Preparation method of layered oxide type composite material serving as positive electrode of sodium-ion battery

The layered oxide composite material prepared by co-precipitation method solves the problem of cumbersome and high cost of P2-Na2/3Ni1/3Mn2/3O2 modification process, realizes the high cycle performance and rate performance of the material, and simplifies the process flow It also reduces costs and lays a good foundation for the commercial application of sodium ion batteries.

CN118983418AActive Publication Date: 2024-11-19HARBIN INST OF TECH

Patent Information

Application Number
CN202411071679.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The modification method of layered oxide cathode material P2-Na2/3Ni1/3Mn2/3O2 is cumbersome and has high cost, making it difficult to achieve large-scale production and commercial application.

Method used

The layered oxide composite material was prepared by co-precipitation method. The pH was adjusted by dropping ammonia water and alkali liquid in deionized water to adjust the pH to form a metal salt solution, and then uniformly mix it with the sodium source for high-temperature reaction, naturally cool, and uniform doping of iron elements In the material, the sodium ion channel is broadened and the electrochemical performance is improved.

Benefits of technology

The high cycle performance and rate performance of the material are achieved. The capacity retention rate reaches 65.21% after 200 cycles, and the specific capacity of 53.37mAh/g is still available under high current density, which simplifies the process flow and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983418A_ABST
    Figure CN118983418A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a layered oxide composite material serving as a sodium ion battery positive electrode, and relates to a positive electrode material of a sodium ion battery, in particular to a preparation method of the layered oxide composite material. The invention aims to solve the technical problems that the existing modification method of the layered oxide type positive electrode material P2-Na2 / 3Ni1 / 3Mn2 / 3O2 is tedious in process and relatively high in cost. The layered oxide material with a P2 type structure is obtained through a coprecipitation method, and the iron element is uniformly doped into the manganese site of the material in the coprecipitation process, so that doping modification of the iron element is realized. On one hand, iron ions with larger ion radius are doped, the unit cell volume is increased, a sodium ion channel is widened, and on the other hand, the ginger-Taylor effect of manganese can be inhibited to a certain extent, so that the electrochemical performance of the material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a positive electrode material for a sodium ion battery, in particular to a method for preparing a layered oxide type composite material. Background Art

[0002] In recent years, the technology of converting renewable energy such as wind energy, solar energy, hydropower and tidal energy into electrical energy has developed rapidly. However, the electricity generated by it is limited by natural conditions and has the characteristics of randomness, intermittency and volatility, which often leads to energy waste such as abandonment of water, wind and light. Therefore, the development of efficient, convenient and safe energy storage technology has attracted widespread attention from researchers. Among the many energy storage technologies, electrochemical energy storage has the advantages of easy use, high energy conversion efficiency and fast response speed, and has broad application prospects in the field of energy storage. Among them, lithium-ion batteries (LIBs) are widely used due to their long cycle life and high energy density. However, with the rapid increase in demand for batteries for portable electronic products and electric vehicles, the limited reserves of lithium resources make it difficult to support the simultaneous development of consumer electronics, electric vehicles and large-scale energy storage. Compared with limited lithium resources, sodium is abundant on the earth, distributed all over the world, and is cost-effective. Therefore, sodium-ion batteries (NIBs), which mainly rely on sodium resources, are considered to be a promising alternative to the large-scale use of lithium-ion batteries. In addition, since sodium does not alloy with aluminum, the negative electrode current collector can be replaced from copper to cheaper aluminum. Therefore, sodium-ion batteries have received great attention since 2012.

