Preparation of lithium manganese iron phosphate battery electrolyte
By using trimethylsilyl and lone pair electron N or P functional additives in the electrolyte of lithium manganese iron phosphate battery, combined with high-temperature stability solvent and lithium salt, the poor performance of lithium manganese iron phosphate battery materials at high temperatures is solved. The problem is to improve the battery's high temperature and circulation performance.
Patent Information
- Application Number
- CN202411069932.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
Lithium manganese iron phosphate battery materials have poor performance at high temperatures, and Mn dissolution, Jahn-Teller effect, side reactions and low ionic conductivity lead to poor cycle and rate performance, limiting its application development.
Additives containing trimethylsilyl (TMS) functional groups and lone pair electron N or P functional groups are used to combine high-temperature stable fluorinated solvents and lithium salts to form TMSF and macromolecule film formation, inhibit Mn dissolution and SEI damage, and improve SEI The membrane is stable and the electrolyte is prevented from contacting the positive electrode directly through the polymer.
Effectively inhibit Mn dissolution, improve the high temperature and circulation performance of lithium manganese iron phosphate batteries, enhance the internal stability of the battery, and extend the life.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to the preparation of an electrolyte for a lithium manganese iron phosphate battery. Background Art
[0002] Compared with NCM, lithium iron phosphate and lithium iron manganese phosphate, the olivine structure lattice stability of lithium iron manganese phosphate material is better than the ternary layered structure, and it has better cycle performance; due to the synergistic effect of Mn and Fe in lithium iron manganese phosphate material, Fe and Mn can be dissolved in any ratio to form a solid solution. Combined with the stable electrochemical properties of lithium iron phosphate and the high voltage advantage of lithium manganese phosphate, lithium iron manganese phosphate has higher energy density and higher safety than lithium iron phosphate, and the voltage platform voltage can reach 4.1V.
[0003] In terms of application, lithium manganese iron phosphate has lower electronic conductivity and lithium ion diffusion rate than lithium iron phosphate materials, which affects the rate performance, and the electrochemical properties of the materials are different due to the different proportions of manganese ions in the materials. For example, if the proportion of manganese ions is too low, it will affect the improvement of energy density and voltage platform, and it will not be able to achieve ideal material performance. However, if the proportion is too high, it will easily promote the Jan-Taylor effect, resulting in material lattice distortion and manganese dissolution, which will affect the cycle stability. Therefore, it is necessary to develop a lithium manganese iron phosphate battery electrolyte that can improve the battery cycle and rate performance. Summary of the invention
[0004] The inventors found that driven by environmental protection and carbon emission pressure, research on new energy sources is being actively carried out. Among them, lithium-ion batteries have attracted much attention in the field of energy storage and power due to their high specific energy, long cycle life, low self-discharge, and good safety performance. Lithium manganese iron phosphate can be positioned as an upgraded version of lithium iron phosphate, combining the advantages of high safety of lithium iron phosphate and high energy density of ternary materials. Theoretically, when the ratio of manganese to iron is 7:3, the performance is improved by 13% to 18% compared with lithium iron, and the performance can be improved by 21% when all manganese is replaced. Lithium manganese phosphate has the advantages of high voltage platform and high energy density, and can be mixed with ternary materials in different proportions to increase the gram capacity without greatly affecting the high voltage platform of ternary materials, making up for the shortcomings of lithium iron phosphate.
[0005] There are still some problems with lithium manganese iron phosphate positive electrode materials: (1) dissolution of Mn2+ in the electrolyte; (2) JahnTeller effect generated by Mn3+, which aggravates the dissolution of Mn, migrates to the surface of the negative electrode material, and destroys the SEI film; (3) side reactions with the electrolyte, generating products such as Li4P2O7, and the positive electrode material gradually loses its activity; (4) low ionic conductivity and electronic conductivity; (5) poor high-temperature performance of lithium manganese iron phosphate. These problems lead to poor actual specific capacity, rate performance and cycle performance of this type of material, which restricts its further development.
[0006] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to propose a preparation of a lithium manganese iron phosphate electrolyte, which can solve the problem of Mn dissolution in the electrode, is crucial to improving the performance of LMFP batteries, and is economical, effective and fast.
