Manufacturing method of micro-textured current collector

By designing a micro-shaped structure on the lithium-ion battery current collector substrate and optimizing the spacing between protrusions and depressions, the problem of insufficient adhesion of positive and negative electrode materials is solved, and the charging and discharging efficiency and life of the battery are improved.

CN118983449APending Publication Date: 2024-11-19RONGENE NEW MATERIALS (BEIJING) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411128366.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, the current collector adhesion of the positive and negative electrode materials of lithium-ion batteries is weak, resulting in low charging and discharging efficiency and short life of the battery, especially the problem of the positive electrode material detachment and low utilization of the negative electrode material after the cycle test.

Method used

By designing a micro-shaped structure on the current collector substrate, the rows of protrusions and depressions are arranged, and the two are spaced apart from each other. The horizontal and longitudinal spacing of protrusions and depressions is optimized to E=F≤1.6*H, ensuring that the protrusions and depressions are The height and depth are the same, and the outer diameter is the same, forming a micro-shaped current collector to enhance the capacity of the positive electrode material.

Benefits of technology

Reduced the lateral and longitudinal spacing of micro-shaped current collector pits and protrusions, solved the problem of lithium electrode film analysis, improved the capacity of the positive electrode material, and maintained the adhesion of the negative electrode material, avoided excessive negative electrode material Lithium excretion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983449A_ABST
    Figure CN118983449A_ABST
Patent Text Reader

Abstract

The invention relates to a manufacturing method of a micro-textured current collector. The manufacturing method of the micro-texturing current collector comprises the following steps: obtaining a current collector base material; based on the current collector base material, obtaining protrusions and recesses on the surface of the current collector base material; wherein the bulges are arranged in rows, the recesses are also arranged in rows, and the bulges and the recesses are positioned in different rows and are arranged at intervals; the distance from the protrusion to the nearest recess in the transverse direction is set as F, the distance from the protrusion to the nearest recess in the longitudinal direction is set as E, and E is equal to F; the height of the bulge and the depth of the recess are the same and are both set as G, and the outer diameter of the bulge and the outer diameter of the recess are the same and are both set as H; according to the manufacturing method of the micro-textured current collector, the transverse and longitudinal distances between the pits and the bosses of the micro-textured current collector are reduced, so that the adhesive force of a pole piece is not reduced, the problem of lithium precipitation of the pole piece is solved, and the gram volume of a positive electrode material is slightly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of current collectors for secondary ion batteries, and in particular relates to a method for manufacturing a micro-shaped current collector. Background Art

[0002] The positive and negative electrode materials of batteries, such as lithium-ion and sodium-ion batteries, have weak adhesion to the current collector, which affects the high-current charging and discharging efficiency and life of the battery. After the battery completes the cycle test, the positive electrode material detaches from the aluminum foil surface, and the negative electrode material also has the same problem.

[0003] Patent No. CN112808771A discloses a technical solution. Specifically, the invention discloses a method for staggered rolling of a surface textured current collector foil, comprising the following steps:

[0004] Step 1: Place two smooth rollers on a CNC lathe and use laser texturing to process annular protrusions of a predetermined size and distribution position on the roller surface. The protrusion design is shown in Figure 1 , where 1 is roller 1, 2 is roller 2, 3 is foil, h is the lateral distance of the roller protrusion, and the embodiment shows that h is 200um, S t1 , S t1 is the longitudinal distance of the rollers, and the embodiment shows that S t1 is 100um, S t2 is 60 to 140 um, d is the protrusion diameter, and the embodiment shows that d is 50 um;

[0005] Step 2: Assemble the prepared roller pair on the rolling mill, adjust the relative positions of the two rollers so that the annular protrusions on the surfaces of the two rollers are staggered, and then pass the foil through the gap between the two rollers, apply rolling force to form a surface roughening structure consisting of non-penetrating pits on the upper and lower surfaces of the foil, and the surface shape of the foil can be seen. Figure 2 , where 3-1 is a protrusion, 3-2 is a pit, and the distance between the center points of adjacent protrusions and pits is ≥100um;

[0006] Patent No. JPH08195202A discloses a technical solution, which has two rollers, one roller has a protrusion, and the other roller has a hard rubber outer layer. After the aluminum foil passes through the two rollers, one side is a protrusion and the other side is a pit. In the embodiment, the outer diameter of the protrusion is 20um, and the protrusion spacing is 100um;

