High-nickel layered oxide positive electrode material coated with Li3Al1-xMxF6 layer and preparation method

By forming a Li3Al1-xMxF6 cladding with high electron conductivity and ionic conductivity on the positive electrode material of high nickel ternary lithium-ion battery, the problems of stability and capacity attenuation of positive electrode material under high voltage are solved, and a higher cycle life is achieved and capacity retention rate, suitable for industrial applications.

CN118983435AActive Publication Date: 2024-11-19QINGHAI UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411065890.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing high-voltage ternary lithium-ion battery positive electrode materials have problems such as body-phase structure decay, interface environment deterioration, poor stability and capacity attenuation under high pressure, which limits its application, and the existing coating modification method is complex and not suitable for large-scale production. .

Method used

Li3Al1-xMxF6 layer is used as the cladding layer, and a cladding layer with high electron conductivity and ionic conductivity is formed on the surface of the high nickel layered oxide LiNix1Coy1Mn1-x1-y1O2, and magnesium, iron, chromium, lanthanum, cerium, and yttrium are used. The same-element-doped Li3AlF6 is modified based on the preparation of the liquid phase method and high-temperature sintering technology to form a uniform coating to isolate the electrolyte and inhibit side reactions.

Benefits of technology

It improves the cycle stability and specific capacity of the positive electrode material, extends the cycle life of the battery, realizes the increase of the charging cut-off voltage and the increase of the capacity retention rate under high voltage, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983435A_ABST
    Figure CN118983435A_ABST
Patent Text Reader

Abstract

The invention provides a high-nickel layered oxide positive electrode material coated with a Li3Al1-xMxF6 layer and a preparation method of the high-nickel layered oxide positive electrode material, a high-nickel layered oxide is LiNix1Coy1Mn1-x1-y1O2, M is one or more of Mg, Fe, Cr, La, Ce and Y, x is greater than 0 and less than or equal to 0.1, and a coating layer has relatively high conductivity; during preparation, the high-nickel layered oxide powder is added into a mixed aqueous solution of a metal salt, a lithium salt, ammonium fluoride and an aluminum salt, the molar ratio of the lithium salt to the ammonium fluoride to the aluminum salt is 3: 6: (0.9-1), the metal salt is one or more of a magnesium salt, an iron salt, a chromium salt, a lanthanum salt, a cerium salt and an yttrium salt, the mixed system is stirred, then centrifugation and drying are performed in sequence, and a precursor is obtained; and carrying out high-temperature calcination treatment on the precursor at 300-800 DEG C in a protective atmosphere to obtain the high-nickel layered oxide, so that the electrochemical performance of the high-nickel ternary lithium ion battery positive electrode material under high pressure can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium ion batteries, and in particular to a 3 Al 1-x M x F 6 Layered high nickel layered oxide positive electrode material and preparation method. Background Art

[0002] In recent years, the environmental problems caused by the use of traditional fossil fuels have received much attention. Therefore, new energy vehicles have successively replaced current fuel vehicles, which has brought new opportunities for the development and application of lithium-ion batteries. At the same time, it has also put forward higher requirements for their energy density, service life, safety and cost. At present, the research and development of new lithium battery materials, battery structure design, battery performance improvement and battery cost control have become the key technologies for the future development of lithium-ion batteries. Among them, the positive electrode material has a vital impact on the safety performance, cycle performance and energy density of lithium-ion batteries. Therefore, high-performance positive electrode materials are one of the important directions in the field of lithium-ion batteries.

[0003] Ternary cathode material LiNi x Co y Mn z O 2 (NCM) is considered to be the most promising candidate for high-performance cathode materials due to its high energy density and rate performance. At present, the development direction of ternary materials is mainly to increase the working voltage, but there are still many serious problems with ternary materials under high voltage. For example, under high voltage, the body structure decay and interface environment deterioration faced by ternary cathode materials lead to shortened battery life; poor stability and serious capacity attenuation restrict the application of materials.

