Battery negative pole piece as well as preparation method and application thereof
By preparing a multilayer porous carbon nanofiber coating with gradually varying electronic conductivity on the surface of a current collector substrate, the problem of uneven deposition of active metals in a three-dimensional framework structure was solved, achieving uniform distribution of active metals and efficient energy storage.
Patent Information
- Application Number
- CN202411182072.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-19
AI Technical Summary
In existing technologies, the slow mass transfer dynamics of three-dimensional framework structures lead to the deposition of active metals on the framework surface, forming dendrites that block internal transport paths and result in low internal utilization.
A multilayer porous carbon nanofiber coating with gradually varying electronic conductivity was prepared on the surface of a current collector substrate. By controlling the migration path of active metal ions, they were uniformly deposited within the three-dimensional framework, thus avoiding dendrite formation.
Uniform deposition of active metals was achieved, which improved the structural stability and energy storage efficiency of the battery and reduced volume changes during charging and discharging.
Abstract
Description
Technical Field
[0001] The present invention relates to a technology in the field of battery material processing, specifically a battery negative electrode sheet and a preparation method and application thereof. Background Art
[0002] Metallic lithium has an extremely high theoretical capacity (3680mAh / g) and an ultra-low redox potential (-3.040Vvs.SHE), and is considered to be a very promising negative electrode material. However, the problem of dendrite growth and unlimited volume expansion seriously hinders its practical application, and other active metal negative electrodes have the same problem. To this end, researchers use stable artificial solid electrolyte interfaces, membrane modification design, development of electrolyte additives and solid electrolytes, and construction of three-dimensional skeleton matrices to regulate the deposition / stripping behavior of active metal ions, alleviate volume expansion during the cycle and inhibit dendrite growth. Among them, structured active metal negative electrodes can simultaneously inhibit dendrite growth and volume change. However, when using a three-dimensional skeleton structure as an active metal substrate, due to the slow mass transfer kinetics and extended diffusion path inside the skeleton, the concentration polarization inside the skeleton occurs, and the active metal is more likely to be directly deposited on the skeleton surface. This "top deposition" behavior of the active metal blocks the transmission of metal ions to the inside of the skeleton, resulting in low internal utilization of the porous structure and the formation of metal dendrites at the top.
[0003] In order to solve the above problems in the prior art, the present invention is provided. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention proposes a battery negative electrode plate and a preparation method and application thereof, and adopts a coating process to prepare a three-dimensional porous carbon nanofiber coating with gradually changing electronic conductivity on the surface of a current collector substrate, thereby obtaining a negative electrode plate with stable structure, good working elasticity, and high active metal transport and storage efficiency.
[0005] The first aspect of the present invention relates to a method for preparing a negative electrode sheet of a battery, comprising the following steps:
[0006] A carbon nanofiber dispersion is mixed with an organic polymer solution to prepare at least three coating slurries with different mixing ratios, wherein at least one of the organic polymer solution and the carbon nanofiber dispersion contains a pore-forming agent; the coating slurries are sequentially layered and coated on the surface of one side of a current collector substrate according to the weight proportion of the carbon nanofibers in the coating slurry, with the coating slurry with the highest carbon nanofiber weight proportion being coated first; thereafter, a drying treatment is performed to remove the solvent and the pore-forming agent, thereby obtaining a battery negative electrode sheet having a multi-layer porous carbon nanofiber coating; the multi-layer porous carbon nanofiber coating is the negative electrode membrane.
[0007] For some specific embodiments, the proportion of the carbon nanofiber dispersion in the coating slurry does not exceed 95wt%, for example, the proportion is 95wt%, 90wt%, 80wt%, 70wt%, 60wt%, 50wt%, 40wt%, 30wt%, 20wt%, 10wt%, 5wt%, 1wt%, etc.