[0003] P2-Na 2 / 3 Ni 1 / 3 Mn 2 / 3 O2 has attracted great attention among P2-type materials due to its electrochemical performance and material properties. (1) P2-Na 2 / 3 Ni 1 / 3 Mn 2 / 3 O2 exhibits high operating voltage (about 3.8 V) and high capacity (about 173 mAh g -1), which in turn enables it to have a high energy density in the layered transition metal oxide cathode when assembling a full battery (Clement RJ, Bruce PG, Grey CP. Review—Manganese-Based P2-Type Transition Metal Oxides as Sodium-Ion Battery Cathode Materials. Journal of The Electrochemical Society, 2015, 162(14): A2589. DOI: 10.1149 / 2.0201514jes.); (2) Most P2-type oxides are sodium-deficient, while P2-Na 2 / 3 Ni 1 / 3 Mn 2 / 3 The amount of sodium ions in O2 is sufficient for electrochemical cycling (Lu Z, Dahn J R. In Situ X-Ray Diffraction Study of P2-Na 2 / 3 [Ni 1 / 3 Mn 2 / 3 ]O2.Journal of The Electrochemical Society, 2001, 148(11):A1225.DOI:10.1149 / 1.1407247), there is no additional component (for example, a sodium-rich sacrificial source is needed during the first charge / discharge process) to compensate for the lack of sodium, and this material has significant advantages in realizing high-energy full batteries; (3) Unlike most layered oxides, P2-Na 2 / 3 Ni 1 / 3 Mn 2 / 3 O2 is stable at room temperature and pressure (Lu Z, Dahn J R. Intercalation of Water in P2, T2 and O2 Structure A z [Co x Ni 1 / 3-x Mn 2 / 3 ]O2.Chemistry of Materials, 2001, 13(4):1252-1257.DOI:10.1021 / cm000721x), which makes the material easy to handle in actual production; (4) P2-Na 2 / 3 Ni 1 / 3 Mn 2 / 3O2 can be generated by natural cooling after conditional sintering, which is significantly different from other P2-type oxide cathodes. This feature is very suitable for large-scale production of materials. Because the P2 phase is unstable during slow cooling, most P2-type oxides must be quenched immediately after sintering at high temperatures (usually 850-950°C) (Pang WK, Kalluri S, Peterson VK, et al. Interplay between Electrochemistry and Phase Evolution of the P2-type Na x (Fe 1 / 2 Mn 1 / 2 )O2 Cathode for Use in Sodium-Ion Batteries. Chemistry of Materials, 2015, 27(8): 3150-3158. DOI: 10.1021 / acs.chemmater.5b00943.). However, this quenching operation is actually dangerous and difficult to handle. Based on the above properties, P2-Na 2 / 3 Ni 1 / 3 Mn 2 / 3 O2 is one of the most promising candidate cathodes for realizing practical applications of high-energy NIBs. However, at a high voltage of 4.2 V, P2-Na 2 / 3 Ni 1 / 3 Mn 2 / 3 O2 will undergo an irreversible phase transition from P2 to O2, which will cause changes in the material's structure, leading to poor cyclic stability. The researchers modified the material through strategies such as element doping, surface coating, and micromorphology control to improve the structural stability of the material under high pressure, thereby improving its cyclic stability. 2 / 3 Ni 1 / 3 Mn 2 / 3 O2 by Atomic LayerDeposition.ACS Applied Materials&Interfaces, 2017, 9(31):26518-26530.DOI:10.1021 / acsami.7b05326.) 2 / 3 Ni 1 / 3 Mn 2 / 3The Al2O3 layer is coated on O2. The Al2O3 layer can reduce the decomposition of the electrolyte, avoid the formation of too thick SEI, and improve the electrochemical performance. After 100 cycles, the capacity of the modified sample remains at about 77.4 mAhg -1 , higher than the 52mAhg of the uncoated sample -1 . Liu Y, Shen Q, Zhao X, et al. Hierarchical Engineering of Porous P2-Na 2 / 3 Ni 1 / 3 Mn 2 / 3O2Nanofibers Assembled by Nanoparticles Enables Superior Sodium-Ion StorageCathodes.Advanced Functional Materials, 2020, 30(6):1907837.DOI:10.1002 / adfm.201907837) synthesized P2-Na 2 / 3 Ni 1 / 3 Mn 2 / 3 O2 nanofibers, which exhibit excellent rate performance (166.7 mAh g at 0.1C) -1 , 73.4mAh g at 20C -1 ) and significantly improved the cycle stability of the material (capacity retention rate ≈ 81% after 500 cycles). However, the above scheme still has problems such as complex process, cumbersome process and high cost. Therefore, by adopting a simple and efficient modification method, while developing a technical route that can be mass-produced, combined with the high discharge capacity of the layered oxide material itself, a good foundation is laid for the practical application of sodium-ion battery positive electrode materials, which has a very important research significance for the commercialization and multi-purpose development of sodium-ion batteries. Summary of the invention

