Carbon-coated chromium-based bimetallic selenide as well as preparation method and application thereof
By synthesizing a carbon cladding on bimetallic selenide, the volume expansion problem in lithium-ion batteries is solved, high specific capacity and excellent electrochemical performance are achieved, and cycling stability is significantly improved.
Patent Information
- Application Number
- CN202410898228.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-19
AI Technical Summary
The application of bimetallic selenide in lithium-ion batteries is caused by the problem of reduced specific capacity and poor circulation stability caused by volume expansion.
采用碳包覆铬基双金属硒化物,通过水热反应和高温固相硒化反应合成,形成碳包覆的铬基双金属硒化物,利用碳层缓冲体积膨胀并提高电化学性能。
It achieves high specific capacity and excellent rate performance in lithium-ion batteries, maintains the structural integrity of the material, and significantly improves the cycle stability.
Smart Images

Figure CN118983401A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of negative electrode materials for metal ion batteries, and in particular to a carbon-coated chromium-based bimetallic selenide and a preparation method and application thereof. Background Art
[0002] It is an inevitable trend for clean energy to replace traditional energy. The rational development and utilization of renewable clean energy resources such as hydropower, wind power, and biomass energy are in line with the trajectory of energy development and play a significant role in establishing a sustainable energy system, promoting national economic development, and protecting the environment. In recent years, energy companies have entered the field of new energy, among which lithium-ion batteries are an important direction for the application and development of new energy. As one of the important components of lithium-ion batteries, the performance of the negative electrode has an important influence on the overall indicators of the battery. Therefore, how to give full play to the theoretical energy density and stability of the material at the negative electrode level is an important research direction.
[0003] Conversion materials include oxide materials, sulfide materials, selenide materials, and phosphide materials. Among them, metal selenides have higher theoretical specific capacity than metal oxides and metal sulfides, and are therefore considered to be promising candidate negative electrode materials. In particular, bimetallic selenides can effectively improve the electrochemical properties of materials due to their synergistic effect. Studies have shown that these bimetallic compounds have higher electrical conductivity and more abundant redox reaction sites compared to single-phase metal selenides. However, the huge volume expansion produced during the cycling of bimetallic selenides leads to a sharp attenuation of capacity, limiting its practical application.
[0004] Patent publication number CN117712302A discloses a preparation method and application of a hollow ring-shaped carbon-coated transition metal selenide nanomaterial with a multi-level pore structure. The invention prepares a hollow ring-shaped carbon-coated transition metal selenide nanomaterial with a multi-level pore structure for the first time. The iron-nickel bimetallic selenide Fe3Ni2Se4 was discovered for the first time. It has very excellent electrochemical properties as a negative electrode material in potassium ion batteries. Its ultra-fast rate performance and ultra-high electrochemical stability are at the top level in current reports. However, the nanomaterial is prepared using transition metal salts, sodium acetate trihydrate, and ammonium fluoride, and is obtained by hydrothermal method, low-temperature water bath method, and two-step high-temperature annealing. The preparation process is complicated. The material has a high electrochemical performance of 100mAg -1 At a current density of 1.5 %, it has 458 mAh g after 190 cycles. -1 The reversible specific capacity of the material. The volume change of the material is inevitable during the charge and discharge process, resulting in a decrease in specific capacity and poor cycle stability. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a carbon-coated chromium-based bimetallic selenide and its preparation method and application. The carbon-coated chromium-based bimetallic selenide buffers the volume expansion of the bimetallic selenide during the charging and discharging process when it is used in a lithium-ion battery and has good electrochemical properties.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] One of the technical solutions of the present invention is to provide a method for preparing a carbon-coated chromium-based bimetallic selenide, comprising the following steps:
[0008] S1, dissolving a chromium source, a second metal source and terephthalic acid in an aqueous solution of N,N-dimethylformamide, and stirring to form a precursor solution;
[0009] S2, subjecting the precursor solution obtained in step S1 to a hydrothermal reaction to obtain a suspension, washing and drying the suspension to obtain a bimetallic-MOF;
[0010] S3, subjecting the bimetallic-MOF obtained in step S2 to a high-temperature solid-phase selenization reaction with selenium powder, washing and drying to obtain a carbon-coated chromium-based bimetallic selenide, and the reaction is completed.
[0011] Further, in step S1, the chromium source includes chromium nitrate, chromium sulfate, chromium chloride, chromium acetate, preferably chromium nitrate.
[0012] Furthermore, in step S1, the second metal source includes a copper source, a nickel source, and an iron source.
[0013] Furthermore, the copper source includes copper nitrate, copper sulfate, copper chloride, copper acetate, preferably copper nitrate.
[0014] Furthermore, the nickel source includes nickel nitrate, nickel sulfate, nickel chloride, nickel acetate, preferably nickel nitrate.
[0015] Furthermore, the iron source includes ferric nitrate, ferric sulfate, ferric chloride, ferric acetate, preferably ferric nitrate.
[0016] Further, in step S1, the molar volume ratio of the aqueous solution of the chromium source, the second metal source, terephthalic acid, and N,N-dimethylformamide is (1-3):1:(2-4):(0.1-0.5);
[0017] The concentration of the aqueous solution of N,N-dimethylformamide is 70% to 80%.
[0018] Furthermore, in step S1, the stirring temperature is room temperature, the stirring time is 30 to 60 minutes, and the stirring speed is 1000 to 2000 r / min.
[0019] Furthermore, in step S2, the temperature of the hydrothermal reaction is 100-160° C., and the time is 24-62 hours.
[0020] Furthermore, in step S2, washing is first performed with N,N-dimethylformamide, and then with 60-80° C. hot ethanol, and the hot ethanol is replaced every 2-6 hours. The purpose of washing and soaking is to remove unreacted terephthalic acid.
