, the steps of forming the tunneling layer and the doped polysilicon layer include: forming a tunneling layer and an intrinsic silicon layer in sequence on the silicon substrate; doping the intrinsic silicon layer to form the doped polysilicon layer, and forming a glass layer on a side of the doped polysilicon layer away from the silicon substrate.
[0006] In one embodiment of the present application, the method for forming the mask includes: using an anti-etchant to cover the glass layer located at the metal contact area; etching and removing the glass layer not covered by the anti-etchant to form a patterned glass layer, and the patterned glass layer serves as the mask.
[0007] In an embodiment of the present application, the laser bombardment increases the surface roughness of the non-metallic contact area and forms a first silicon oxide layer on the non-metallic contact area.
[0008] In one embodiment of the present application, the method for preparing a solar cell further includes: forming a passivation layer on a surface of the doped polysilicon layer facing away from the silicon substrate, the passivation layer including one or more layers of an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer.
[0009] In one embodiment of the present application, before forming the tunneling layer and the doped polysilicon layer, it also includes: forming a second silicon oxide layer on the front and back sides of the silicon substrate; removing the second silicon oxide layer on the front or back side of the silicon substrate; and forming the tunneling layer and the doped polysilicon layer on the side not covered by the second silicon oxide layer.
[0010] In one embodiment of the present application, after the step of etching the non-metallic contact area after laser bombardment using an alkaline solution, the method further includes: removing the mask and the second silicon oxide layer.
[0011] In one embodiment of the present application, before the step of forming the second silicon oxide layer, it also includes: performing a texturing treatment on the front and back sides of the silicon substrate, and after the step of removing the second silicon oxide layer on the front or back side of the silicon substrate, it also includes: polishing the side not covered by the second silicon oxide layer.
[0012] In an embodiment of the present application, the alkaline solution does not completely etch and remove the doped polysilicon layer at the non-metallic contact area.
[0013] On the other hand, the present application further provides a solar cell, which is prepared by the preparation method as described above.
[0014] Compared with the prior art, the present application has the following advantages: thanks to the laser bombardment, the surface roughness of the non-metallic contact area is improved, the contact area between the non-metallic contact area and the alkaline solution is larger, and at the same time, the first silicon oxide layer formed on the non-metallic contact area by laser bombardment has a higher wettability. Therefore, the reaction between the non-metallic contact area and the alkaline solution is more uniform, thereby improving the thickness uniformity of the non-metallic contact area after etching. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The accompanying drawings are included to provide a further understanding of the present application. They are included and constitute a part of the present application. The accompanying drawings illustrate embodiments of the present application and together with the present specification serve to explain the principles of the present application. In the accompanying drawings:
[0016] Figure 1 is a schematic flow chart of a method for preparing a solar cell in one embodiment of the present application;
[0017] Figures 2 to 9 It is a schematic cross-sectional view of a solar cell in different steps of a method for preparing a solar cell.
[0018] Reference numerals
[0019] Silicon substrate 210 Non-metal contact region 232 Second silicon oxide layer 290
[0020] Front surface 211 Intrinsic silicon layer 240 Electrode 310
[0021] Back side 212 Glass layer 250 Aluminum oxide layer 320
[0022] Tunneling layer 220 Mask 260 Silicon oxynitride layer 330
[0023] Doped polysilicon layer 230 Anti-etching agent 270
[0024] Metal contact region 231 First silicon oxide layer 280 DETAILED DESCRIPTION
[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios based on these drawings without creative work. Unless it is obvious from the language environment or otherwise explained, the same reference numerals in the figures represent the same structure or operation.
[0026] As shown in this application and claims, unless the context clearly indicates an exception, the words "a", "an", "an" and / or "the" do not refer to the singular and may also include the plural. Generally speaking, the terms "include" and "comprise" only indicate the inclusion of the steps and elements that have been clearly identified, and these steps and elements do not constitute an exclusive list. The method or device may also include other steps or elements.
[0027] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values of the parts and steps set forth in these embodiments do not limit the scope of the present application. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, method and equipment known to those of ordinary skill in the relevant field may not be discussed in detail, but in appropriate cases, the technology, method and equipment should be considered as a part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so that once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.
[0028] In the description of the present application, it should be understood that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing the present application and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction, and therefore cannot be understood as limiting the scope of protection of the present application; the directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.
[0029] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.
[0030] In addition, it should be noted that the use of words such as "first" and "second" to define components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above words have no special meaning and cannot be understood as limiting the scope of protection of this application. In addition, although the terms used in this application are selected from well-known and commonly used terms, some terms mentioned in the specification of this application may be selected by the applicant at his or her discretion, and their detailed meanings are explained in the relevant parts of the description of this article. In addition, it is required to understand this application not only by the actual terms used, but also by the meaning implied by each term.