[0004] The purpose of alleviating and suppressing the serious problems of high-voltage ternary materials can be achieved by one or more methods such as structural modification of the secondary agglomerate particles of high-voltage ternary cathode materials, doping other elements in the layered structure, coating the surface of the material with a stable film layer, and preparing an excellent high-voltage electrolyte. Among them, surface coating is one of the most common modification methods. It can physically block the direct contact between the electrode active material and the electrolyte, which is beneficial to inhibit the decomposition of the electrolyte, reduce the dissolution of active transition metal ions in the electrode material, and weaken the interface side reactions. For example, patent CN 112366297 A discloses a method for surface coating modification of high-nickel ternary cathode materials. A layered high-voltage resistant cathode material with a molecular formula of Li(Ni 0.8 Co 0.1 Mn 0.1 ) 1-x M x O 2@Z, 0.005≤x≤0.02, the doping element M is one or more of Ti, Cr, V, Al, Mg, F, B, and Z is a material that can combine with lithium to form lithium oxide. This modification method focuses on the surface improvement of high-nickel ternary materials, while slowing down the side reactions between the electrolyte and the material surface, stabilizing the crystal structure of the positive electrode material, and reducing lithium-nickel mixing. However, since it relies on joint modification by doping and coating, the sample preparation process is relatively complicated and is not suitable for large-scale production. Patent CN 117254015 A reports a cadmium sulfide nanorod coated matrix material LiNi x Co y Mn z O 2 The preparation method of cadmium sulfide nanorods has a large specific surface area, which is conducive to improving the reaction activity and adsorption performance; the high-nickel ternary positive electrode material coated with cadmium sulfide nanorods can effectively realize the regulation of electronic structure, improve the stability of the material, and improve the electronic conductivity of the positive electrode material. Therefore, after the positive electrode material prepared by the invention is assembled into a battery, the battery capacity retention rate is high and the stability is improved. However, the invention has certain limitations in improving the electrochemical performance of high-nickel ternary materials, especially the coating layer has almost no ionic conductivity. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides a Li-coated 3 Al 1-x M x F 6 Layered high nickel layered oxide positive electrode material and preparation method, coating layer Li 3 Al 1-x M x F 6 It has high electronic conductivity and ionic conductivity, and can improve the electrochemical performance of high-nickel layered oxides, the positive electrode materials of high-nickel ternary lithium-ion batteries, under high voltage.

[0006] The present invention is achieved through the following technical solutions:

[0007] A Li-coated 3 Al 1-x M x F 6 A high nickel layered oxide positive electrode material, wherein the high nickel layered oxide is LiNi x1 Co y1 Mn 1-x1-y1 O 2 , M is one or more of Mg, Fe, Cr, La, Ce and Y, 0<x≤0.1.

[0008] Preferably, x1 and y1 satisfy the following relationship:

[0009] 0.5≤x1<1,0≤y1≤0.2.

[0010] A Li-coated 3 Al 1-x M x F 6 The method for preparing a high nickel layered oxide positive electrode material comprises the following steps:

[0011] S1, adding the high-nickel layered oxide powder to a mixed aqueous solution of a metal salt, a lithium salt, ammonium fluoride and an aluminum salt, wherein the molar ratio of the lithium salt, the ammonium fluoride and the aluminum salt is 3:6:(0.9-1), and the metal salt is one or more of a magnesium salt, an iron salt, a chromium salt, a lanthanum salt, a cerium salt and a yttrium salt, to obtain a mixed system;

[0012] S2, stirring the mixed system, and then centrifuging and drying in sequence to obtain a precursor;

[0013] S3, calcining the precursor at 300°C to 800°C under a protective atmosphere to obtain a Li-coated 3 Al 1-x M x F 6 Layered high nickel layered oxide positive electrode material.

[0014] Preferably, the magnesium salt, iron salt, chromium salt, lanthanum salt, cerium salt, yttrium salt, lithium salt and aluminum salt described in S1 are all corresponding nitrates.

[0015] Further, the aluminum nitrate is Al(NO 3 ) 3 9H 2 O, S1 medium-high nickel layered oxide powder and lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of O is 1:(0.001~0.1):(0.001~0.1):(0.001~0.05).

[0016] Preferably, when the metal salt in S1 is a magnesium salt, an iron salt, a chromium salt, a lanthanum salt, a cerium salt or a yttrium salt, the molar ratio of the aluminum salt to the magnesium salt, the iron salt, the chromium salt, the lanthanum salt, the cerium salt or the yttrium salt is (0.9-1):(0-0.1);

[0017] When the metal salt in S1 is a plurality of magnesium salts, iron salts, chromium salts, lanthanum salts, cerium salts and yttrium salts, the molar ratio of the aluminum salt to the corresponding salt is (0.9-1):(0-0.1).

[0018] Preferably, the stirring in S2 is performed at 20°C to 90°C for 1 h to 6 h.

[0019] Preferably, the drying in S2 is performed at 60° C. to 70° C. for 11 h to 13 h.

[0020] Preferably, the precursor described in S3 is calcined at a high temperature of 300° C. to 800° C. for 2 h to 12 h.