[0021] Furthermore, in step S3, the molar ratio of the chromium source to the selenium powder is 1:(1-3).
[0022] Furthermore, in step S3, the temperature of the selenization reaction is 500-600° C., and the time is 2-4 hours. The selenization reaction is carried out in a vacuum glass tube.
[0023] Furthermore, in step S3, deionized water and anhydrous ethanol are used for washing in sequence.
[0024] Furthermore, in step S3, drying is performed under vacuum, the drying temperature is 80 to 100°C, and the drying time is 12 to 24 hours.
[0025] The second technical solution of the present invention is to provide a carbon-coated chromium-based bimetallic selenide, which is prepared by the above-mentioned preparation method. Carbon is coated on the surface of the chromium-based bimetallic selenide. The entire material has no obvious regular morphology, and a large number of small particles of uneven sizes are agglomerated together to form an amorphous structure.
[0026] The third technical solution of the present invention is to provide an application of a carbon-coated chromium-based bimetallic selenide, and to apply the carbon-coated chromium-based bimetallic selenide as a negative electrode material in the battery field.
[0027] Furthermore, the carbon-coated chromium-based bimetallic selenide is evenly mixed with a conductive agent and an adhesive and then coated on a copper foil, dried, and rolled to form a lithium-ion battery negative electrode sheet, a metal lithium sheet, a separator, and an electrolyte.
[0028] Furthermore, the mass ratio of the carbon-coated chromium-based bimetallic selenide, the binder and the conductive agent is (7-8): (1-2):1.
[0029] Furthermore, the binder is sodium carboxymethyl cellulose.
[0030] Furthermore, the conductive agent is conductive carbon Super-P or conductive carbon black.
[0031] Furthermore, the thickness of the coating on the copper foil is 100 to 180 microns; after rolling, the thickness of the coating material on the copper foil is 75 to 150 microns. Within these thickness ranges, the prepared single pole piece has a moderate load, is easy to penetrate the electrolyte, and is not easy to fall off.
[0032] Furthermore, the drying is carried out under vacuum conditions, the drying temperature is 50-120° C., and the drying time is 5-24 hours. Drying at this temperature can not only dry the coating completely, but also will not affect the coated material.
[0033] Furthermore, (0.5-2)M LiPF6 dissolved in EC:DMC (volume ratio = 1:(0.5-2)) was used as the electrolyte, wherein EC was ethylene carbonate and DMC was dimethyl carbonate.
[0034] Compared with the prior art, the present invention has the following advantages:
[0035] (1) The present invention synthesizes a bimetallic-MOF by a simple hydrothermal reaction, and forms a carbon-coated chromium-based bimetallic selenide battery negative electrode material by selenization. Selenization by a vacuum solid phase reaction method can ensure that the purity of the obtained product is high. In the material, the bimetallic selenide is coated with a carbon skeleton, wherein the carbon is formed by carbonization during the high-temperature selenization process. This layer of carbon skeleton can not only serve as a conductive channel for ions / electrons, greatly shortening the charge transfer path, but also avoid direct contact between the bimetallic selenide and the electrolyte, reducing the occurrence of side reactions. More importantly, this layer of carbon layer can offset the mechanical strain caused by the volume expansion of the material, maintain the structural integrity of the material particles during the cycle process, and thus make the material have good electrochemical properties. The carbon-coated chromium-based bimetallic selenide negative electrode material prepared by the present invention has high first charge and discharge coulomb efficiency, high specific capacity, excellent rate performance and cycle performance, buffers the volume expansion of the metal selenide during the charge and discharge process when it is used in lithium-ion batteries, and is a very promising lithium-ion battery negative electrode material.
[0036] (2) The present invention uses a simple hydrothermal method and solid phase reaction to synthesize a series of carbon-coated chromium-based bimetallic selenides without fixed morphology in two steps. Since carbonization occurs at the same time as selenization, the carbon matrix encapsulated nanoparticles obtained by in-situ carbonization of MOF has great advantages. This special structure composed of an external carbon layer and nanoparticles has great advantages. The prepared CuCr2Se4@C, NiCr2Se4@C, and FeCr2Se4@C have good thermal conductivity and good thermal conductivity. -1 Under the condition of 200 cycles, they can maintain 593.35, 566.36 and 762.51 mAh g respectively. -1 High specific capacity.
[0037] (3) Carbon composites derived from bimetallic MOFs can effectively combine the advantages of two monometallic MOFs. The introduction of two metals can adjust the electronic structure and accelerate the reaction kinetics. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a comparison chart of X-ray diffraction tests of the CuCr2Se4@C composite material obtained in Example 1, the CuCr2Se4 material obtained in Comparative Example 1, and the standard CuCr2Se4 powder;
[0039] Figure 2 This is a Raman comparison diagram of the CuCr2Se4@C composite material obtained in Example 1 and the CuCr2Se4 material obtained in Comparative Example 1;
[0040] Figure 3 is a scanning electron microscope image of the CuCr2Se4@C composite material obtained in Example 1;
[0041] Figures 4 to 6 Transmission electron microscope images of the CuCr2Se4@C composite materials obtained in Example 1 of different sizes, Figure 4-2 μm, Figure 5-10 0nm, Figure 6-5 0nm;
[0042] Figure 7 This is a comparison chart of the cycle performance of the CuCr2Se4@C composite material obtained in Example 1 and the CuCr2Se4 material obtained in Comparative Example 1;
[0043] Figure 8 This is a comparison chart of the rate performance of the lithium ion battery obtained in Example 1 and the lithium ion battery obtained in Comparative Example 1;
[0044] Fig. 9 This is a comparison chart of X-ray diffraction tests of the NiCr2Se4@C composite material obtained in Example 2, the NiCr2Se4 material obtained in Comparative Example 2, and the standard NiCr2Se4 powder;
[0045] Fig.10 This is a Raman comparison diagram of the NiCr2Se4@C composite material obtained in Example 2 and the NiCr2Se4 material obtained in Comparative Example 2;
[0046] Fig.11 is a scanning electron microscope image of the NiCr2Se4@C composite material obtained in Example 2;
[0047] Figures 12-14 Transmission electron microscope images of NiCr2Se4@C composite materials obtained in Example 2 of different sizes, Figure 12-10 0nm, Figure 13-5 0nm, Figure 14-5 nm;
[0048] Fig.15 This is a comparison chart of the cycle performance of the NiCr2Se4@C composite material obtained in Example 2 and the NiCr2Se4 material obtained in Comparative Example 2;
[0049] Fig.16 This is a comparison chart of the rate performance of the lithium ion battery obtained in Example 2 and the lithium ion battery obtained in Comparative Example 2.