[0007] However, patents CN112808771A and JPH08195202A have similar problems. Patent CN112808771A is used for illustration. The outer diameter of the root of the roller protrusion in the public solution is 50um. When rolling the foil, pits will be rolled on the foil. The outer diameter of the pit mouth is actually 20-30um. The average diameter of the ternary and lithium cobalt oxide positive electrode material particles is about 12um, the diameter of lithium iron phosphate particles is about 6um, and the diameter of the negative electrode particles is about 18um, so the positive and negative electrode particles will fall into the pits. Figure 3 As shown, 401-403 are positive electrode sheets, 404 is a separator, and 405-406 are negative electrode sheets. Compared with the flat part of the aluminum foil 402, there are fewer positive electrode particles in the convex part of 403, and more positive electrode particles in the concave part of 407. After being assembled into a battery, when charging, the lithium ions in the positive electrode particles migrate to the negative electrode through the separator and enter the interior of the negative electrode particles. There are too many positive electrode particles in the concave part of 407, and the corresponding negative electrode cannot provide enough particles to absorb the lithium ions migrated from the positive electrode. The lithium ions are deposited on the surface of the negative electrode particles to form dead lithium, causing capacity loss. There are fewer positive electrode particles in the convex part of 403, and the corresponding negative electrode part has redundant negative electrode particles, resulting in low utilization of negative electrode particles. Summary of the invention

[0008] The purpose of the present invention is to provide a method for manufacturing a micro-shaped current collector with a simple structure and reasonable design in order to solve the above problems. The method of the present application can solve the problem of lithium deposition in the corresponding negative electrode part due to excessive positive electrode particles in the pits.

[0009] The present invention achieves the above-mentioned purpose through the following technical solutions:

[0010] A method for manufacturing a micro-shaped current collector, the method comprising the following steps:

[0011] obtaining a current collector substrate;

[0012] Based on the current collector substrate, protrusions and depressions on its surface are obtained;

[0013] The protrusions are arranged in a row, and the depressions are also arranged in a row. The two are located in different rows but are spaced apart from each other.

[0014] The distance from the protrusion to the nearest depression in the horizontal direction is set to F, and the distance in the vertical direction is set to E, and E is equal to F.

[0015] As a further optimization solution of the present invention, the height of the protrusion is the same as the depth of the depression, both are set to G, and the outer diameter of the protrusion is the same as the outer diameter of the depression, both are set to H.

[0016] As a further optimization scheme of the present invention, the protrusions and depressions in the current collector substrate satisfy: E=F≤1.6*H.

[0017] As a further optimization scheme of the present invention, the protrusions and depressions in the current collector substrate satisfy: E=F=1.0*H.

[0018] As a further optimization scheme of the present invention, the protrusions and depressions in the current collector substrate satisfy: E=F=1.2*H.

[0019] As a further optimization scheme of the present invention, the protrusions and depressions in the current collector substrate satisfy: E=F=1.4*H.

[0020] As a further optimization scheme of the present invention, the protrusions and depressions in the current collector substrate satisfy: E=F=1.6*H.

[0021] As a further optimization scheme of the present invention, a positive electrode sheet and a negative electrode sheet are obtained; and the battery component is assembled based on the positive electrode sheet and the negative electrode sheet.

[0022] As a further optimization scheme of the present invention, the preparation of the positive electrode sheet is to prepare a slurry with a mass ratio of NCA: CNT: KS-6: PVDF = 97.8: 0.5: 0.5: 1.2; obtain an aluminum foil substrate of 12um, and coat the slurry on the current collector substrate by a coating method to prepare an NCA single-sided positive electrode sheet, and the surface density of the sheet material is 22.19 mg / cm 2 ; After rolling, the thickness of the positive electrode sheet is 73um.

[0023] As a further optimization scheme of the present invention, the preparation of the negative electrode sheet is to prepare a slurry with a mass ratio of silicon carbon: carbon black: CMC: SBR = 95.1:1:1.6:2.3; obtain a copper foil substrate of 8um, and coat the slurry on the copper foil by a coating method to prepare a silicon carbon single-sided negative electrode sheet, and the surface density of the electrode sheet material is 11.5mg / cm 2 ; After rolling, the thickness of the negative electrode sheet is 80um.