[0021] Preferably, the temperature of 300°C to 800°C in S3 is increased from room temperature at a rate of 2°C / min to 10°C / min.

[0022] Compared with the prior art, the present invention has the following beneficial technical effects:

[0023] The present invention is a Li-coated 3 Al 1-x M x F 6 Layered high nickel layered oxide cathode material, Li 3 Al 1-x M x F 6 As a coating layer, it can simply and effectively isolate the high nickel layered oxide LiNi as the positive electrode material x1 Co y1 Mn 1-x1-y1 O 2 The coating layer can weaken the volume change of the bulk structure of the electrode material, which will help maintain the stability of its layered structure, thereby improving the transmission environment of lithium ions and achieving the goal of stabilizing the electrode material structure and improving its cycle stability. 3 Al 1-x M x F 6 The cladding layer is more suitable as a high-voltage coating material than traditional inert coatings because 3 AlF 6 Doping with magnesium, as well as more transition metal elements (Fe, Y and Cr) and rare earth elements La and Ce can further increase Li 3 AlF 6 The thermal stability of the cathode interface ionic conductivity and electronic conductivity. Especially under high pressure, Li 3 Al 1-x M x F 6 It shows great potential as a high-voltage positive electrode coating material, and can successfully increase the charge cut-off voltage to 4.5V. In the voltage range of 2.7 to 4.5V, the capacity retention rate after 200 cycles is as high as over 80%.

[0024] The present invention is a Li-coated 3 Al 1-x M xF 6 Preparation method of high nickel layered oxide positive electrode material, using liquid phase method to prepare Li 3 Al 1-x M x F 6 Layered and high nickel layered oxide LiNi x1 Co y1 Mn 1-x1-y1 O 2 The precursor is then calcined at 300°C to 800°C to obtain Li 3 Al 1-x M x F surface coating, because below 300℃, Li 3 Al 1-x M x F 6 The layer cannot be formed on the NCM surface. When the temperature exceeds 800°C, the excessively high calcination temperature will cause side reactions during the calcination process, generating transition metal oxide particles attached to the surface of the high-nickel layered oxide, affecting the performance of the coating layer and hindering the transmission of lithium ions. Calcination is carried out in a protective atmosphere to avoid the formation of excessive Li on the surface of the high-nickel layered oxide. 3 Al 1-x M x F 6 Particles, resulting in serious agglomeration. Finally, Li 3 Al 1-x M x F 6 The layer is evenly coated on LiNi x1 Co y1 Mn 1-x1-y1 O 2 The surface acts as a physical barrier to isolate LiNi x1 Co y1 Mn 1-x1-y1 O 2 and electrolyte, thereby inhibiting the occurrence of side reactions and the dissolution of transition metals, improving the ionic conductivity, electronic conductivity and structural stability of the material, thereby improving the specific capacity of the high-nickel ternary positive electrode high-voltage lithium ion battery positive electrode material and the cycle life of the material. The preparation method of the present invention is simple, controllable in operation, high in yield, good in repetitive effect, and extremely easy to realize industrialization, which can meet the application needs of high voltage and high specific capacity materials in the market. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a SEM image of the target substance synthesized in Example 7 of the present invention.

[0026] Figure 2 It is a constant current charge and discharge curve diagram of the target substance synthesized in Example 7 of the present invention at a high voltage of 2.7 to 4.5V.

[0027] Figure 3 It is a SEM picture of the target substance synthesized in Comparative Example 1 of the present invention.

[0028] Figure 4 It is a constant current charge and discharge curve diagram of the target substance synthesized in Comparative Example 1 of the present invention at a high voltage of 2.7 to 4.5V.

[0029] Figure 5 It is a cycle-capacity diagram of Example 7 of the present invention and Comparative Example 1 after a long cycle of 200 cycles at a high voltage of 2.7 to 4.5 V. DETAILED DESCRIPTION

[0030] The present invention is further described in detail below in conjunction with the accompanying drawings. It should be understood that the following embodiments are only used to illustrate the present invention, rather than to limit the present invention. All technologies implemented based on the above content of the present invention are included in the scope of protection intended by the present invention.