[0050] Fig.17 It is a comparison chart of X-ray diffraction tests of the FeCr2Se4@C composite material obtained in Example 3, the FeCr2Se4 material obtained in Comparative Example 3 and the standard FeCr2Se4 powder;
[0051] Fig.18 This is a Raman comparison diagram of the FeCr2Se4@C composite material obtained in Example 3 and the FeCr2Se4 material obtained in Comparative Example 3;
[0052] Fig.19 is a scanning electron microscope image of the FeCr2Se4@C composite material obtained in Example 3;
[0053] Figures 20-22 Transmission electron microscope images of the FeCr2Se4@C composite materials obtained in Example 3 of different sizes, Figure 20-10 0nm, Figure 21-5 0nm, Figure 22-5 nm;
[0054] Fig.23 It is a comparison chart of the cycle performance of the FeCr2Se4@C composite material obtained in Example 3 and the FeCr2Se4 material obtained in Comparative Example 3;
[0055] Fig.24 This is a comparison chart of the rate performance of the lithium ion battery obtained in Example 3 and the lithium ion battery obtained in Comparative Example 3;
[0056] Fig.25 This is a scanning electron microscope image of the CuCr2Se4 material obtained in Comparative Example 1;
[0057] Fig.26 This is a scanning electron microscope image of the NiCr2Se4 material obtained in Comparative Example 2;
[0058] Fig. 27 This is a scanning electron microscope image of the FeCr2Se4 material obtained in Comparative Example 3. DETAILED DESCRIPTION
[0059] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments. Based on the given embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0060] In the following examples, the specific sources of various reagents and raw materials are shown in Table 1. Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art.
[0061] Table 1 Experimental reagents
[0062]
[0063] A method for preparing a carbon-coated chromium-based bimetallic selenide comprises the following steps:
[0064] S1, dissolving a chromium source, a second metal source and terephthalic acid in an aqueous solution of N,N-dimethylformamide, and stirring to form a precursor solution;
[0065] S2, subjecting the precursor solution obtained in step S1 to a hydrothermal reaction to obtain a suspension, washing and drying the suspension to obtain a bimetallic-MOF;
[0066] S3, subjecting the bimetallic-MOF obtained in step S2 to a high-temperature solid-phase selenization reaction with selenium powder, washing and drying to obtain a carbon-coated chromium-based bimetallic selenide, and the reaction is completed.
[0067] As one of the preferred implementations, in step S1, the chromium source includes chromium nitrate, chromium sulfate, chromium chloride, chromium acetate, preferably chromium nitrate.
[0068] As one of the preferred implementations, in step S1, the second metal source includes a copper source, a nickel source, and an iron source.
[0069] As one of the preferred implementations, the copper source includes copper nitrate, copper sulfate, copper chloride, copper acetate, preferably copper nitrate.
[0070] As one of the preferred implementations, the nickel source includes nickel nitrate, nickel sulfate, nickel chloride, and nickel acetate, preferably nickel nitrate.
[0071] As one of the preferred embodiments, the iron source includes ferric nitrate, ferric sulfate, ferric chloride, ferric acetate, preferably ferric nitrate.
[0072] As one of the preferred embodiments, in step S1, the molar volume ratio of the chromium source, the second metal source, terephthalic acid, and the aqueous solution of N,N-dimethylformamide is (1-3):1:(2-4):(0.1-0.5);
[0073] The concentration of the aqueous solution of N,N-dimethylformamide is 70% to 80%.
[0074] As one of the preferred implementations, in step S1, the stirring temperature is room temperature, the stirring time is 30 to 60 minutes, and the stirring speed is 1000 to 2000 r / min.
[0075] As one of the preferred implementations, in step S2, the temperature of the hydrothermal reaction is 100 to 160° C., and the time is 24 to 62 hours.
[0076] As one of the preferred embodiments, in step S2, washing is first performed with N,N-dimethylformamide, and then with 60-80°C hot ethanol, with the hot ethanol being replaced every 2-6 hours. The purpose of washing and soaking is to remove unreacted terephthalic acid.
[0077] As one of the preferred implementations, in step S3, the molar ratio of the chromium source to the selenium powder is 1:(1-3).
[0078] As one of the preferred embodiments, in step S3, the temperature of the selenization reaction is 500-600° C., and the time is 2-4 hours. The selenization reaction is carried out in a vacuum glass tube.
[0079] As one of the preferred implementations, in step S3, deionized water and anhydrous ethanol are used for washing in sequence.
[0080] As one of the preferred implementations, in step S3, drying is performed under vacuum, the drying temperature is 80 to 100° C., and the drying time is 12 to 24 hours.
[0081] A carbon-coated chromium-based bimetallic selenide is prepared by the above-mentioned preparation method. Carbon is coated on the surface of the chromium-based bimetallic selenide. The entire material has no obvious regular morphology, and a large number of small particles of uneven sizes are agglomerated together to present an amorphous structure.
[0082] An application of a carbon-coated chromium-based bimetallic selenide, wherein the carbon-coated chromium-based bimetallic selenide is used as a negative electrode material in the field of batteries.