[0031] Flowcharts are used in the present application to illustrate the operations performed by the system according to the embodiments of the present application. It should be understood that the preceding or following operations are not necessarily performed accurately in order. On the contrary, various steps may be processed in reverse order or simultaneously. At the same time, other operations may be added to these processes, or one or more operations may be removed from these processes.
[0032] Next, the preparation method of the solar cell and the solar cell of the present application are described through examples.
[0033] refer to Figure 1 A schematic flow chart of a method for preparing a solar cell in one embodiment of the present invention, wherein the method for preparing a solar cell in this embodiment comprises the following steps:
[0034] Step S110: providing a silicon substrate;
[0035] Step S120: sequentially forming a tunneling layer and a doped polysilicon layer on the front side and / or the back side of the silicon substrate, wherein the doped polysilicon layer includes adjacent metal contact regions and non-metal contact regions;
[0036] Step S130: forming a mask on a surface of the doped polysilicon layer away from the silicon substrate, wherein the mask covers the metal contact area and exposes the non-metal contact area;
[0037] Step S140: bombarding the non-metallic contact area with laser;
[0038] Step S150: etching the non-metallic contact area after laser bombardment using an alkaline solution;
[0039] Step S160: forming an electrode in the metal contact region, wherein the electrode is electrically connected to the doped polysilicon layer.
[0040] Next, steps S110 to S160 are described in detail.
[0041] refer to Figures 2 to 4 As shown, in step S110, a silicon substrate 210 is provided. The silicon substrate 210 can be N-type doped single crystal silicon or P-type doped single crystal silicon. The silicon substrate 210 has a front side 211 and a back side 212 opposite to each other in the thickness direction thereof. When the solar cell is working, the front side 211 faces the sun.
[0042] In step S120, a tunneling layer 220 and a doped polysilicon layer 230 are sequentially formed on the back surface 212. It should be noted that the tunneling layer 220 and the doped polysilicon layer 230 may be formed on the front surface 211 alone, or may be formed on the front surface 211 and the back surface 212 at the same time. The method for preparing the solar cell of the present application is described below by taking the formation of the tunneling layer 220 and the doped polysilicon layer 230 on the back surface 212 as an example.
[0043] The doped polysilicon layer 230 may be an N-type doped polysilicon layer or a P-type doped polysilicon layer, and the doping type of the doped polysilicon layer 230 may be the same as that of the silicon substrate 210 or may be opposite to that of the silicon substrate 210. The doped polysilicon layer 230 includes adjacent metal contact regions 231 and non-metal contact regions 232, and the electrode formed in the subsequent steps is located in the metal contact region 231.
[0044] In one embodiment, the steps of forming the tunneling layer 220 and the doped polysilicon layer 230 include: sequentially forming a tunneling layer and an intrinsic silicon layer on a silicon substrate; doping the intrinsic silicon layer to form a doped polysilicon layer, and forming a glass layer on a side of the doped polysilicon layer away from the silicon substrate. Figure 2 and Figure 3 As shown, a tunneling layer 220 and an intrinsic silicon layer 240 are sequentially formed on the front surface 211. The intrinsic silicon layer 240 may be intrinsic amorphous silicon or intrinsic polycrystalline silicon. The intrinsic silicon layer 240 may be formed using a low pressure chemical vapor deposition (LPCVD) process. Figure 3 and Figure 4 As described above, the intrinsic silicon layer 240 is doped to form a doped polysilicon layer 230, and a glass layer 250 is formed on a side of the doped polysilicon layer 230 away from the silicon substrate 210. When the doping element in the doped polysilicon layer 230 is phosphorus (P), the glass layer 250 is phosphorus silicon glass (PSG), and when the doping element in the doped polysilicon layer 230 is boron (B), the glass layer 250 is borosilicate glass (BSG). The thickness of the glass layer 250 can be 35nm to 75nm, for example, 35nm, 45nm, 55nm, 65nm or 75nm.
[0045] In one embodiment, before forming the tunneling layer and the doped polysilicon layer, the following steps 1 to 3 are also included:
[0046] Step 1: Reference Figure 2 As shown, a second silicon oxide layer 290 is formed on the front surface 211 and the back surface 212 .
[0047] Step 2: Reference Figure 3 As shown, the second silicon oxide layer 290 on the back side 212 is removed, and the second silicon oxide layer 290 on the front side 211 is retained. The second silicon oxide layer 290 on the front side 211 can protect the front side 211 from being etched in subsequent steps. It should be noted that if the tunneling layer and the doped polysilicon layer are formed on the front side 211, the second silicon oxide layer 290 on the back side 212 needs to be removed.
[0048] Step three: forming a tunneling layer and a doped polysilicon layer on the side not covered by the second silicon oxide layer 290 (ie, the back side 212 ).