[0004] The present invention aims to solve the problem of the current layered oxide type positive electrode material P2-Na 2 / 3 Ni 1 / 3 Mn 2 / 3 In order to solve the technical problems of complicated process and high cost of O2 modification method, a method for preparing a layered oxide composite material as the positive electrode of a sodium ion battery is provided.

[0005] The preparation method of the layered oxide type composite material as the positive electrode of the sodium ion battery of the present invention is carried out according to the following steps:

[0006] 1. Co-precipitation to obtain a precursor: add ammonia water to deionized water to make the pH value be 10.8-11.2, then add a metal salt solution, and then add alkali solution to adjust the pH value to 10.6-10.8 for co-precipitation, continue stirring for 12h-16h for aging, and then filter, wash and dry in sequence to obtain a precursor;

[0007] The solute in the metal salt solution is composed of a nickel source, a manganese source and an iron source, and the ratio of the amount of nickel element in the nickel source, the amount of manganese element in the manganese source and the amount of iron element in the iron source is 0.33:0.67-x:x, x≤0.1;

[0008] The sum of the molar concentrations of nickel, manganese and iron in the metal salt solution is 2 mol / L to 2.5 mol / L;

[0009] The volume ratio of the deionized water to the metal salt solution is 1:(2.09-3.01);

[0010] 2. The precursor prepared in step 1 is mixed evenly with the metal salt of the sodium source, and pre-reacted at 450°C to 500°C for 5h to 5.5h, and then heated to 850°C to 900°C and kept warm for 16h to 17h, and naturally cooled to room temperature, and then taken out and fully ground to obtain a layered oxide type positive electrode material;

[0011] The ratio of the amount of the sodium element in the sodium source to the sum of the three metal elements in the precursor is (1.05-1.1):1;

[0012] The reaction atmosphere during the entire reaction process of step 2 is air.

[0013] The present invention uses a coprecipitation method to dissolve a nickel source, a manganese source and an iron source in deionized water in a stoichiometric ratio to form a metal salt solution, and then drips the metal salt solution into the deionized water, and adjusts the pH with an alkaline solution composed of sodium hydroxide and ammonia water. After the coprecipitation reaction is completed, stirring is continued for aging, and then filtering, washing and drying are performed to obtain a precursor; then the precursor is evenly mixed with a metal salt of a sodium source in a certain proportion, a high-temperature reaction is performed, and naturally cooled to room temperature to obtain a layered oxide material with a P2 type structure. During the coprecipitation process, the iron element is uniformly doped into the manganese position of the material to achieve doping modification of the iron element. On the one hand, iron ions with a larger ionic radius (larger than +4-valent manganese ions) are doped to increase the unit cell volume and broaden the sodium ion channel. On the other hand, the Jan-Taylor effect of manganese can be suppressed to a certain extent, thereby improving the electrochemical properties of the material. After the material prepared by the present invention is assembled into a battery as a positive electrode, in terms of cycle performance, at 100mAg -1 After 200 cycles at a current density of 5.18 mAh g -1The discharge capacity retention rate is 65.21%; in terms of rate performance, at 1000mAg -1 The current density is still 53.37 mAh g -1 Specific capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is the SEM image of the layered oxide type positive electrode material prepared in Experiment 1;