[0031] The present invention is a Li-coated 3 Al 1-x M x F 6 The high-nickel layered oxide positive electrode material is a high-voltage lithium-ion battery positive electrode material based on surface coating modification. The coating layer is Li 3 Al 1-x M x F 6 , 0<x≤0.1, the matrix is ​​a high nickel layered oxide (chemical formula is LiNi x Co y Mn 1-x-y O 2 , wherein 0.5≤x<1, 0≤y≤0.2, 0<z≤0.3, x+y+z=1), wherein the element M is one or more of Mg, Fe, Cr, La, Ce and Y, in Li 3 AlF 6 Doping with magnesium, as well as more transition metal elements (Fe, Y and Cr) and rare earth elements La and Ce can further increase Li 3 AlF 6 The conductivity of the modified cathode material can be improved, and it helps to improve the electrochemical stability of the cathode material of high-nickel ternary lithium-ion batteries under high voltage. The prepared modified cathode material shows higher capacity and better cycle stability at high cut-off voltage (2.7-4.5V).

[0032] The present invention is a Li-coated 3 Al 1-x M x F 6 The method for preparing a high-nickel layered oxide positive electrode material comprises the following steps:

[0033] (1) High nickel layered oxide positive electrode material powder (chemical formula is LiNi x Co y Mn 1-x-y O 2 , where 0.5≤x<1, 0≤y≤0.2, 0<z≤0.3, x+y+z=1) is added to nitrate (Fe(NO 3 ) 3 9H 2 O、Mg(NO 3 ) 2 6H 2 O and Cr(NO 3 ) 3 9H 2 O) and lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 O aqueous solution, the cathode material powder and lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of O is 1:(0.001~0.1):(0.001~0.1):(0.001~0.05), Al(NO 3 ) 3 9H 2 O, Fe(NO 3 ) 3 9H 2 O、Mg(NO 3 ) 2 6H 2 O and Cr(NO 3 ) 3 9H 2 O、Ce(NO 3 ) 3 6H 2 O、Y(NO 3 ) 3 6H 2 O、La(NO 3 ) 3 6H 2 The molar ratio of O is (0.9~1):(0~0.1):(0~0.1):(0~0.1):(0~0.1):(0~0.1):(0~0.1):(0~0.1).

[0034] (2) The mixed system obtained in step (1) is stirred at a temperature of 20°C to 90°C for 1 h to 6 h, then centrifuged, and then dried at 60°C to 70°C for 11 h to 13 h.

[0035] (3) placing the powder obtained in step (2) into a tubular furnace and subjecting it to high-temperature calcination at 300°C to 800°C in a nitrogen atmosphere for 2h to 12h, heating the powder from room temperature at a heating rate of 2°C / min to 10°C / min, and finally obtaining the modified high-nickel ternary layered oxide positive electrode material.

[0036] Example 1

[0037] This embodiment provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer covering the core; the high nickel layered oxide is LiNi 0.8 Co 0.1 Mn 0.1 O 2 (denoted as NCM811), with an average particle size of 5 μm; the coating layer is Li 3 Al 0.9 Mg 0.1 F 6 ;

[0038] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0039] first step:

[0040] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 O and Mg(NO 3 ) 2 6H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of Al(NO) is 1:0.001:0.001:0.001. 3 ) 3 9H 2 O and Mg(NO 3 ) 2 6H 2 The molar ratio of O is 0.9:0.1.

[0041] Step 2:

[0042] The mixed system obtained in the first step was stirred at 20°C for 1 h, then centrifuged, and then dried at 65°C for 12 h.

[0043] Step 3:

[0044] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 300°C, the calcination time was 2h, and the heating rate was 2°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0045] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6 A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. In the 2.7-4.5V voltage window and at a current density of 0.1C, the first cycle discharge capacity was 209.9mAh / g. At a current density of 1C, the capacity retention rate after 200 cycles was 80.28%.

[0046] Example 2

[0047] This embodiment provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer covering the core; the core is LiNi 0.6 Co 0.2 Mn 0.2 O 2 (denoted as NCM622), with an average particle size of 2.5 μm; the coating layer is Li 3 Al 0.93 Cr 0.07 F 6 ;

[0048] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0049] first step:

[0050] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 O and Cr(NO 3 ) 2 9H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of Al(NO) is 1:0.1:0.1:0.05.3 ) 3 9H 2 O and Cr(NO 3 ) 2 9H 2 The molar ratio of O is 0.93:0.07.

[0051] Step 2:

[0052] The mixed system obtained in the first step was stirred at 90°C for 5 h, then centrifuged and dried at 65°C for 12 h.

[0053] Step 3:

[0054] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 600°C, the calcination time was 12 hours, and the heating rate was 10°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0055] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6 A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. In the 2.7-4.5V voltage window and at a current density of 0.1C, the first cycle discharge capacity was 203.78mAh / g. At a current density of 1C, the capacity retention rate after 200 cycles was 81.53%.