[0083] As one of the preferred embodiments, the carbon-coated chromium-based bimetallic selenide is evenly mixed with a conductive agent and an adhesive and then coated on a copper foil, and the dried and rolled lithium-ion battery negative electrode sheet is assembled with a metal lithium sheet, a separator and an electrolyte into a lithium-ion battery.
[0084] As one of the preferred implementations, the mass ratio of the carbon-coated chromium-based bimetallic selenide, the binder and the conductive agent is (7-8): (1-2):1.
[0085] As one of the preferred implementations, the binder is sodium carboxymethyl cellulose.
[0086] As one of the preferred implementations, the conductive agent is conductive carbon Super-P or conductive carbon black.
[0087] As one of the preferred embodiments, the thickness of the coating on the copper foil is 100-180 microns; after rolling, the thickness of the coating material on the copper foil is 75-150 microns. Within these thickness ranges, the prepared single pole piece has a moderate load, is easy to penetrate the electrolyte, and is not easy to fall off.
[0088] As one of the preferred embodiments, the drying is carried out under vacuum conditions, the drying temperature is 50-120° C., and the drying time is 5-24 hours. Drying at this temperature can not only dry the coating completely, but also will not affect the coated material.
[0089] As one of the preferred embodiments, (0.5-2)M LiPF6 dissolved in EC:DMC (volume ratio = 1:(0.5-2)) is used as the electrolyte, wherein EC is ethylene carbonate and DMC is dimethyl carbonate.
[0090] Example 1
[0091] A method for preparing a carbon-coated chromium-based bimetallic selenide comprises the following steps:
[0092] Step 1: First, take 1 mmol of Cu(NO3)2·3H2O, 2 mmol of Cr(NO3)3·3H2O and 3 mmol of terephthalic acid (H2DBC) and add them into a solution of 20 mL of N,N-dimethylformamide (DMF) and 7 mL of deionized water, and stir the mixed solution at room temperature at a speed of 1500 r / min for 60 min;
[0093] Step 2: then transferring the above precursor solution to a polytetrafluoroethylene-lined hydrothermal reactor, heating and reacting at 120° C. for 48 hours, and cooling to room temperature to obtain a suspension;
[0094] Step 3: The suspension was centrifuged to obtain a precipitate, which was first washed with N,N-dimethylformamide and then soaked in hot ethanol (70°C) for 12 hours (ethanol was changed every four hours), and the CuCr-MOF obtained by filtration was vacuum dried at 80°C for 12 hours;
[0095] Step 4: Grind CuCr-MOF and 4 mmol selenium powder for 1 hour, put them into a vacuum glass tube, and selenize them at 600°C in a muffle furnace at a heating rate of 2°C / min for 120 minutes to obtain a crude CuCr2Se4@C product;
[0096] Step 5: Wash the obtained CuCr2Se4@C crude product with deionized water and anhydrous ethanol three times respectively, and then dry it at 80°C for 12 hours to obtain a CuCr2Se4@C composite material, i.e., a carbon-coated chromium-based bimetallic selenide.
[0097] The XRD pattern of CuCr2Se4@C composite material was obtained by D2-Phaser X-ray diffractometer. Figure 1 As shown, the scanning rate is 6° / min. It can be seen that the peaks of the CuCr2Se4@C composite material in the figure correspond well to the standard peaks. The results of the XRD spectrum show that the CuCr2Se4@C composite material was successfully prepared in the experiment.
[0098] The Raman spectrometer Renishaw inVia Micro was used to analyze the CuCr2Se4@C composite material and obtain the Raman map. Figure 2 As shown, the Raman spectrum of the CuCr2Se4@C composite material shows the positions of ∼1338 and ∼1610 cm -1 The two scattering peaks at correspond to the D band and G band of graphite carbon material, thus confirming the presence of carbon in the CuCr2Se4@C composite material obtained in Example 1.
[0099] The morphology of the CuCr2Se4@C composite material was observed using a JSM-6700F scanning electron microscope to obtain a SEM image. Figure 3 As shown, it can be seen that the CuCr2Se4@C composite material has no obvious regular morphology, because a large number of small particles of uneven size are agglomerated together to form an amorphous structure.
[0100] The morphology of CuCr2Se4@C composite materials was observed using a JEM-2100F high-resolution transmission electron microscope to obtain TEM images of different sizes. Figures 4 to 6 As shown, it can be seen that a thin carbon layer of about 5 nm is coated on the CuCr2Se4 particles, proving the successful preparation of the CuCr2Se4@C composite material.
[0101] 0.02 g of the prepared CuCr2Se4@C composite material, 0.0025 g of the binder sodium carboxymethyl cellulose and 0.0025 g of the conductive agent Super-P were uniformly mixed, water was used as a solvent, a slurry was prepared, the slurry was coated on a copper foil (the coating thickness was 150 μm), and the slurry was dried at 110°C in a vacuum for 12 h and rolled (the rolling thickness was 130 μm) to prepare a lithium-ion battery negative electrode sheet.
[0102] The lithium ion battery negative electrode sheet, metal lithium sheet and electrolyte prepared in this embodiment are assembled into a lithium ion battery for constant current charge and discharge test. The electrolyte used is EC:DMC (volume ratio = 1:1) containing 1M LiPF6. The constant current charge and discharge test is carried out at a current density of 100mA / g using Shenzhen Neware CT-3008 battery test system. The potential window is 0.01-3V. The cycle performance diagram is as follows Figure 7 As shown in the figure, it can be seen that the first discharge capacity of the CuCr2Se4@C composite material is as high as 670.23mAh / g. After the 200th cycle, the discharge capacity is still maintained at 593.35mAh / g. Figure 8 As shown, it can be seen that under a large current of 5000 mA / g, the discharge specific capacity of the CuCr2Se4@C composite material prepared in this embodiment is still 360.83 mAh / g. When the current density is restored to a low current density of 100 mA / g, the CuCr2Se4@C composite material electrode can recover to the initial discharge capacity, indicating that the material has good rate performance.