[0015] Figure 2 is the XRD pattern;

[0016] Figure 3 It is a comparison curve of battery rate performance;

[0017] Figure 4 This is a comparison chart of battery cycle performance;

[0018] Figure 5 This is the cyclic voltammetry curve of the battery. DETAILED DESCRIPTION

[0019] Specific implementation method 1: This implementation method is a method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery, which is specifically carried out according to the following steps:

[0020] 1. Co-precipitation to obtain a precursor: add ammonia water to deionized water to make the pH value be 10.8-11.2, then add a metal salt solution, and then add alkali solution to adjust the pH value to 10.6-10.8 for co-precipitation, continue stirring for 12h-16h for aging, and then filter, wash and dry in sequence to obtain a precursor;

[0021] The solute in the metal salt solution is composed of a nickel source, a manganese source and an iron source, and the ratio of the amount of nickel element in the nickel source, the amount of manganese element in the manganese source and the amount of iron element in the iron source is 0.33:0.67-x:x, x≤0.1;

[0022] The sum of the molar concentrations of nickel, manganese and iron in the metal salt solution is 2 mol / L to 2.5 mol / L;

[0023] The volume ratio of the deionized water to the metal salt solution is 1:(2.09-3.01);

[0024] 2. The precursor prepared in step 1 is mixed evenly with the metal salt of the sodium source, and pre-reacted at 450°C to 500°C for 5h to 5.5h, and then heated to 850°C to 900°C and kept warm for 16h to 17h, and naturally cooled to room temperature, and then taken out and fully ground to obtain a layered oxide type positive electrode material;

[0025] The ratio of the amount of the sodium element in the sodium source to the sum of the three metal elements in the precursor is (1.05-1.1):1;

[0026] The reaction atmosphere during the entire reaction process of step 2 is air.

[0027] Specific implementation method 2: This implementation method is different from the specific implementation method 1 in that the alkali solution described in step 1 is 10 molL -1 of sodium hydroxide solution and 0.2 molL -1 The ammonia water is mixed in a volume ratio of 7:3. Other aspects are the same as those of the first embodiment.

[0028] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the washing described in step 1 is washing with deionized water. The rest is the same as specific implementation method 1 or 2.

[0029] Specific embodiment 4: This embodiment is different from specific embodiments 1 to 3 in that the drying temperature in step 1 is 100°C and the drying time is 12 hours. The rest is the same as specific embodiments 1 to 3.

[0030] Specific embodiment 5: This embodiment differs from specific embodiment 4 in that the nickel source in step 1 is nickel acetate tetrahydrate, nickel nitrate hexahydrate, nickel chloride hexahydrate or nickel sulfate hexahydrate. The rest is the same as specific embodiment 4.

[0031] Specific embodiment 6: This embodiment is different from specific embodiment 5 in that the manganese source in step 1 is manganese acetate tetrahydrate, manganese chloride tetrahydrate or manganese sulfate monohydrate. The rest is the same as specific embodiment 5.

[0032] Specific embodiment 7: This embodiment is different from specific embodiment 6 in that the iron source in step 1 is ferrous oxalate dihydrate or ferrous sulfate heptahydrate. The rest is the same as specific embodiment 6.

[0033] Specific embodiment eight: This embodiment differs from specific embodiment seven in that the sodium source in step two is sodium acetate, sodium citrate, sodium carbonate, sodium bicarbonate or sodium hydroxide. The rest is the same as specific embodiment seven.

[0034] Specific embodiment 9: This embodiment is different from specific embodiment 8 in that the ratio of the amount of the sodium element in the sodium source in step 2 to the sum of the three metal elements in the precursor is 1.05:1. The rest is the same as specific embodiment 8.