[0024] The beneficial effect of the present invention is that the present invention reduces the lateral and longitudinal spacings of the micro-shaped current collector pits and bosses, thereby solving the problem of lithium plating on the pole pieces without reducing the adhesion of the pole pieces and slightly improving the gram capacity of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the overall structure in CN112808771A, a comparative document of the present invention;

[0026] Figure 2 It is a schematic diagram of the foil surface shape in the reference document CN112808771A of the present invention;

[0027] Figure 3 It is a diagram of the pairing of positive and negative electrode materials of the present invention;

[0028] Figure 4 It is the lithium electron concentration difference diffusion path diagram of the present invention;

[0029] Figure 5 This is the micro-shaped current collector structure intention of the present invention;

[0030] Figure 6 It is a schematic flow chart of the method for making the micro-shaped current collector of the present invention;

[0031] Figure 7 Schematic diagram of the excess coefficient of the negative electrode of the present invention;

[0032] Figure 8 It is the embodiment scheme table data of the present invention;

[0033] Fig. 9 The positive electrode sheet adhesion test table data of each embodiment of the present invention;

[0034] Fig.10 It is the data of the positive electrode gram capacity performance table of each embodiment of the present invention;

[0035] Fig.11 The data of the battery lithium deposition table of each embodiment of the present invention;

[0036] Fig.12 It is a lithium electron migration path diagram of the present invention. DETAILED DESCRIPTION

[0037] The present application is further described in detail below in conjunction with the accompanying drawings. It is necessary to point out here that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technical personnel in this field can make some non-essential improvements and adjustments to the present application based on the above application content.

[0038] Conduct experimental verification based on the problems in the background technology;

[0039] 1. Production of positive electrode

[0040] A. Preparation of slurry: prepare slurry with a mass ratio of NCA:CNT:KS-6:PVDF=97.8:0.5:0.5:1.2;

[0041] B. Preparation of CN 112808771A positive electrode sheet: Aluminum foil substrate 12um, foil material is prepared according to patent number CN 112808771A, boss height 12um, boss lateral spacing 180um, boss longitudinal spacing 130um, the slurry in step A is coated on the foil by coating method, and NCA single-sided positive electrode sheet is prepared, and the surface density of the electrode sheet material is 22.19mg / cm2; by rolling, the thickness of the positive electrode sheet after rolling is 73um;

[0042] C. Preparation of conventional positive electrode sheet: The aluminum foil substrate is 12um. The slurry in step A is coated on the foil by coating to prepare the NCA single-sided positive electrode sheet. The surface density of the sheet material is 22.19mg / cm2. After rolling, the thickness of the positive electrode sheet is 73um.

[0043] 2. Production of negative electrode

[0044] A. Preparation of slurry: prepare slurry with a mass ratio of silicon carbon: carbon black: CMC: SBR = 95.1:1:1.6:2.3;

[0045] B. Preparation of negative electrode sheet: conventional copper foil substrate 8um, the slurry in step A is coated on conventional copper foil by coating method to prepare silicon-carbon single-sided negative electrode sheet, the surface density of the sheet material is 11.5mg / cm2; after rolling, the thickness of the negative electrode sheet is 80um;

[0046] Negative electrode excess coefficient Figure 7 ;

[0047] Assemble the battery according to Table 2

[0048] Table 2 Battery assembly plan

[0049]

[0050] 3. Battery Test

[0051] A Battery positive electrode capacity test

[0052] Solution No. Positive electrode capacity mAh / g Solution 1 183.39 Solution 2 185.41

[0053] B charges the battery to 4.25V, disassembles the battery, and observes the lithium deposition on the negative electrode.

[0054] Solution No. Is lithium deposited on the negative electrode? Solution 1 Lithium Separation Solution 2 No lithium precipitation

[0055] Therefore, it is shown that the above problem does exist; and the present invention defines the foil with protrusions and pits on the foil surface as micro-shaped foil, which solves the problem of lithium deposition at the corresponding negative electrode due to excessive positive electrode particles in the pits. Fig.12In the structure shown in FIG. 1 , when charging, the lithium ions in the pit of the positive electrode sheet 507 migrate vertically to the surface of the negative electrode under the action of the electric field force, causing the lithium ion concentration at the corresponding negative electrode site to be higher than that at other sites; the lithium ion concentration at the negative electrode site corresponding to the protrusion 503 is lower. Due to the difference in concentration, the lithium ions diffuse from the site with high concentration to the site with low concentration, but the diffusion path is too long and cannot reach the negative electrode site corresponding to the protrusion 503, causing lithium precipitation. Figure 4 As shown in the figure, the distance between the protrusions and the pits is shortened to 50um. During charging, the six lithium ions in the pits in the figure migrate vertically to the corresponding negative electrode surface under the action of the electric field. Under the traction of the concentration diffusion force, two lithium ions are diffused to the corresponding negative electrode part of the protrusion, and the lithium ions are evenly distributed on the negative electrode sheet.