[0007] In the first aspect of the present invention, the present invention proposes a lithium iron manganese phosphate battery electrolyte. According to an embodiment of the present invention, the lithium iron manganese phosphate battery electrolyte includes an additive, which is a mixture of one or more of trimethylsilyl acetate, acetoxymethyl trimethoxysilane, acetoxyethyl trimethoxysilane, acetoxymethyl triethoxysilane, (acetoxy) acetoxyethyl dimethylchlorosilane, 2-acetoxyethyl trichlorosilane tetrafluoroethyl trifluoroethyl ether, tetrafluoroethyl tetrafluoropropyl ether, tetrafluoroethyl ethyl ether, tetrafluoroethyl methyl ether, and difluoroanisole.
[0008] According to an embodiment of the present invention, the above-mentioned lithium manganese iron phosphate battery electrolyte may further include at least one of the following additional technical features:
[0009] According to an embodiment of the present invention, the additive is trimethylsilyl methyl acetate, acetoxymethyl trimethoxysilane or tetrafluoroethyl tetrafluoropropyl ether.
[0010] According to an embodiment of the present invention, an additive is applied to a lithium iron manganese phosphate electrolyte, wherein the additive contains a trimethylsilyl (TMS) functional group and an N or P functional group having a lone pair of electrons. The trimethylsilyl (TMS) is connected to N or P and has high activity. It defluorinates F- with a lithium salt (LiPF6 or LiFSI) or a fluorinated solvent (such as a fluorinated solvent with high temperature stability provided by the present invention) commonly used in the electrolyte to form TMSF and other macromolecular film-forming components, which can effectively isolate the positive electrode from the electrolyte, prevent the free F- ions from corroding and damaging the lithium iron manganese phosphate material, thereby effectively inhibiting the dissolution of manganese; in addition, the N or P bond having a lone pair of electrons has a strong oxidizing property, which can inhibit the Mn 3+ Disproportionation reaction occurs to generate Mn 2+ and Mn 4+ions, further reducing Mn dissolution, reducing free Mn ions in the electrolyte, preventing Mn from being reduced and precipitated at the negative electrode, and avoiding damage caused by SEI; at the same time, the additive has a macromolecular structure (C≥7) with 1 to 3 trimethylsilyl groups, or a long chain structure. The additive is easy to polymerize with the solvent and the electrolyte lithium salt to form a dense macromolecular polymer, which can further effectively prevent the electrolyte from directly contacting the positive electrode material and inhibit the dissolution of the transition metal Mn. In addition, the additive of the structure of the present invention is used in combination with conventional basic film-forming additives to inhibit the precipitation of transition metal Mn at the negative electrode, improve the stability of the SEI film and reduce the loss of capacity, improve the stability of the entire battery internal system, and thus improve the high temperature and cycle performance of the lithium manganese iron phosphate battery.
[0011] According to an embodiment of the present invention, the lithium manganese iron phosphate battery electrolyte further includes a lithium salt and a carbonate solvent.
[0012] According to an embodiment of the present invention, the lithium salt is one or a mixture of lithium hexafluorophosphate (LiPF6), lithium difluorooxalate borate (LiDFOB), lithium tetrafluoroborate (LiBF4), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium difluorophosphate (LiPO2F2), lithium bisoxalate borate (LiBOB), lithium bisfluorosulfonyl imide (LiFSI), lithium trifluoromethanesulfonate (LiSO3CF3). According to an embodiment of the present invention, the lithium salt of the present invention is not limited thereto, and any existing lithium salt for lithium batteries can be used.
[0013] According to an embodiment of the present invention, the carbonate solvent is ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC) or ethyl propyl carbonate (EPC).
[0014] According to an embodiment of the present invention, based on the total weight of the electrolyte, the content of the basic solvent is 10-30%, for example, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, but not limited thereto.
[0015] According to an embodiment of the present invention, based on the total weight of the electrolyte, the additive may account for 0.5% to 2% of the total mass of the electrolyte, for example, 0.5% to 1.9%, 0.6% to 1.8%, 0.7% to 1.7%, 0.8% to 1.6%, 1.0% to 1.4% or a combination of the above ranges.
[0016] In another aspect of the present invention, the present invention also proposes a method for preparing the above-mentioned lithium manganese iron phosphate battery electrolyte. According to an embodiment of the present invention, the method comprises the following steps:
[0017] In a glove box filled with argon, the water content and oxygen content are controlled below 0.1ppm, the basic solvent and the high-temperature stable solvent are mixed evenly, and the mixed solvent is placed in a low-temperature environment for cooling, and then lithium salt is slowly added. After the lithium salt is completely dissolved, the basic film-forming additive and the additives described above are added, and after stirring evenly and dissolving fully, a lithium manganese iron phosphate battery electrolyte is obtained.