[0008] Preferably, the carbon nanofiber dispersion comprises carbon nanofibers and an organic solvent, and the weight ratio of the carbon nanofibers to the organic solvent is 1:(5-10), for example, the ratio is 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, etc.
[0009] Preferably, the organic polymer solution comprises a binder and an organic solvent, and the weight ratio of the binder to the organic solvent is 1:(5-10), for example, the ratio is 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, etc.
[0010] Preferably, the binder includes at least one of polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), and polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP).
[0011] Preferably, the organic solvent is at least one of dimethylformamide (DMF), dimethylacetamide (DMAc) and acetone, and the organic solvents used in the carbon nanofiber dispersion and the organic polymer solution may be the same or different.
[0012] For some specific embodiments, the pore former is at least one of glycerol, hexane, butanol, and cyclohexanol; preferably, both the carbon nanofiber dispersion and the organic polymer solution include pore formers, so as to better control the porosity and its range as well as the uniformity of pore distribution; further preferably, the weight of the pore former in the carbon nanofiber dispersion is 1 to 2 times the weight of the carbon nanofiber, and the weight of the pore former in the organic polymer solution is 1 to 2 times the weight of the binder.
[0013] For some specific embodiments, the battery negative electrode plate is coated with the organic polymer solution on the porous carbon nanofiber coating, and the organic polymer solution includes the pore-forming agent, which can form a diaphragm after drying, so there is no need to configure an additional diaphragm when making the battery.
[0014] For some specific implementation schemes, the drying process can be performed after each layer of dispersion is applied, or after multiple layers of dispersion are applied together; when multiple layers of dispersion are applied together, there is a high probability that dispersions of different concentrations will mix at the contact interface of two adjacent layers.
[0015] The second aspect of the present invention relates to a battery negative electrode plate, which is manufactured by the above method; the negative electrode film on the battery negative electrode plate has a porosity of 70% to 90%, a pore size of 1 to 5 μm, and a specific surface area of 16 to 20 m 2 / g.
[0016] The third aspect of the present invention relates to an application of the above-mentioned battery negative electrode plate in an alkali metal battery, such as a lithium ion battery, a sodium ion battery, or a potassium ion battery.
[0017] Compared with the prior art, the present invention has the following technical effects:
[0018] 1) The porous carbon nanofiber coating is a multi-layer structure coating; in the multi-layer structure coating, along the thickness direction of the electrode sheet, from the current collector substrate side to the outside (diaphragm direction), the electronic conductivity of the coating gradually decreases, and the electrode potential distribution inside the negative electrode after injecting the electrolyte and applying the electric field is different. The closer to the current collector substrate, the lower the electrode potential, which promotes the active metal ions in the electrolyte to migrate to the inside of the carbon nanofiber three-dimensional skeleton, that is, to the direction close to the current collector substrate. The active metal is first deposited near the current collector, and then deposited outward along the three-dimensional pores in sequence, ensuring the "inside-out" electrodeposition behavior, effectively avoiding the active metal deposition on the outside of the three-dimensional skeleton to form dendrites; moreover, the three-dimensional network skeleton in the coating has a high porosity and a large pore size, and has a large energy storage space, which can ensure that as many active metals as possible are evenly deposited inside the carbon nanofiber layer, so that the volume change of the battery negative electrode during the charge and discharge process is zero;
[0019] 2) Used in lithium, sodium or potassium ion battery negative electrodes, with good electrochemical performance, high active metal storage efficiency and stable structure;
[0020] 3) The carbon nanofibers and the binder are made into dispersion and solution respectively and then mixed, which avoids the problem of carbon nanofibers agglomerating locally due to the influence of the binder during direct addition and mixing, thus ensuring the uniformity of each layer of the coating;
[0021] 4) The preparation method is simple, the product consistency is good, the operability is strong, and it has broad commercial application prospects. DETAILED DESCRIPTION
[0022] The present invention is described in detail below in conjunction with specific embodiments. Experimental methods without specific conditions in the examples are carried out according to conventional methods and conditions.