[0056] Example 3

[0057] This embodiment provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer covering the core; the core is LiNi 0.9 Co 0.05 Mn 0.05 O 2 (denoted as NCM955), with an average particle size of 4.5 μm; the coating layer is Li 3 Al 0.95 Fe 0.05 F 6 ;

[0058] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0059] first step:

[0060] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 O and Fe(NO 3 ) 3 9H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of Al(NO 3 ) 3 9H 2 O and Fe(NO 3 ) 3 9H 2 The molar ratio of O is 0.95:0.05.

[0061] Step 2:

[0062] The mixed system obtained in the first step was stirred at 70°C for 3 h, then centrifuged, and then dried at 65°C for 12 h.

[0063] Step 3:

[0064] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 500°C, the calcination time was 10 hours, and the heating rate was 8°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0065] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6 A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. In the 2.7-4.5V voltage window and at a current density of 0.1C, the first cycle discharge capacity was 212.64mAh / g. At a current density of 1C, the capacity retention rate after 200 cycles was 80.76%.

[0066] Example 4

[0067] This embodiment provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer covering the core; the core is LiNi 0.8 Co 0.1 Mn 0.1 O 2 (denoted as NCM811), with an average particle size of 5 μm; the coating layer is Li 3 Al 0.96 Cr 0.02 Mg 0.02 F 6 ;

[0068] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0069] first step:

[0070] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 O、Cr(NO 3 ) 3 9H 2 O and Mg(NO 3 ) 2 6H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of Al(NO) is 1:0.03:0.06:0.01. 3 ) 3 9H 2 O、Cr(NO 3 ) 3 9H 2 O and Mg(NO 3 ) 2 6H 2 The molar ratio of O is 0.96:0.02:0.02.

[0071] Step 2:

[0072] The mixed system obtained in the first step was stirred at 60°C for 2 h, then centrifuged, and then dried at 65°C for 12 h.

[0073] Step 3:

[0074] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 450°C, the calcination time was 8 hours, and the heating rate was 6°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0075] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6 A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. In the 2.7-4.5V voltage window and a current density of 0.1C, the first cycle discharge capacity was 210.10mAh / g. At a current density of 1C, the capacity retention rate after 200 cycles was 80.56%.

[0076] Example 5

[0077] This embodiment provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer covering the core; the core is LiNi 0.6 Co 0.2 Mn 0.2 O 2 (denoted as NCM622), with an average particle size of 2.5 μm; the coating layer is Li 3 Al 0.96 Cr 0.02 Fe 0.02 F 6 ;

[0078] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0079] first step:

[0080] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 O、Cr(NO 3 ) 3 9H 2 O and Fe(NO 3 ) 3 9H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO3 ) 3 9H 2 The mass ratio of Al(NO) is 1:0.03:0.06:0.01. 3 ) 3 9H 2 O、Cr(NO 3 ) 3 9H 2 O and Fe(NO 3 ) 3 9H 2 The molar ratio of O is 0.96:0.02:0.02.

[0081] Step 2:

[0082] The mixed system obtained in the first step was stirred at 40°C for 4 h, then centrifuged, and then dried at 65°C for 12 h.

[0083] Step 3:

[0084] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 350°C, the calcination time was 5 hours, and the heating rate was 3°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0085] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6 A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. In the 2.7-4.5V voltage window and at a current density of 0.1C, the first cycle discharge capacity was 204.23mAh / g. At a current density of 1C, the capacity retention rate after 200 cycles was 81.92%.

[0086] Example 6

[0087] This embodiment provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer covering the core; the core is LiNi 0.5 Co 0.2 Mn 0.3 O 2 (denoted as NCM523), with an average particle size of 1.5 μm; the coating layer is Li 3 Al0.94 Cr 0.02 Fe 0.02 Mg 0.02 F 6 ;

[0088] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0089] first step:

[0090] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 O、Cr(NO 3 ) 3 9H 2 O, Fe(NO 3 ) 3 9H 2 O and Mg(NO 3 ) 2 6H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of Al(NO) is 1:0.03:0.06:0.01. 3 ) 3 9H 2 O、Cr(NO 3 ) 3 9H 2 O、Mg(NO 3 ) 2 6H 2 O and Fe(NO 3 ) 3 9H 2 The molar ratio of O is 0.94:0.02:0.02:0.02.

[0091] Step 2:

[0092] The mixed system obtained in the first step was stirred at 30°C for 4 h, then centrifuged and dried at 65°C for 12 h.

[0093] Step 3:

[0094] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 550°C, the calcination time was 10 hours, and the heating rate was 5°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0095] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6 A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. In the 2.7-4.5V voltage window and at a current density of 0.1C, the first cycle discharge capacity was 214.78mAh / g. At a current density of 1C, the capacity retention rate after 200 cycles was 82.23%.