[0035] Specific embodiment 10: This embodiment differs from specific embodiment 9 in that in step 2, the pre-reaction is first performed at 450°C for 5 hours, then the temperature is raised to 850°C and kept for reaction for 16 hours, and then the material is naturally cooled to room temperature, taken out and fully ground to obtain a layered oxide positive electrode material. The rest is the same as specific embodiment 9.

[0036] The present invention is verified by the following tests:

[0037] Experiment 1: This experiment is a method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery, which is specifically carried out in the following steps:

[0038] 1. Co-precipitation to obtain a precursor: Add ammonia water to deionized water to make the pH value 11, then add a metal salt solution, and then add alkali solution to adjust the pH value to 10.7 for co-precipitation, continue stirring for 14 hours for aging, and then filter, wash and dry in sequence to obtain a precursor;

[0039] The solute in the metal salt solution is composed of a nickel source, a manganese source and an iron source, and the ratio of the amount of nickel element in the nickel source, the amount of manganese element in the manganese source and the amount of iron element in the iron source is 0.33:0.57:0.1;

[0040] The sum of the concentrations of nickel, manganese and iron in the metal salt solution is 2 mol / L -1 ;

[0041] The volume ratio of the deionized water to the metal salt solution is 1:3;

[0042] The alkali solution is composed of 10 molL -1 of sodium hydroxide solution and 0.2 molL -1 Ammonia water is mixed in a volume ratio of 7:3;

[0043] The washing is washing with deionized water;

[0044] The drying temperature is 100°C and the drying time is 12h;

[0045] The nickel source is nickel sulfate hexahydrate;

[0046] The manganese source is manganese sulfate monohydrate;

[0047] The iron source is ferrous sulfate heptahydrate;

[0048] 2. The precursor prepared in step 1 is mixed evenly with the metal salt of the sodium source, pre-reacted at 450°C for 5 hours, then heated to 850°C and kept for reaction for 16 hours, cooled naturally to room temperature, taken out and fully ground to obtain a layered oxide type positive electrode material;

[0049] The ratio of the amount of sodium element in the sodium source to the sum of the three metal elements in the precursor is 1.05:1;

[0050] The reaction atmosphere during the entire reaction process of step 2 is air;

[0051] The sodium source is sodium carbonate.

[0052] Figure 1 This is the SEM image of the layered oxide positive electrode material prepared in experiment 1. From the image, it can be seen that the material size is uniform, there is no obvious agglomeration, and the dispersion is good, which is conducive to increasing the utilization rate of active materials.

[0053] The layered oxide positive electrode material obtained in Experiment 1 was weighed and mixed with the conductive agent (conductive carbon black) and the binder (PVDF) in a mass ratio of 7:2:1, and then subjected to operations such as activating paste, coating, and punching. It was then assembled with the sodium sheet (negative electrode) into a CR2032 button cell, recorded as No. 1 battery, and tested. The electrolyte used was 1 mol L -1 NaClO4, the solvent is EC / PC, the volume ratio of the two is 1:1, 5% FEC is used as an additive, and the separator is glass fiber GF / D; finally, the assembled battery is left for more than 12 hours for electrochemical performance testing.

[0054] Comparative test: In this test, no iron source was added during the preparation of the layered oxide positive electrode material. The specific process is different from that of test 1:

[0055] The solute in the metal salt solution described in step 1 is composed of a nickel source and a manganese source, and the molar ratio of the nickel element in the nickel source to the manganese element in the manganese source is 1:2; the sum of the molar concentrations of the nickel element and the manganese element in the metal salt solution is 2 mol / L. Others are the same as in experiment 1.