[0049] In one embodiment, before the step of forming the second silicon oxide layer 290, the step further includes: performing a texturing process on the front surface 211 and the back surface 212. After removing the second silicon oxide layer 290 on the front surface 211 or the back surface 212, the step further includes: performing a polishing process on the side not covered by the second silicon oxide layer 290. The texturing process can form a pyramid velvet morphology, thereby reducing the reflection of light by the battery.
[0050] refer to Figure 4 and Figure 5 As shown, in step S130 , a mask 260 is formed on a surface of the doped polysilicon layer 230 away from the silicon substrate 210 , and the mask 260 covers the metal contact region 231 and exposes the non-metal contact region 232 .
[0051] In one embodiment, the mask 260 may be formed by the following method steps: using an etchant to cover the glass layer at the metal contact region, and etching away the glass layer not covered by the etchant. Figure 4 As shown, the glass layer 250 at the metal contact area 231 is covered with an anti-etching agent 270, and the glass layer 250 at the non-metal contact area 232 is not covered; Figure 5 As shown, the glass layer 250 not covered by the anti-etching agent 270 (i.e., the glass layer 250 at the non-metal contact area 232) is etched away to form a patterned glass layer, and the patterned glass layer serves as a mask 260. The anti-etching agent 270 can be an ink resistant to hydrofluoric acid corrosion, and a solution containing hydrofluoric acid can be used to etch away the glass layer 250 at the non-metal contact area 232. Figure 5 As shown, the mask 260 covers the metal contact region 231 and exposes the non-metal contact region 232 .
[0052] In one embodiment, after the mask 260 is formed, the resist 270 is removed.
[0053] refer to Figure 5 and Figure 6 As shown, in step S140, laser bombardment is used to bombard the non-metallic contact area 232. The laser bombardment improves the surface roughness of the non-metallic contact area 232 on the one hand, and heats the non-metallic contact area 232 on the other hand, so that the non-metallic contact area 232 with a certain thickness reacts with oxygen to generate a first silicon oxide layer 280, and the first silicon oxide layer 280 covers the non-metallic contact area 232. The thickness of the first silicon oxide layer 280 can be 2nm to 3nm, for example, the thickness is 2nm, 2.5nm or 3nm.
[0054] refer to Figure 6 and Figure 7 As shown, in step S150, an alkaline solution is used to etch the non-metallic contact area 232 after laser bombardment. Figure 7 In the embodiment, after being etched by the alkaline solution, the non-metallic contact region 232 is thinned, and the thickness of the non-metallic contact region 232 is less than the thickness of the metal contact region 231. In some other embodiments, after being etched by the alkaline solution, the non-metallic contact region 232 is completely etched away. Thinning or removing the non-metallic contact region 232 can reduce the parasitic absorption caused by the non-metallic contact region 232 and increase the short-circuit current of the battery.
[0055] Thanks to the laser bombardment, the surface roughness of the non-metallic contact area 232 is improved, the contact area between the non-metallic contact area 232 and the alkaline solution is larger, and the first silicon oxide layer 280 located on the non-metallic contact area 232 has a higher wettability, so the reaction between the non-metallic contact area 232 and the alkaline solution is more uniform, thereby improving the thickness uniformity of the non-metallic contact area 232 after etching. The thickness uniformity of the non-metallic contact area 232 of the solar cell prepared by the method for preparing a solar cell of the present application can reach 5%.
[0056] refer to Figure 7 and Figure 8 As shown, in one embodiment, after etching the non-metal contact region 232 after laser bombardment using an alkaline solution, the process further includes: removing the mask 260 and the second silicon oxide layer 290 .
[0057] refer to Fig. 9 As described above, in step S160 , an electrode 310 is formed in the metal contact region 231 , and the electrode 310 is electrically connected to the doped polysilicon layer 230 .
[0058] refer to Figure 8 and Fig. 9 As shown, in one embodiment, the method for preparing a solar cell further includes: forming a passivation layer on a side of the doped polysilicon layer 230 facing away from the silicon substrate 210, the passivation layer including one or more layers of an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer; Fig. 9 In the embodiment, the passivation layer includes an aluminum oxide layer 320 and a silicon oxynitride layer 330. The electrode 310 penetrates the aluminum oxide layer 320 and the silicon oxynitride layer 330 and contacts the doped polysilicon layer 230.
[0059] On the other hand, the present application also provides a solar cell, which is prepared by the preparation method as described above.
[0060] The basic concepts have been described above. Obviously, for those skilled in the art, the above application disclosure is only an example and does not constitute a limitation of the present application. Although not explicitly stated herein, those skilled in the art may make various modifications, improvements and amendments to the present application. Such modifications, improvements and amendments are suggested in the present application, so such modifications, improvements and amendments still belong to the spirit and scope of the exemplary embodiments of the present application.