[0018] In another aspect of the present invention, the present invention further provides a lithium iron manganese phosphate battery. According to an embodiment of the present invention, the lithium iron manganese phosphate battery comprises the lithium iron manganese phosphate battery electrolyte described above.
[0019] According to an embodiment of the present invention, the above-mentioned lithium manganese iron phosphate battery may further include at least one of the following additional technical features:
[0020] According to an embodiment of the present invention, the lithium manganese iron phosphate battery further includes a positive electrode membrane.
[0021] According to an embodiment of the present invention, the material of the positive electrode membrane is lithium manganese iron phosphate.
[0022] According to an embodiment of the present invention, the lithium manganese iron phosphate battery further includes a negative electrode material.
[0023] According to an embodiment of the present invention, the negative electrode material may be any one selected from graphite, porous carbon, soft carbon, hard carbon, and mesophase carbon microbeads.
[0024] According to an embodiment of the present invention, the lithium manganese iron phosphate battery further includes a separator.
[0025] According to an embodiment of the present invention, the diaphragm is polyethylene, polypropylene or a polyethylene-polypropylene composite diaphragm.
[0026] According to the embodiment of the present invention, the positive electrode sheet, the negative electrode sheet and the assembly of the battery can be prepared by any method known in the art.
[0027] According to an embodiment of the present invention, the preparation steps of the positive electrode sheet are as follows: the positive electrode material, the conductive agent and the binder are evenly mixed, and then they are dispersed in N-methyl-2-pyrrolidone (NMP) to obtain a positive electrode slurry, and then the slurry is evenly coated on both sides of the aluminum foil, and the positive electrode sheet is obtained after drying and rolling.
[0028] According to an embodiment of the present invention, the steps for preparing the negative electrode sheet are as follows: the negative electrode material, the conductive agent and the binder are evenly mixed, and then they are dispersed in deionized water to obtain a negative electrode slurry, and then the slurry is evenly coated on both sides of the aluminum foil, and the negative electrode sheet is obtained after drying and rolling.
[0029] According to an embodiment of the present invention, the preparation steps of a lithium manganese iron phosphate battery are as follows: stack the positive electrode sheet, the diaphragm, and the negative electrode sheet in order, ensure that the diaphragm separates the positive electrode sheet and the negative electrode sheet, and the negative electrode sheet completely wraps the positive electrode sheet, and then put the stacked battery cell into an aluminum-plastic film packaging bag, and then inject the above-prepared electrolyte into the battery cell. After formation, the lithium manganese iron phosphate battery is made after sealing, aging, double sealing and capacity division and other processes.
[0030] According to the embodiments of the present invention, the present invention has at least one of the following technical effects:
[0031] (1) Adding an additive having a structure shown in Formula I to the electrolyte of the present invention can effectively inhibit manganese dissolution, reduce free Mn ions in the electrolyte, prevent Mn from being reduced and precipitated at the negative electrode, and avoid damage to SEI; at the same time, the polymer additive-N / P bond is easily polymerized with the solvent and the electrolyte lithium salt to form a dense macromolecular polymer, which can further effectively prevent the electrolyte from directly contacting the positive electrode and inhibit the dissolution of the transition metal Mn.
[0032] (2) The additive of the structure shown in Formula I provided by the present invention is used in combination with conventional film-forming additives in the negative electrode film formation, which can inhibit the precipitation of transition metal Mn at the negative electrode, improve the stability of the SEI film and reduce the loss of capacity, and improve the stability of the entire battery internal system, thereby improving the high temperature and cycle performance of the lithium manganese iron phosphate battery.
[0033] (3) The addition of a high-temperature stable organic solvent to the electrolyte of the present invention has a good effect of inhibiting the dissolution of Mn, and is not easily oxidized and gasified under high-temperature conditions, thereby reducing the corrosion of the lithium manganese iron phosphate material. DETAILED DESCRIPTION
[0034] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0035] Example 1
[0036] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salt is lithium hexafluorophosphate (LiPF6), the concentration is 1mol / L, the organic solvent is dimethyl carbonate (DMC): ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, 0.5% by mass of trimethylsilyl acetate was added, and the electrolyte was obtained by shaking evenly.
[0037] Example 2
[0038] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salt is lithium hexafluorophosphate (LiPF6), the concentration is 1mol / L, the organic solvent is dimethyl carbonate (DMC): ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, 1.5% by mass of trimethylsilyl acetate was added, and the prepared electrolyte was obtained by shaking evenly.