[0056] The layered oxide positive electrode material obtained in Experiment 2 was weighed and mixed with a conductive agent (conductive carbon black) and a binder (PVDF) in a mass ratio of 7:2:1, and then subjected to operations such as activating paste, coating, and punching. It was then assembled with a sodium sheet (negative electrode) into a CR2032 button cell, recorded as a No. 2 battery, and tested. The electrolyte used was 1 mol L -1 NaClO4, the solvent is EC / PC, the volume ratio of the two is 1:1, 5% FEC is used as an additive, and the separator is glass fiber GF / D; finally, the assembled battery is left for more than 12 hours for electrochemical performance testing.

[0057] Figure 2It is the XRD diagram. Curve 1 corresponds to the product of test 1, and curve 2 corresponds to the product of the comparative test. It can be observed that there is no obvious difference between the two, but the product of the comparative test has impurity peaks, indicating that Fe doping can improve the purity of the material to a certain extent.

[0058] Figure 3 The figure is a comparison curve of the battery rate performance. Curve 1 (black) is for battery No. 1 and curve 2 (red) is for battery No. 2. Table 1 shows the rate performance data of battery No. 1. It can be seen that in terms of rate performance, battery No. 1 retains 53.37 mAh g at a high current density of 1000 mA / g. -1 Specific capacity, 1000mAg -1 The specific capacity is 10mAg -1 The rate performance is improved by 50.04% which is a considerable improvement.

[0059] Table 1

[0060] <![CDATA[Current density / mAg -1 > 10 20 50 100 200 500 1000 <![CDATA[Specific capacity / mAh g -1 > 106.66 94.51 83.38 75.33 68.51 55.07 53.37

[0061] Table 2 is the rate performance data of No. 2 battery. It can be seen that in terms of rate performance, for No. 2 battery composed of positive electrode materials without iron addition, at 1000mAg -1 At high current density, only 20.55 mAh g was released. -1 The specific capacity of 1000mA / g is only 10mA g -1 The rate performance is 19.15% which is inferior to that of No. 1 battery.

[0062] Table 2

[0063] <![CDATA[Current density / mA g -1 > 10 20 50 100 200 500 1000 <![CDATA[Specific capacity / mAh g -1 > 107.32 90.61 72.48 59.90 47.25 32.79 20.55

[0064] Figure 4 This is a comparison chart of battery cycle performance, with a current density of 100 mA g -1 , Curve 1 is for battery No. 1, and Curve 2 is for battery No. 2. Table 3 shows the cycle performance data of battery No. 1 (100mA g -1 Cycle 200 times), it can be seen that the discharge capacity of battery No. 1 is 100mA g -1 The capacity can reach 86.15mAhg during the cycle -1 , and the capacity retention rate reaches 65.21%, indicating that the battery has excellent cycle performance.

[0065] Table 3

[0066] <![CDATA[Initial discharge capacity / mAhg -1 > <![CDATA[Discharge capacity after cycling / mAh g -1 > Capacity retention rate 86.15 51.18 65.21%

[0067] Table 4 is the cycle performance data of No. 2 battery (100mAg -1Cycle 200 times), it can be seen that the discharge capacity of battery No. 2 is 100mA g -1 The capacity during the cycle is only 74.92 mAhg -1 , and the capacity retention rate is only 14.15%, indicating that the cycle performance of battery No. 2 is poor.

[0068] Table 4

[0069] <![CDATA[Initial discharge capacity / mAh g -1 > <![CDATA[Discharge capacity after cycling / mAh g -1 > Capacity retention rate 74.92 10.60 14.15%

[0070] Figure 5 The cyclic voltammetry curve of the battery, curve 1 is battery No. 1, and curve 2 is battery No. 2. It can be observed that the peak intensity of the third pair of redox peaks (representing the P2→O2 phase transition) of battery No. 1 is significantly reduced, indicating that the degree of the P2→O2 phase transition of the material is reduced, and the potential difference between the first two pairs of oxidation peaks and reduction peaks is smaller, indicating that the polarization is smaller; and the peak shape is sharper, indicating a faster reaction rate.