[0096] Example 7

[0097] This embodiment provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer covering the core; the core is LiNi 0.5 Co 0.2 Mn 0.3 O 2 (denoted as NCM523), with an average particle size of 1.5 μm; the coating layer is Li 3 Al 0.96 Fe 0.02 Mg 0.02 F 6 ;

[0098] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0099] first step:

[0100] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 O, Fe(NO 3 ) 3 9H 2 O and Mg(NO 3 ) 2 6H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of Al(NO) is 1:0.03:0.06:0.01. 3 ) 3 9H 2O, Fe(NO 3 ) 3 9H 2 O and Mg(NO 3 ) 2 6H 2 The molar ratio of O is 0.96:0.02:0.02.

[0101] Step 2:

[0102] The mixed system obtained in the first step was stirred at 80°C for 6 h, then centrifuged and dried at 65°C for 12 h.

[0103] Step 3:

[0104] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 400°C, the calcination time was 6 hours, and the heating rate was 5°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0105] The target product obtained in this embodiment is coated with Li 3 Al 0.96 Fe 0.02 Mg 0.02 F 6 High nickel layered oxide LiNi 0.5 Co 0.2 Mn 0.3 O 2 The positive electrode material was scanned by electron microscope, and the results were as follows Figure 1 shown; through Figure 1 High nickel layered oxide LiNi 0.5 Co 0.2 Mn 0.3 O 2 Still maintaining a good polygonal structure, Li 3 Al 0.96 Fe 0.02 Mg 0.02 F 6 The modification of the layer did not affect the high nickel layered oxide LiNi 0.5 Co 0.2 Mn 0.3 O 2 affects the crystal structure.

[0106] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. At a voltage window of 2.7 to 4.5 V and a current density of 0.1 C, Figure 2 As shown, the first cycle discharge capacity is 215.50mAh / g, at a current density of 1C. Figure 5 As shown, the capacity retention rate after 200 cycles is 85.89%.

[0107] Example 8

[0108] This embodiment provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer covering the core; the core is LiNi 0.6 Co 0.2 Mn 0.2 O 2 (denoted as NCM622), with an average particle size of 2.5 μm; the coating layer is Li 3 Al 0.96 Cr 0.02 Ce 0.02 F 6 ;

[0109] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0110] first step:

[0111] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 O、Cr(NO 3 ) 3 9H 2 O and Ce(NO 3 ) 3 6H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of Al(NO) is 1:0.03:0.06:0.01. 3 ) 3 9H 2 O、Cr(NO 3 ) 3 9H 2 O and Ce(NO 3 ) 3 6H2 The molar ratio of O is 0.96:0.02:0.02.

[0112] Step 2:

[0113] The mixed system obtained in the first step was stirred at 50°C for 3 h, then centrifuged, and then dried at 65°C for 12 h.

[0114] Step 3:

[0115] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 400°C, the calcination time was 4h, and the heating rate was 5°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0116] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6 A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. In the 2.7-4.5V voltage window and at a current density of 0.1C, the first cycle discharge capacity was 204.79mAh / g. At a current density of 1C, the capacity retention rate after 200 cycles was 82.22%.

[0117] Example 9

[0118] This embodiment provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer covering the core; the core is LiNi 0.8 Co 0.1 Mn 0.1 O 2 (denoted as NCM811), with an average particle size of 5 μm; the coating layer is Li 3 Al 0.96 Y 0.02 Mg 0.02 F 6 ;

[0119] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0120] first step:

[0121] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride, Al(NO 3 )3 9H 2 O、Y(NO 3 ) 3 6H 2 O and Mg(NO 3 ) 2 6H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of Al(NO) is 1:0.03:0.06:0.01. 3 ) 3 9H 2 O、Y(NO 3 ) 3 6H 2 O and Mg(NO 3 ) 2 6H 2 The molar ratio of O is 0.96:0.02:0.02.

[0122] Step 2:

[0123] The mixed system obtained in the first step was stirred at 50°C for 5 h, then centrifuged and dried at 65°C for 12 h.

[0124] Step 3:

[0125] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 450°C, the calcination time was 5 hours, and the heating rate was 6°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0126] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6 A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. In the 2.7-4.5V voltage window and at a current density of 0.1C, the first cycle discharge capacity was 211.12mAh / g. At a current density of 1C, the capacity retention rate after 200 cycles was 81.26%.