[0103] Example 2
[0104] A method for preparing a carbon-coated chromium-based bimetallic selenide comprises the following steps:
[0105] Step 1: First, take 1 mmol of Ni(NO3)2·6H2O, 2 mmol of Cr(NO3)3·3H2O and 3 mmol of terephthalic acid (H2DBC) and add them into a solution of 20 mL of N,N-dimethylformamide (DMF) and 7 mL of deionized water, and stir the mixed solution at room temperature at a speed of 1500 r / min for 60 min;
[0106] Step 2: then transferring the above precursor solution to a polytetrafluoroethylene-lined hydrothermal reactor, heating and reacting at 120° C. for 48 hours, and cooling to room temperature to obtain a suspension;
[0107] Step 3: The suspension was centrifuged to obtain a precipitate, which was first washed with N,N-dimethylformamide and then soaked in hot ethanol (70°C) for 12 hours (ethanol was changed every four hours), and the filtered NiCr-MOF was vacuum dried at 80°C for 12 hours;
[0108] Step 4: Grind NiCr-MOF and 4 mmol selenium powder for 1 hour, put them into a vacuum glass tube, and selenize them at 600°C in a muffle furnace at a heating rate of 2°C / min for 120 minutes to obtain a crude NiCr2Se4@C product;
[0109] Step 5: Wash the obtained NiCr2Se4@C crude product with deionized water and anhydrous ethanol three times respectively, and then dry it at 80°C for 12 hours to obtain a NiCr2Se4@C composite material, i.e., a carbon-coated chromium-based bimetallic selenide.
[0110] The XRD pattern of NiCr2Se4@C composite material was obtained by D2-Phaser X-ray diffractometer. Fig. 9 As shown, the scanning rate is 6° / min. It can be seen that the peaks of the NiCr2Se4@C composite material in the figure correspond well to the standard peaks. The results of the XRD spectrum show that the NiCr2Se4@C composite material was successfully prepared in the experiment.
[0111] The Raman spectrometer Renishaw inVia Micro was used to analyze the NiCr2Se4@C composite material and obtain the Raman map. Fig.10 As shown, the Raman spectrum of the NiCr2Se4@C composite material shows that the -1 The two scattering peaks at correspond to the D band and G band of the disordered graphite carbon material, thus confirming the presence of carbon in the NiCr2Se4@C composite material obtained in Example 2.
[0112] The morphology of the NiCr2Se4@C composite material was observed using a JSM-6700F scanning electron microscope to obtain a SEM image. Fig.11 As shown, it can be seen that the NiCr2Se4@C composite material presents nanoparticles with uneven sizes and smooth surfaces, with carbon rods doped in the middle.
[0113] The morphology of NiCr2Se4@C composite material was observed by JEM-2100F high-resolution transmission electron microscope to obtain TEM images of different sizes. Figures 12-14 As shown, it can be seen that a thin carbon layer of about 2 to 3 nm is coated on the NiCr2Se4 particles, proving the successful preparation of the NiCr2Se4@C composite material.
[0114] 0.02 g of the prepared NiCr2Se4@C composite material, 0.0025 g of the binder sodium carboxymethyl cellulose and 0.0025 g of the conductive agent Super-P were uniformly mixed, and water was used as a solvent to prepare a slurry, which was coated on a copper foil (the coating thickness was 150 μm), and then dried at 110°C in a vacuum for 12 h and rolled (the rolling thickness was 130 μm) to prepare a lithium-ion battery negative electrode sheet.
[0115] The lithium ion battery negative electrode sheet, metal lithium sheet and electrolyte prepared in this embodiment are assembled into a lithium ion battery for constant current charge and discharge test. The electrolyte used is EC:DMC (volume ratio = 1:1) containing 1M LiPF6. The constant current charge and discharge test is carried out at a current density of 100mA / g using Shenzhen Neware CT-3008 battery test system. The potential window is 0.01-3V. The cycle performance diagram is as follows Fig.15 As shown in the figure, it can be seen that the first discharge capacity of the NiCr2Se4@C composite material is as high as 721.28 mAh / g. After the 200th cycle, the discharge capacity is still maintained at 566.36 mAh / g. Fig.16 As shown, it can be seen that under a large current of 5000 mA / g, the discharge specific capacity of the NiCr2Se4@C composite material prepared in this embodiment is still 218.24 mAh / g. When the current density is restored to a low current density of 100 mA / g, the NiCr2Se4@C composite material electrode can be restored to the initial discharge capacity, indicating that the material has good rate performance.
[0116] Example 3
[0117] A method for preparing a carbon-coated chromium-based bimetallic selenide comprises the following steps:
[0118] Step 1: First, take 1 mmol of Fe(NO3)3·9H2O, 2 mmol of Cr(NO3)3·3H2O and 3 mmol of terephthalic acid (H2DBC), add them into a solution of 20 mL of N,N-dimethylformamide (DMF) and 7 mL of deionized water, and stir the mixed solution at room temperature at a speed of 1500 r / min for 60 min;
[0119] Step 2: then transferring the above precursor solution to a polytetrafluoroethylene-lined hydrothermal reactor, heating and reacting at 120° C. for 48 hours, and cooling to room temperature to obtain a suspension;
[0120] Step 3: The suspension was centrifuged to obtain a precipitate, which was first washed with N,N-dimethylformamide and then soaked in hot ethanol (70°C) for 12 hours (ethanol was changed every four hours), and the FeCr-MOF obtained by filtration was vacuum dried at 80°C for 12 hours;
[0121] Step 4: Grind FeCr-MOF and 4 mmol selenium powder for 1 hour, put them into a vacuum glass tube, and selenize them at 600°C in a muffle furnace at a heating rate of 2°C / min for 120 minutes to obtain a crude FeCr2Se4@C product;
[0122] Step 5: Wash the obtained FeCr2Se4@C crude product with deionized water and anhydrous ethanol three times respectively, and then dry it at 80°C for 12 hours to obtain a FeCr2Se4@C composite material, i.e., a carbon-coated chromium-based bimetallic selenide.