[0023] Add PVDF (Mw=900000) and PEO (Mw=1000000) to a mixed solution of DMF-glycerol, the weight ratio of PVDF, PEO, glycerol and DMF is 1:0.5:1.5:7.5, and stir vigorously at 80°C for 3-4 hours, for example, at a speed of 1500RPM for 3.5 hours to obtain an organic polymer solution A. 100 .
[0024] Add carbon nanofibers (Suzhou First Element Nanotechnology Co., Ltd., CNTp, the same below) into a mixed solution of DMF-glycerol, with a weight ratio of carbon nanofibers, glycerol and DMF being 1:1:5, and ultrasonically disperse for 1 to 4 hours, for example, at a power of 3 kW and a frequency of 20 kHz for 2 hours to obtain a carbon nanofiber dispersion B.
[0025] The organic polymer solution A 100 and carbon nanofiber dispersion B in different weight ratios. For example, 9:1, 8.5:1.5, 8:2, 7:3, 6:4, 5:5, 4:6, 3:7, 2:8, 1:9, 0.5:9.5 are mixed to obtain coating slurries of different concentrations, which are marked as A in turn. 90 B 10 , A 85 B 15 , A 80 B 20 , …, A 20 B 80 , A 10 B 90 , A 05 B 95 .
[0026] Example 1
[0027] Press A 05 B 95 , A 20 B 80 , A 40 B 60 , A 60 B 40 , A 80 B 20 , A 90 B 10 , A 100 The coating slurries are coated on the surface of the current collector substrate copper foil in layers in the order of 100The corresponding coating head slit width is 40 μm, and the remaining coating heads slit width is 20 μm; it is then transferred to a drying room at 100°C to evaporate the solvent DMF and roll it up, and then placed in a 100°C vacuum oven to dry for 12 hours to remove glycerol, thereby obtaining a battery negative electrode sheet with a multi-layer porous carbon nanofiber coating.
[0028] The total thickness of the negative electrode sheet of the battery obtained in this embodiment is 50 μm, and the average porosity is 85.6%; wherein, the total thickness of the active metal host layer composed of the multi-layer porous carbon nanofiber coating is 30 μm, and the thickness of the outermost organic polymer layer is 10 μm.
[0029] Using metallic lithium as the counter electrode and 1 mol / L LiPF6 (EC:DMC=1:1 volume ratio) as the electrolyte, CR2032 button cells were assembled in a glove box filled with argon. Constant current charge and discharge performance tests were performed on the LAND battery test system, with a charge and discharge range of 1.5V to 3.8V. The battery's initial efficiency was 93.2%, and after 500 cycles at 0.01C, the volumetric capacity could still be maintained at 1630.6mAh / cm 3 , with excellent capacity retention rate.
[0030] Example 2
[0031] The difference from Example 1 is that in this embodiment: press A 10 B 90 , A 30 B 70 , A 50 B 50 , A 70 B 30 , A 90 B 10 , A 100 The coating slurries are coated on the surface of the current collector substrate copper foil in layers in the order of 100 The corresponding coating head slit width is 40 μm, and the slit widths of the other coating heads are 25 μm.
[0032] The total thickness of the negative electrode sheet of the battery obtained in this embodiment is 45.6 μm, and the average porosity is 88.5%; among them, the total thickness of the active metal host layer composed of the multi-layer porous carbon nanofiber coating is 25.6 μm, and the thickness of the outermost organic polymer layer is 10 μm.
[0033] Using a metal sodium sheet as the counter electrode and 1 mol / L NaClO4 (EC:DEC=1:1 volume ratio) as the electrolyte, a CR2032 button cell was assembled in an argon-filled glove box. Constant current charge and discharge performance tests were performed on the LAND battery test system, with a charge and discharge range of 0.01V to 3.0V. The battery's initial efficiency was 92.6%, and after 200 cycles at 0.01C, the volumetric capacity was still maintained at 989.2mAh / cm 3 , with excellent capacity retention rate.