[0127] Example 10

[0128] This embodiment provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer covering the core; the core is LiNi 0.6 Co 0.2 Mn 0.2 O 2 (denoted as NCM622), with an average particle size of 2.5 μm; the coating layer is Li 3 Al 0.93 La 0.07 F 6 ;

[0129] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0130] first step:

[0131] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 O and La (NO 3 ) 3 6H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of Al(NO) is 1:0.1:0.1:0.05. 3 ) 3 9H 2 O and La (NO 3 ) 3 6H 2 The molar ratio of O is 0.93:0.07.

[0132] Step 2:

[0133] The mixed system obtained in the first step was stirred at 80°C for 4 h, then centrifuged and dried at 65°C for 12 h.

[0134] Step 3:

[0135] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 500°C, the calcination time was 10 hours, and the heating rate was 10°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0136] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6 A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. In the 2.7-4.5V voltage window and at a current density of 0.1C, the first cycle discharge capacity was 202.92mAh / g. At a current density of 1C, the capacity retention rate after 200 cycles was 81.22%.

[0137] Comparative Example 1

[0138] This comparative example provides a coated modified lithium ion battery positive electrode material. The positive electrode material comprises a high nickel layered oxide positive electrode material powder as a core and a coating layer coating the core; the core is LiNi 0.5 Co 0.2 Mn 0.3 O 2 (denoted as NCM523), with an average particle size of 1.5 μm; the coating layer is Li 3 AlF 6 ;

[0139] The method for preparing the coated lithium ion battery positive electrode material comprises the following steps:

[0140] first step:

[0141] The high nickel layered oxide cathode material powder was added with lithium nitrate, ammonium fluoride and Al(NO 3 ) 3 9H 2 O in an aqueous solution, and all the powders are weighed in a certain proportion. Among them, the positive electrode material powder is mixed with lithium nitrate, ammonium fluoride, Al(NO 3 ) 3 9H 2 The mass ratio of O is 1:0.03:0.06:0.01.

[0142] Step 2:

[0143] The mixed system obtained in the first step was stirred at 80°C for 6 h, then centrifuged and dried at 65°C for 12 h.

[0144] Step 3:

[0145] The powder obtained in the second step was placed in a tube furnace and subjected to high-temperature calcination treatment in a nitrogen atmosphere, wherein the calcination temperature was 400°C, the calcination time was 6 hours, and the heating rate was 5°C / min. Finally, the modified high-nickel ternary layered oxide positive electrode material was obtained.

[0146] The target product obtained in this comparative example is coated with Li 3 AlF 6 High nickel layered oxide LiNi 0.5 Co 0.2 Mn 0.3 O 2 The positive electrode material was scanned by electron microscope, and the results were as follows Figure 3 shown; through Figure 3 High nickel layered oxide LiNi 0.5 Co 0.2 Mn 0.3 O 2 Still maintaining a good polygonal structure, Li 3 AlF 6 The modification of the layer did not affect the high nickel layered oxide LiNi 0.5 Co 0.2 Mn 0.3 O 2 affects the crystal structure.

[0147] The electrochemical performance of the obtained coated modified lithium-ion battery positive electrode material was tested. The electrode sheet ratio was a lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1; the metal lithium sheet was the counter electrode, the polypropylene microporous membrane Celgard2400 was the diaphragm, and 1 mol / L LiPF 6 A CR2032 button cell was prepared using an aqueous solution (in which EC, DEC and DMC were dissolved in a volume ratio of 1:1:1) as the electrolyte. The battery was subjected to constant current charge and discharge tests using the LAND battery test system. At a voltage window of 2.7 to 4.5 V and a current density of 0.1 C, Figure 4 As shown, the first cycle discharge capacity is 199.70 mAh / g, at a current density of 1C. Figure 5 As shown, the capacity retention rate after 200 cycles is 78.57%, while the capacity retention rate of NCM523 after 200 cycles at a current density of 1C is only 46.0%.

[0148] From the comparison between Example 7 and Comparative Example 1, it can be seen that in Li 3 AlF 6 Compared with pure Li, the modified materials doped with Fe and Mg in the coating layer 3 AlF 6 The coated modified material has higher capacity and higher capacity retention after 200 cycles.

[0149] In summary, the present invention introduces Li 3 Al 1-x M x F 6 The coating layer modifies the positive electrode material of high nickel ternary lithium ion battery, improves the ionic conductivity and structural stability of the material, thereby improving the specific capacity and cycle life of the material. 3 Al 1-x M x F 6 The coating layer can serve as a physical barrier to isolate the positive electrode material from the electrolyte, thereby inhibiting the occurrence of side reactions and the dissolution of transition metals. Through the above modification strategy, the coated positive electrode material obtained by the present invention has better conductivity, specific capacity and longer cycle life when used as a positive electrode material for lithium-ion batteries.