[0056] refer to Figure 6 The present invention discloses a method for manufacturing a micro-shaped current collector, which comprises the following steps:

[0057] Step S102, obtaining a current collector substrate;

[0058] Step S104, based on the current collector substrate, obtaining protrusions 701 and depressions 702 on its surface;

[0059] The protrusions 701 are arranged in a row, and the depressions 702 are also arranged in a row. The two are located in different rows but are spaced apart from each other.

[0060] The distance from the protrusion 701 to the nearest depression 702 in the horizontal direction is set to F, and the distance in the vertical direction is set to E, and E is equal to F;

[0061] Step S106, preparing the battery based on the current collector substrate.

[0062] It should be noted that the current collector substrate refers to the structure or part that collects current. In lithium-ion batteries, it mainly refers to metal foil, such as copper foil and aluminum foil. In this solution, the current collector substrate refers to aluminum foil. Of course, it can also be used in other metal foils such as copper foil.

[0063] Furthermore, the height of the protrusion 701 is the same as the depth of the recess 702, both of which are set to G, and the outer diameter of the protrusion 701 is the same as the outer diameter of the recess 702, both of which are set to H.

[0064] In this embodiment, the protrusion 701 and the boss have the same meaning, and the depression 702 and the pit also have the same meaning. Figure 4 and Figure 5 As shown in the schematic diagram, a current collector with the following parameters is prepared: boss height = pit depth = G = 12 um, boss outer diameter = pit outer diameter = H = 50 um;

[0065] Among them, according to the sequence numbers 1-6, prepare respectively:

[0066] The protrusions 791 and the depressions 702 in the current collector substrate satisfy: E = F = 1.0 * H = 50 um;

[0067] The protrusions 791 and the depressions 702 in the current collector substrate satisfy: E = F = 1.2*H = 60 um;

[0068] The protrusions 791 and the depressions 702 in the current collector substrate satisfy: E = F = 1.4 * H = 70 um;

[0069] The protrusions 791 and the depressions 702 in the current collector substrate satisfy: E = F = 1.6 * H = 80 um;

[0070] The protrusions 791 and the depressions 702 in the current collector substrate satisfy: E = F = 1.8 * H = 90 um;

[0071] The protrusions 791 and the depressions 702 in the current collector substrate satisfy: E = F = 2.0 * H = 100 um;

[0072] Obtain a positive electrode sheet and a negative electrode sheet; and assemble the battery component based on the positive electrode sheet and the negative electrode sheet.

[0073] The positive electrode sheet is prepared by preparing a slurry with a mass ratio of NCA: CNT: KS-6: PVDF = 97.8: 0.5: 0.5: 1.2; obtaining an aluminum foil substrate of 12um, coating the slurry on the current collector substrate by a coating method, and preparing an NCA single-sided positive electrode sheet, the surface density of the sheet material is 22.19 mg / cm 2 ; After rolling, the thickness of the positive electrode sheet is 73um.

[0074] Preparation of conventional positive electrode sheets: Aluminum foil substrate is 12um, and the above slurry is coated on the foil by coating to prepare NCA single-sided positive electrode sheets, and the surface density of the sheet material is 22.19mg / cm2; by rolling, the thickness of the positive electrode sheet after rolling is 73um.

[0075] The negative electrode sheet is prepared by preparing a slurry with a mass ratio of silicon carbon: carbon black: CMC: SBR = 95.1:1:1.6:2.3; obtaining a copper foil substrate of 8um, coating the slurry on the copper foil by a coating method, and preparing a silicon carbon single-sided negative electrode sheet, the surface density of the electrode sheet material is 11.5mg / cm 2 ; After rolling, the thickness of the negative electrode sheet is 80um.

[0076] Calculation of excess capacity coefficient of negative electrode: See the negative electrode excess coefficient Figure 7 .

[0077] The above positive and negative electrodes are used to prepare batteries and test battery performance. The data of the embodiment scheme can be referred to Figure 8 Data shown;

[0078] The adhesion of the positive electrode sheets of each embodiment was tested by the Hundred Grid Method. The test results can be referred to Fig. 9 The data shown; from Fig. 9 From the above, it can be seen that the reduction of the lateral and longitudinal spacing between pits and bosses has no obvious effect on the adhesion, and both are higher than those of conventional aluminum foil.