[0061] At the same time, the present application uses specific words to describe the embodiments of the present application. For example, "one embodiment", "an embodiment", and / or "some embodiments" refer to a certain feature, structure or characteristic related to at least one embodiment of the present application. Therefore, it should be emphasized and noted that "one embodiment" or "an embodiment" or "an alternative embodiment" mentioned twice or more in different positions in this specification does not necessarily refer to the same embodiment. In addition, some features, structures or characteristics in one or more embodiments of the present application can be appropriately combined.
[0062] Similarly, it should be noted that in order to simplify the description of the disclosure of this application and thus help understand one or more application embodiments, in the above description of the embodiments of this application, multiple features are sometimes merged into one embodiment, figure or description thereof. However, this disclosure method does not mean that the features required by the object of this application are more than the features mentioned in the claims. In fact, the features of the embodiments are less than all the features of the single embodiment disclosed above.
[0063] In some embodiments, numbers describing the number of components and attributes are used. It should be understood that such numbers used in the description of the embodiments are modified by the modifiers "about", "approximately" or "substantially" in some examples. Unless otherwise specified, "about", "approximately" or "substantially" indicate that the numbers are allowed to vary by ±20%. Accordingly, in some embodiments, the numerical parameters used in the specification and claims are approximate values, which may change according to the required features of individual embodiments. In some embodiments, the numerical parameters should take into account the specified significant digits and adopt the general method of retaining digits. Although the numerical domains and parameters used to confirm the breadth of their range in some embodiments of the present application are approximate values, in specific embodiments, the setting of such numerical values is as accurate as possible within the feasible range.
[0064] Although the present application has been described with reference to the current specific embodiments, ordinary technicians in this technical field should recognize that the above embodiments are only used to illustrate the present application, and various equivalent changes or substitutions may be made without departing from the spirit of the present application. Therefore, as long as the changes and modifications to the above embodiments are within the essential spirit of the present application, they will fall within the scope of the claims of the present application.
Claims
1. A method for preparing a solar cell, characterized in that: include: providing a silicon substrate; forming a tunneling layer and a doped polysilicon layer in sequence on the front side and / or the back side of the silicon substrate, wherein the doped polysilicon layer includes adjacent metal contact areas and non-metal contact areas; forming a mask on a surface of the doped polysilicon layer away from the silicon substrate, wherein the mask covers the metal contact area and exposes the non-metal contact area; bombarding the non-metallic contact area with a laser; Etching the non-metallic contact area after laser bombardment using an alkaline solution; as well as An electrode is formed in the metal contact region, and the electrode is electrically connected to the doped polysilicon layer.
2. The method for preparing a solar cell according to claim 1, characterized in that: The steps of forming the tunneling layer and the doped polysilicon layer include: forming a tunneling layer and an intrinsic silicon layer in sequence on the silicon substrate; The intrinsic silicon layer is doped to form the doped polysilicon layer, and a glass layer is formed on a surface of the doped polysilicon layer away from the silicon substrate.
3. The method for preparing a solar cell according to claim 2, characterized in that: The method of forming the mask comprises: Covering the glass layer at the metal contact area with an etchant; The glass layer not covered by the resist is removed by etching to form a patterned glass layer, and the patterned glass layer serves as the mask.
4. The method for preparing a solar cell according to claim 1, wherein: The laser bombardment increases the surface roughness of the non-metal contact area and forms a first silicon oxide layer on the non-metal contact area.
5. The method for preparing a solar cell according to claim 1, wherein: Also includes: A passivation layer is formed on a side of the doped polysilicon layer facing away from the silicon substrate, wherein the passivation layer includes one or more layers of an aluminum oxide layer, a silicon nitride layer, and a silicon nitride oxide layer.
6. The method for preparing a solar cell according to claim 1, characterized in that: Before forming the tunneling layer and the doped polysilicon layer, the method further includes: forming a second silicon oxide layer on the front and back sides of the silicon substrate; removing the second silicon oxide layer on the front side or the back side of the silicon substrate; The tunneling layer and the doped polysilicon layer are formed on the side not covered by the second silicon oxide layer.
7. The method for preparing a solar cell according to claim 6, characterized in that: After the step of etching the non-metal contact area after laser bombardment with an alkaline solution, the method further includes: removing the mask and the second silicon oxide layer.
8. The method for preparing a solar cell according to claim 6, wherein: Before the step of forming the second silicon oxide layer, the method further includes: performing a texturing process on the front and back sides of the silicon substrate; and after the step of removing the second silicon oxide layer on the front or back sides of the silicon substrate, the method further includes: performing a polishing process on the side not covered by the second silicon oxide layer.
9. The method for preparing a solar cell according to claim 1, wherein: The alkaline solution incompletely etches and removes the doped polysilicon layer at the non-metallic contact area.
10. A solar cell, characterized in that: The solar cell is prepared by the preparation method according to any one of claims 1 to 9.