[0034] Example 3
[0035] The preparation of the negative electrode of the battery is the same as that in Example 1.
[0036] A positive electrode sheet was prepared using lithium iron phosphate LFP as the positive electrode material. Lithium iron phosphate, polyvinylidene fluoride, and conductive carbon black were added to 35 parts by weight of N-methylpyrrolidone in a ratio of 40 parts by weight, 1.49 parts by weight, and 1.06 parts by weight. After being fully mixed, the mixture was coated, baked, and roll-pressed to obtain a positive electrode sheet.
[0037] The obtained positive electrode sheet was used as the counter electrode, 1 mol / L LiPF6 (EC:DMC=1:1 volume ratio) was used as the electrolyte, and the battery was assembled in a glove box filled with argon. The battery had an initial coulombic efficiency of 93%, and the capacity retention rates of 0.5C and 1C cycles for 100 times were 99.9% and 99.2% respectively, the capacity retention rates of 200 cycles were 99.6% and 98.9%, and the capacity retention rates of 400 cycles were 99.2% and 98.1%.
[0038] It should be emphasized that the above are only preferred embodiments of the present invention and do not limit the present invention in any form. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a negative electrode sheet of a battery, characterized in that: The following steps are involved: A carbon nanofiber dispersion is mixed with an organic polymer solution to prepare at least three coating slurries with different mixing ratios, wherein at least one of the organic polymer solution and the carbon nanofiber dispersion contains a pore-forming agent; the coating slurries are sequentially layered and coated on the surface of one side of a current collector substrate according to the weight proportion of the carbon nanofibers in the coating slurry, with the coating slurry with the highest weight proportion of carbon nanofibers being coated first; and then a drying treatment is performed to remove the solvent and the pore-forming agent, thereby obtaining a battery negative electrode sheet with a multi-layer porous carbon nanofiber coating.
2. The preparation method according to claim 1, characterized in that: The proportion of the carbon nanofiber dispersion in the coating slurry does not exceed 95wt%.
3. The preparation method according to claim 1, characterized in that: The carbon nanofiber dispersion comprises carbon nanofibers and an organic solvent, and the weight ratio of the carbon nanofibers to the organic solvent is 1:(5-10).
4. The preparation method according to claim 1, characterized in that: The organic polymer solution comprises a binder and an organic solvent, and the weight ratio of the binder to the organic solvent is 1:(5-10).
5. The preparation method according to claim 4, characterized in that: The binder includes at least one of polyvinylidene fluoride, polyethylene oxide, and polyvinylidene fluoride-hexafluoropropylene.
6. The preparation method according to claim 3 or 4, characterized in that: The organic solvent is at least one of dimethylformamide, dimethylacetamide and acetone.
7. The preparation method according to claim 1, characterized in that: The pore former is at least one of glycerol, hexane, butanol and cyclohexanol; preferably, the weight of the pore former in the carbon nanofiber dispersion is 1 to 2 times the weight of the carbon nanofiber, and the weight of the pore former in the organic polymer solution is 1 to 2 times the weight of the binder.
8. The preparation method according to claim 1, characterized in that: The battery negative electrode plate is coated with the organic polymer solution on the porous carbon nanofiber coating, and the organic polymer solution includes the pore-forming agent, and can form a diaphragm after drying.
9. A battery negative electrode plate, characterized in that: The preparation method according to claim 1 to 8 is used; the negative electrode film on the negative electrode sheet of the battery has a porosity of 70% to 90%, a pore size of 1 to 5 μm, and a specific surface area of 16 to 20 m 2 / g.
10. Use of the battery negative electrode sheet according to claim 9 in an alkali metal battery.
Citation Information
Cited By
Electrode composite material and pre-metallization method thereof, pre-metallized electrode complex and metal battery
CN121355188A