[0079] Charge the battery to 4.2V at 0.5C constant current and constant voltage, cut off current 0.05C, leave for 5 minutes, discharge at 0.5C constant current to 3.0V, positive electrode material gram capacity = battery discharge capacity / positive electrode coating weight / positive electrode active material ratio, for details, please refer to Fig.10 The data in the table of positive electrode capacity in grams is shown; from Fig.10 It can be seen that in Example 1, when the lateral spacing and longitudinal spacing of the bosses and recesses and the outer diameters of the bosses and recesses are equal, the gram capacity of the positive electrode material is slightly higher than the gram capacity of the positive electrode material of the conventional foil in the comparison example. This is because the micro-shaped foil improves adhesion, improves electron transfer efficiency, and improves the gram capacity of the battery.

[0080] Charge the battery to 4.25V, disassemble the battery, and observe the lithium deposition on the negative electrode. For details, please refer to Fig.11 From the data shown, it can be found that the conventional aluminum foil battery negative electrode sheet of comparative example 1 does not deposit lithium, and the lateral and longitudinal spacings between the bosses and pits in examples 1 and 2 are relatively small, and the negative electrode sheet does not deposit lithium; from examples 3 to 6, as the lateral and longitudinal spacings between the bosses and pits increase, the lithium deposition on the negative electrode sheet becomes more and more serious.

[0081] It should be noted that when using the method for making the micro-shaped current collector, the present invention solves the problem of lithium plating on the electrode sheet without reducing the adhesion of the electrode sheet by reducing the lateral and longitudinal spacing of the micro-shaped current collector pits and bosses, and slightly improves the gram capacity of the positive electrode material.

[0082] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily referring to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.

[0083] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

[0084] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A method for making a micro-shaped current collector, characterized in that: The Method The following steps are included: obtaining a current collector substrate; Based on the current collector substrate, protrusions and depressions on its surface are obtained; The protrusions are arranged in a row, and the depressions are also arranged in a row. The two are located in different rows but are spaced apart from each other. The distance from the protrusion to the nearest depression in the horizontal direction is set to F, and the distance in the vertical direction is set to E, and E is equal to F.

2. The method for manufacturing a micro-shaped current collector according to claim 1, characterized in that: The height of the protrusion is the same as the depth of the depression, both of which are set to G, and the outer diameter of the protrusion is the same as the outer diameter of the depression, both of which are set to H.

3. The method for making a micro-shaped current collector according to claim 2, characterized in that: The protrusions and depressions in the current collector substrate satisfy: E=F≤1.6*H.

4. The method for making a micro-shaped current collector according to claim 3, characterized in that: The protrusions and depressions in the current collector substrate satisfy: E=F=1.0*H.

5. The method for manufacturing a micro-shaped current collector according to claim 3, characterized in that: The protrusions and depressions in the current collector substrate satisfy: E=F=1.2*H.

6. The method for manufacturing a micro-shaped current collector according to claim 3, characterized in that: The protrusions and depressions in the current collector substrate satisfy: E=F=1.4*H.

7. The method for manufacturing a micro-shaped current collector according to claim 2, characterized in that: The protrusions and depressions in the current collector substrate satisfy: E=F=1.6*H.

8. The method for manufacturing a micro-shaped current collector according to claim 1, characterized in that: Obtain a positive electrode sheet and a negative electrode sheet; and assemble the battery component based on the positive electrode sheet and the negative electrode sheet.

9. The method for manufacturing a micro-shaped current collector according to claim 8, characterized in that: The positive electrode sheet is prepared by preparing a slurry with a mass ratio of NCA: CNT: KS-6: PVDF = 97.8: 0.5: 0.5: 1.2; obtaining an aluminum foil substrate of 12um, coating the slurry on the current collector substrate by a coating method, and preparing an NCA single-sided positive electrode sheet, the surface density of the sheet material is 22.19 mg / cm 2 ; After rolling, the thickness of the positive electrode sheet is 73um.

10. The method for manufacturing a micro-shaped current collector according to claim 8, characterized in that: The negative electrode sheet is prepared by preparing a slurry with a mass ratio of silicon carbon: carbon black: CMC: SBR = 95.1:1:1.6:2.3; obtaining a copper foil substrate of 8um, coating the slurry on the copper foil by a coating method, and preparing a silicon carbon single-sided negative electrode sheet, the surface density of the electrode sheet material is 11.5mg / cm 2 ; After rolling, the thickness of the negative electrode sheet is 80um.