[0123] The XRD pattern of FeCr2Se4@C composite material was obtained by D2-Phaser X-ray diffractometer. Fig.17 As shown, the scanning rate is 6° / min. It can be seen that the peaks of the FeCr2Se4@C composite material in the figure correspond well to the standard peaks. The results of the XRD spectrum show that the FeCr2Se4@C composite material was successfully prepared in the experiment.
[0124] The Raman spectrometer ReFeshaw inVia Micro was used to analyze the FeCr2Se4@C composite material and obtain the Raman map. Fig.18 As shown, the Raman spectrum of the FeCr2Se4@C composite material shows that the -1 The two scattering peaks at correspond to the D band and G band of the disordered graphite carbon material, thus confirming the presence of carbon in the FeCr2Se4@C composite material obtained in Example 3.
[0125] The morphology of the FeCr2Se4@C composite material was observed using a JSM-6700F scanning electron microscope to obtain a SEM image. Fig.19 As shown, it can be seen that the FeCr2Se4@C composite material presents irregular nanoparticles.
[0126] The morphology of FeCr2Se4@C composites was observed using a JEM-2100F high-resolution transmission electron microscope to obtain TEM images of different sizes. Figures 20-22 As shown, it can be seen that a thin carbon layer is coated on the FeCr2Se4 particles, proving the successful preparation of the FeCr2Se4@C composite material.
[0127] 0.02 g of the prepared FeCr2Se4@C composite material, 0.0025 g of the binder sodium carboxymethyl cellulose and 0.0025 g of the conductive agent Super-P were uniformly mixed, water was used as a solvent, a slurry was prepared, the slurry was coated on a copper foil (the coating thickness was 150 μm), and the slurry was dried at 110°C in a vacuum for 12 h and rolled (the rolling thickness was 130 μm) to prepare a lithium-ion battery negative electrode sheet.
[0128] The lithium ion battery negative electrode sheet, metal lithium sheet and electrolyte prepared in this embodiment are assembled into a lithium ion battery for constant current charge and discharge test. The electrolyte used is EC:DMC (volume ratio = 1:1) containing 1M LiPF6. The constant current charge and discharge test is carried out at a current density of 100mA / g using Shenzhen Neware CT-3008 battery test system. The potential window is 0.01-3V. The cycle performance diagram is as follows Fig.23 As shown in the figure, it can be seen that the first discharge capacity of the FeCr2Se4@C composite material is as high as 870.87 mAh / g. After the 200th cycle, the discharge capacity is still maintained at 762.51 mAh / g. Fig.24 As shown, it can be seen that under a large current of 5000 mA / g, the discharge specific capacity of the FeCr2Se4@C composite material prepared in this embodiment is still 501.49 mAh / g. When the current density is restored to a low current density of 100 mA / g, the FeCr2Se4@C composite material electrode can be restored to the initial discharge capacity, indicating that the material has good rate performance.
[0129] Example 4
[0130] Compared with Example 1, most of the steps are the same, except that in step 1, 1 mmol of Cu(NO3)2·3H2O, 1 mmol of Cr(NO3)3·3H2O and 3 mmol of terephthalic acid (H2DBC) are first added to a solution of 20 mL of N,N-dimethylformamide (DMF) and 7 mL of deionized water, and the mixed solution is stirred at room temperature at a speed of 1500 r / min for 60 min.
[0131] Example 5
[0132] Compared with Example 1, most of the steps are the same, except that in step 1, 1 mmol of Cu(NO3)2·3H2O, 3 mmol of Cr(NO3)3·3H2O and 3 mmol of terephthalic acid (H2DBC) are first added to a solution of 20 mL of N,N-dimethylformamide (DMF) and 7 mL of deionized water, and the mixed solution is stirred at room temperature at a speed of 1500 r / min for 60 min.
[0133] Example 6
[0134] Compared with Example 1, most of the contents are the same, except that in step 4, the CuCr-MOF and 2 mmol selenium powder are ground for 1 h and then placed in a vacuum glass tube, and selenized at 600°C for 120 min at a heating rate of 2°C / min in a muffle furnace to obtain a crude CuCr2Se4@C product.
[0135] Example 7
[0136] Compared with Example 1, most of the contents are the same, except that in step 4, the CuCr-MOF and 6 mmol selenium powder are ground for 1 h and then placed in a vacuum glass tube, and selenized at 600°C for 120 min at a heating rate of 2°C / min in a muffle furnace to obtain a crude CuCr2Se4@C product.
[0137] Comparative Example 1
[0138] A bimetallic selenide CuCr2Se4 is prepared by the following steps:
[0139] Step 1: 1 mmol of Cu metal powder, 2 mmol of Cr metal powder and 4 mmol of Se metal powder were placed in a crucible and ground for 1 hour to make them evenly mixed;
[0140] Step 2: Place the uniformly ground mixture in step 1 in a vacuum glass tube, and selenize at 600° C. in a muffle furnace at a heating rate of 2° C. / min for 120 min;
[0141] Step 3: Wash the product obtained in step 2 with deionized water and anhydrous ethanol for several times, and then dry it at 80°C for 12 hours to obtain a pure bimetallic selenide CuCr2Se4 material. The CuCr2Se4 material is subjected to phase analysis using a D2-Phaser X-ray diffractometer to obtain an XRD pattern as shown below: Figure 1 As shown, the scanning rate is 6° / min. It can be seen that the diffraction peak of CuCr2Se4 prepared in this embodiment is consistent with the diffraction peak of the standard card, indicating that the CuCr2Se4 material is successfully prepared.