[0150] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A Li3Al coated 1-x M x The high nickel layered oxide positive electrode material of the F6 layer is characterized by: The high nickel layered oxide is LiNi x1 Co y1 Mn 1-x1-y1 O2, M is one or more of Mg, Fe, Cr, La, Ce and Y, 0<x≤0.

1.

2. The Li3Al coated according to claim 1 1-x M x The high nickel layered oxide positive electrode material of the F6 layer is characterized by: x1 and y1 satisfy the following relationship respectively: 0.5≤x1<1,0≤y1≤0.

2.

3. A Li3Al coated substrate as claimed in any one of claims 1 to 2 1-x M x The method for preparing a high-nickel layered oxide positive electrode material of the F6 layer is characterized in that: The steps include: S1, adding the high-nickel layered oxide powder to a mixed aqueous solution of a metal salt, a lithium salt, ammonium fluoride and an aluminum salt, wherein the molar ratio of the lithium salt, the ammonium fluoride and the aluminum salt is 3:6:(0.9-1), and the metal salt is one or more of a magnesium salt, an iron salt, a chromium salt, a lanthanum salt, a cerium salt and a yttrium salt, to obtain a mixed system; S2, stirring the mixed system, and then centrifuging and drying in sequence to obtain a precursor; S3, calcining the precursor at 300°C to 800°C under a protective atmosphere to obtain a Li3Al 1- x M x F6 layer of high nickel layered oxide positive electrode material.

4. The Li3Al coated according to claim 3 1-x M x The method for preparing a high-nickel layered oxide positive electrode material of the F6 layer is characterized in that: The magnesium salt, iron salt, chromium salt, lanthanum salt, cerium salt, yttrium salt, lithium salt and aluminum salt described in S1 are all corresponding nitrates.

5. The Li3Al coated according to claim 4 1-x M x The method for preparing a high-nickel layered oxide positive electrode material of the F6 layer is characterized in that: The aluminum nitrate is Al(NO3)3·9H2O, and the mass ratio of the high nickel layered oxide powder in S1 to lithium nitrate, ammonium fluoride and Al(NO3)3·9H2O is 1:(0.001-0.1):(0.001-0.1):(0.001-0.05).

6. The Li3Al coated according to claim 3 1-x M x The method for preparing a high-nickel layered oxide positive electrode material of the F6 layer is characterized in that: When the metal salt in S1 is a magnesium salt, an iron salt, a chromium salt, a lanthanum salt, a cerium salt or a yttrium salt, the molar ratio of the aluminum salt to the magnesium salt, the iron salt, the chromium salt, the lanthanum salt, the cerium salt or the yttrium salt is (0.9-1):(0-0.1); When the metal salt in S1 is a plurality of magnesium salts, iron salts, chromium salts, lanthanum salts, cerium salts and yttrium salts, the molar ratio of the aluminum salt to the corresponding salt is (0.9-1):(0-0.1).

7. The Li3Al coated according to claim 3 1-x M x The method for preparing a high-nickel layered oxide positive electrode material of the F6 layer is characterized in that: The stirring in S2 is performed at 20°C to 90°C for 1 h to 6 h.

8. The Li3Al coated according to claim 3 1-x M x The method for preparing a high-nickel layered oxide positive electrode material of the F6 layer is characterized in that: The drying described in S2 is performed at 60°C to 70°C for 11 h to 13 h.

9. The Li3Al coated according to claim 3 1-x M x The method for preparing a high-nickel layered oxide positive electrode material of the F6 layer is characterized in that: The precursor described in S3 is calcined at a high temperature of 300°C to 800°C for 2h to 12h.

10. The Li3Al coated substrate according to claim 3 1-x M x The method for preparing a high-nickel layered oxide positive electrode material of the F6 layer is characterized in that: The temperature of 300°C to 800°C described in S3 is increased from room temperature at a rate of 2°C / min to 10°C / min.

Citation Information

Patent Citations

  • High-nickel ternary positive electrode material coated with fast ion conductor, preparation method thereof, and lithium ion battery prepared from material

    CN109879331A

  • Nickel-cobalt-manganese-tantalum composite quaternary positive electrode material coated with fast ion conductor and preparation method thereof

    CN112670506A

  • Ternary composite material for all-solid-state battery as well as preparation method and application of ternary composite material

    CN114614012A