Claims

1. A method for preparing a layered oxide composite material as a positive electrode for a sodium ion battery, characterized in that The preparation method of the layered oxide type composite material as the positive electrode of the sodium ion battery is carried out according to the following steps:

1. Co-precipitation to obtain a precursor: add ammonia water to deionized water to make the pH value be 10.8-11.2, then add a metal salt solution, and then add alkali solution to adjust the pH value to 10.6-10.8 for co-precipitation, continue stirring for 12h-16h for aging, and then filter, wash and dry in sequence to obtain a precursor; The solute in the metal salt solution is composed of a nickel source, a manganese source and an iron source, and the ratio of the amount of nickel element in the nickel source, the amount of manganese element in the manganese source and the amount of iron element in the iron source is 0.33:0.67-x:x, x≤0.1; The sum of the molar concentrations of nickel, manganese and iron in the metal salt solution is 2 mol / L to 2.5 mol / L; The volume ratio of the deionized water to the metal salt solution is 1:(2.09-3.01); 2. The precursor prepared in step 1 is mixed evenly with the metal salt of the sodium source, and pre-reacted at 450°C to 500°C for 5h to 5.5h, and then heated to 850°C to 900°C and kept warm for 16h to 17h, and naturally cooled to room temperature, and then taken out and fully ground to obtain a layered oxide type positive electrode material; The ratio of the amount of the sodium element in the sodium source to the sum of the three metal elements in the precursor is (1.05-1.1):1; The reaction atmosphere during the entire reaction process of step 2 is air.

2. The method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery according to claim 1, characterized in that The alkali solution described in step 1 is 10 mol L -1 of sodium hydroxide solution and 0.2 mol L -1 Ammonia water is mixed in a volume ratio of 7:

3.

3. The method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery according to claim 1, characterized in that The washing described in step 1 is washing with deionized water.

4. The method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery according to claim 1, characterized in that The drying temperature in step 1 is 100° C. and the drying time is 12 h.

5. The method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery according to claim 1, characterized in that The nickel source described in step 1 is nickel acetate tetrahydrate, nickel nitrate hexahydrate, nickel chloride hexahydrate or nickel sulfate hexahydrate.

6. The method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery according to claim 1, characterized in that The manganese source described in step 1 is manganese acetate tetrahydrate, manganese chloride tetrahydrate or manganese sulfate monohydrate.

7. The method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery according to claim 1, characterized in that The iron source described in step 1 is ferrous oxalate dihydrate or ferrous sulfate heptahydrate.

8. The method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery according to claim 1, characterized in that The sodium source described in step 2 is sodium acetate, sodium citrate, sodium carbonate, sodium bicarbonate or sodium hydroxide.

9. The method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery according to claim 1, characterized in that The ratio of the amount of the sodium element in the sodium source described in step 2 to the sum of the three metal elements in the precursor is 1.05:

1.

10. The method for preparing a layered oxide composite material as a positive electrode of a sodium ion battery according to claim 1, characterized in that In step 2, the pre-reaction is first carried out at 450° C. for 5 h, then the temperature is raised to 850° C. and kept for reaction for 16 h, and then naturally cooled to room temperature. After being taken out, it is fully ground to obtain a layered oxide-type positive electrode material.

Citation Information

Patent Citations

  • Preparation method of sodium ion battery polyanionic composite material

    CN114203996A

  • A P2 and P3 mixed-phase layered oxide cathode material for sodium-ion batteries, its preparation method and application

    CN114937774A

  • Precursor of sodium ion positive electrode material, preparation method and positive electrode material

    CN114956202A

  • Sodium-ion battery positive electrode material with stable oxygen variable valence and preparation method of sodium-ion battery positive electrode material

    CN115020676A

  • Multi-strategy modified cobalt-doped coated single-crystal layered oxide sodium-ion battery positive electrode material

    CN115881920A

Cited By

  • High-nickel ternary modified layered oxide positive electrode material and preparation method and application thereof