[0142] The CuCr2Se4 material was analyzed using a Renishaw inVia Micro Raman spectrometer to obtain a Raman map. Figure 2 As shown, it can be seen that there is no obvious carbon peak in the Raman spectrum of CuCr2Se4 prepared in this embodiment, indicating that there is no carbon in the CuCr2Se4 prepared in this embodiment.
[0143] The morphology of the CuCr2Se4 material was observed using a JSM-6700F scanning electron microscope to obtain a SEM image. Fig.25As shown, it can be seen that the particles of the CuCr2Se4 material prepared in this embodiment are tightly agglomerated together, and the volume is much larger than that of the CuCr2Se4 particles in the CuCr2Se4@C composite material prepared in Example 1.
[0144] 0.02 g of the CuCr2Se4 material prepared in Comparative Example 1, 0.0025 g of a binder, sodium carboxymethyl cellulose, and 0.0025 g of a conductive agent, Super-P, were uniformly mixed, water was used as a solvent, a slurry was prepared, the slurry was coated on a copper foil (the coating thickness was 150 μm), and the slurry was dried at 110°C in a vacuum for 12 h and rolled (the rolling thickness was 130 μm) to prepare a negative electrode sheet for a lithium-ion battery.
[0145] The lithium-ion battery negative electrode sheet, metal lithium sheet and electrolyte prepared in this comparative example were assembled into a lithium-ion battery for constant current charge and discharge test. The electrolyte used was EC:DMC (volume ratio = 1:1) containing 1M LiPF6. The constant current charge and discharge test was carried out at a current density of 100mA / g using Shenzhen Neware CT-3008 battery test system. The potential window was 0.01-3V. The cycle performance diagram is as follows Figure 7 As shown in the figure, it can be seen that the first discharge capacity of CuCr2Se4 material is 571.99 mAh / g, and the discharge capacity has dropped to 93.39 mAh / g after the 200th cycle. Figure 8 As shown, it can be seen that at a large current of 5000 mA / g, the discharge specific capacity of the CuCr2Se4 material prepared in this embodiment is only 47.33 mAh / g, indicating that its rate performance is extremely poor.
[0146] Comparative Example 2
[0147] A bimetallic selenide NiCr2Se4 is prepared by the following steps:
[0148] Step 1: 1 mmol Ni metal powder, 2 mmol Cr metal powder and 4 mmol Se metal powder are placed in a crucible and ground for 1 hour to make them evenly mixed;
[0149] Step 2: Place the uniformly ground mixture in step 1 in a vacuum glass tube, and selenize at 600° C. in a muffle furnace at a heating rate of 2° C. / min for 120 min;
[0150] Step 3: Wash the product obtained in step 2 with deionized water and anhydrous ethanol for several times, and then dry it at 80°C for 12 hours to obtain a pure bimetallic selenide NiCr2Se4 material. The NiCr2Se4 material is subjected to phase analysis using a D2-Phaser X-ray diffractometer to obtain an XRD pattern as shown below: Fig. 9As shown, the scanning rate is 6° / min. It can be seen that the diffraction peak of the NiCr2Se4 material prepared in this comparative example is consistent with the diffraction peak of the standard card, indicating that the NiCr2Se4 material is successfully prepared.
[0151] The NiCr2Se4 material was analyzed using a Renishaw inVia Micro Raman spectrometer to obtain a Raman map. Fig.10 As shown, it can be seen that there is no obvious carbon peak in the Raman spectrum of the NiCr2Se4 material prepared in this comparative example, indicating that there is no carbon in the NiCr2Se4 prepared in this embodiment.
[0152] The morphology of the NiCr2Se4 material was observed using a JSM-6700F scanning electron microscope to obtain a SEM image. Fig.26 As shown, it can be seen that the particles of the NiCr2Se4 material prepared in this embodiment are tightly agglomerated together, and the volume is much larger than that of the NiCr2Se4 particles in the NiCr2Se4@C composite material prepared in Example 2.
[0153] 0.02 g of the NiCr2Se4 material prepared in this comparative example, 0.0025 g of the binder sodium carboxymethyl cellulose and 0.0025 g of the conductive agent Super-P were uniformly mixed, water was used as a solvent, and a slurry was prepared, which was coated on a copper foil (the coating thickness was 150 μm), and dried at 110°C in vacuum for 12 h and rolled (the rolling thickness was 130 μm) to prepare a negative electrode sheet for a lithium-ion battery.
[0154] The lithium-ion battery negative electrode sheet, metal lithium sheet and electrolyte prepared in this comparative example were assembled into a lithium-ion battery for constant current charge and discharge test. The electrolyte used was EC:DMC (volume ratio = 1:1) containing 1M LiPF6. The constant current charge and discharge test was carried out at a current density of 100mA / g using Shenzhen Neware CT-3008 battery test system. The potential window was 0.01-3V. The cycle performance diagram is as follows Fig.15 As shown in the figure, it can be seen that the first discharge capacity of NiCr2Se4 material is 526.35 mAh / g, and the discharge capacity has dropped to 90.08 mAh / g after the 200th cycle. Fig.16 As shown, it can be seen that under a large current of 5000 mA / g, the discharge specific capacity of the NiCr2Se4 material prepared in this comparative example is only 36.38 mAh / g, indicating that its rate performance is extremely poor.
[0155] Comparative Example 3
[0156] A bimetallic selenide FeCr2Se4 is prepared by the following steps:
[0157] Step 1: 1 mmol Fe metal powder, 2 mmol Cr metal powder and 4 mmol Se metal powder were placed in a crucible and ground for 1 hour to make them evenly mixed;
[0158] Step 2: Place the uniformly ground mixture in step 1 in a vacuum glass tube, and selenize at 600° C. in a muffle furnace at a heating rate of 2° C. / min for 120 min;
[0159] Step 3: Wash the product obtained in step 2 with deionized water and anhydrous ethanol for several times, and then dry it at 80°C for 12 hours to obtain a pure bimetallic selenide FeCr2Se4 material. The FeCr2Se4 material is subjected to phase analysis using a D2-Phaser X-ray diffractometer to obtain an XRD pattern as shown below: Fig.17 As shown, the scanning rate is 6° / min. It can be seen that the diffraction peak of FeCr2Se4 prepared in this embodiment is consistent with the diffraction peak of the standard card, indicating that the FeCr2Se4 material is successfully prepared.
[0160] The Raman spectrometer Renishaw inVia Micro was used to analyze the FeCr2Se4 material and obtain the Raman map. Fig.18 As shown, it can be seen that there is no obvious carbon peak in the Raman spectrum of FeCr2Se4 prepared in this embodiment, indicating that there is no carbon in the FeCr2Se4 prepared in this embodiment.
[0161] The morphology of the FeCr2Se4 material was observed using a JSM-6700F scanning electron microscope to obtain a SEM image. Fig. 27 As shown, it can be seen that the particles of the FeCr2Se4 material prepared in this embodiment are tightly agglomerated together, and the volume is much larger than that of the FeCr2Se4 particles in the FeCr2Se4@C composite material prepared in Example 3.
[0162] 0.02 g of the FeCr2Se4 material prepared in this comparative example, 0.0025 g of the binder sodium carboxymethyl cellulose and 0.0025 g of the conductive agent Super-P were uniformly mixed, water was used as a solvent, and a slurry was prepared, which was coated on a copper foil (the coating thickness was 150 μm), and dried at 110°C in vacuum for 12 h and rolled (the rolling thickness was 130 μm) to prepare a negative electrode sheet for a lithium-ion battery.
[0163] The lithium-ion battery negative electrode sheet, metal lithium sheet and electrolyte prepared in this comparative example were assembled into a lithium-ion battery for constant current charge and discharge test. The electrolyte used was EC:DMC (volume ratio = 1:1) containing 1M LiPF6. The constant current charge and discharge test was carried out at a current density of 100mA / g using Shenzhen Neware CT-3008 battery test system. The potential window was 0.01-3V. The cycle performance diagram is as follows Fig.23 As shown in the figure, it can be seen that the first discharge capacity of FeCr2Se4 material is 543.23 mAh / g, and the discharge capacity has dropped to 183.4 mAh / g after the 200th cycle. Fig.24 As shown, it can be seen that under a large current of 5000 mA / g, the discharge specific capacity of the FeCr2Se4 material prepared in this comparative example is only 81.42 mAh / g, indicating that its rate performance is extremely poor.
[0164] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for preparing a carbon-coated chromium-based bimetallic selenide, characterized in that: The following steps are involved: S1, dissolving a chromium source, a second metal source and terephthalic acid in an aqueous solution of N,N-dimethylformamide, and stirring to form a precursor solution; S2, subjecting the precursor solution obtained in step S1 to a hydrothermal reaction to obtain a suspension, washing, and drying to obtain a bimetallic-MOF; S3, subjecting the bimetallic-MOF obtained in step S2 to a high-temperature solid-phase selenization reaction with selenium powder, washing and drying to obtain a carbon-coated chromium-based bimetallic selenide, and the reaction is completed.
2. The method for preparing a carbon-coated chromium-based bimetallic selenide according to claim 1, characterized in that: In step S1, the chromium source includes chromium nitrate, chromium sulfate, chromium chloride, and chromium acetate.
3. The method for preparing a carbon-coated chromium-based bimetallic selenide according to claim 1, characterized in that: In step S1, the second metal source includes a copper source, a nickel source, and an iron source; The copper source includes copper nitrate, copper sulfate, copper chloride, and copper acetate; The nickel source includes nickel nitrate, nickel sulfate, nickel chloride, and nickel acetate; The iron source includes ferric nitrate, ferric sulfate, ferric chloride and ferric acetate.
4. The method for preparing a carbon-coated chromium-based bimetallic selenide according to claim 1, characterized in that: In step S1, the molar volume ratio of the chromium source, the second metal source, terephthalic acid, and the aqueous solution of N,N-dimethylformamide is (1-3):1:(2-4):(0.1-0.5); The concentration of the aqueous solution of N,N-dimethylformamide is 70% to 80%.
5. The method for preparing a carbon-coated chromium-based bimetallic selenide according to claim 1, characterized in that: In step S2, the temperature of the hydrothermal reaction is 100-160°C.
6. The method for preparing a carbon-coated chromium-based bimetallic selenide according to claim 1, characterized in that: In step S3, the molar ratio of the chromium source to the selenium powder is 1:(1-3).
7. The method for preparing a carbon-coated chromium-based bimetallic selenide according to claim 1, characterized in that: In step S3, the temperature of the selenization reaction is 500-600°C.
8. A carbon-coated chromium-based bimetallic selenide, which is prepared by the preparation method according to any one of claims 1 to 7, wherein carbon is coated on the surface of the chromium-based bimetallic selenide, and the entire material has an amorphous structure.
9. The use of a carbon-coated chromium-based bimetallic selenide as claimed in claim 8, characterized in that: The carbon-coated chromium-based bimetallic selenide is used as a negative electrode material in the field of batteries.
10. The use of a carbon-coated chromium-based bimetallic selenide according to claim 9, characterized in that: The carbon-coated chromium-based bimetallic selenide is evenly mixed with a conductive agent and an adhesive and then coated on a copper foil, dried, and rolled with a lithium-ion battery negative electrode sheet, and assembled with a metal lithium sheet, a separator and an electrolyte into a lithium-ion battery.