[0039] Example 3
[0040] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salt is lithium hexafluorophosphate (LiPF6), the concentration is 1mol / L, the organic solvent is dimethyl carbonate (DMC): ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, 0.5% by mass of acetoxymethyltrimethoxysilane is added, and shaken evenly to obtain the prepared electrolyte.
[0041] Example 4
[0042] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salt is lithium hexafluorophosphate (LiPF6), the concentration is 1mol / L, the organic solvent is dimethyl carbonate (DMC): ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, 0.5% by mass of acetoxymethyltrimethoxysilane is added, and shaken evenly to obtain the prepared electrolyte.
[0043] Example 5
[0044] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salt is lithium hexafluorophosphate (LiPF6), the concentration is 1mol / L, the organic solvent is dimethyl carbonate (DMC): ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, 0.5% by mass of tetrafluoroethyl tetrafluoropropyl ether was added, and the prepared electrolyte was obtained by shaking evenly.
[0045] Example 6
[0046] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salt is lithium hexafluorophosphate (LiPF6), the concentration is 1mol / L, the organic solvent is dimethyl carbonate (DMC): ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, add 1.5% by mass of tetrafluoroethyl tetrafluoropropyl ether, shake evenly to obtain the prepared electrolyte.
[0047] Example 7
[0048] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salt is lithium hexafluorophosphate (LiPF6), the concentration is 1mol / L, the organic solvent is dimethyl carbonate (DMC): propylene carbonate (PC) = 7:3 (volume ratio), mixed evenly, 0.5% by mass of trimethylsilyl acetate was added, and the electrolyte was obtained by shaking evenly.
[0049] Example 8
[0050] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salt is lithium hexafluorophosphate (LiPF6), the concentration is 1mol / L, the organic solvent is dimethyl carbonate (DMC): propylene carbonate (PC) = 7:3 (volume ratio), mixed evenly, 1.5% by mass of trimethylsilyl acetate was added, and the electrolyte was obtained by shaking evenly.
[0051] Example 9
[0052] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salts are lithium bis(oxalatoborate) (LiBOB) and lithium tetrafluoroborate (LiBF4), with concentrations of 0.8mol / L and 0.2mol / L respectively, and organic solvents are ethyl methyl carbonate (EMC):ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, 1.5% by mass of trimethylsilyl acetate was added, and the prepared electrolyte was obtained by shaking evenly.
[0053] Example 10
[0054] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salts are lithium bis(oxalatoborate) (LiBOB) and lithium tetrafluoroborate (LiBF4), with concentrations of 0.8mol / L and 0.2mol / L respectively, and organic solvents are dimethyl carbonate (DMC):ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, 1.5% by mass of acetoxymethyltrimethoxysilane is added, and the prepared electrolyte is obtained by shaking evenly.
[0055] Embodiment 11
[0056] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salts are lithium bis(oxalatoborate) (LiBOB) and lithium tetrafluoroborate (LiBF4), with concentrations of 0.8mol / L and 0.2mol / L respectively, and organic solvents are dimethyl carbonate (DMC): propylene carbonate (PC) = 7:3 (volume ratio), mixed evenly, 1.5% by mass of tetrafluoroethyl tetrafluoropropyl ether is added, and the prepared electrolyte is obtained by shaking evenly.
[0057] Example 12
[0058] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), the lithium salt is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) with a concentration of 1.5mol / L, the organic solvent is ethyl methyl carbonate (EMC):ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, 1.5% by mass of trimethylsilyl acetate was added, and the prepared electrolyte was obtained by shaking evenly.
[0059] Embodiment 13
[0060] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), the lithium salt is lithium bistrifluoromethanesulfonyl imide (LiTFSI) with a concentration of 1.5mol / L, the organic solvent is dimethyl carbonate (DMC):ethylene carbonate (EC) = 7:3 (volume ratio) and mixed evenly, 1.5% by mass of acetoxymethyltrimethoxysilane is added, and the prepared electrolyte is obtained by shaking evenly.
[0061] Embodiment 14
[0062] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), the lithium salt is lithium bistrifluoromethanesulfonyl imide (LiTFSI) with a concentration of 1.5mol / L, the organic solvent is dimethyl carbonate (DMC): ethylene carbonate (EC) = 7:3 (volume ratio), and 1.5% of tetrafluoroethyl tetrafluoropropyl ether is added and shaken to obtain the prepared electrolyte.
[0063] Comparative Example 1
[0064] In an inert glove box filled with argon atmosphere (water < 0.1 ppm, oxygen < 0.1 ppm), lithium salt is lithium hexafluorophosphate (LiPF6), the concentration is 1 mol / L, and the organic solvent is dimethyl carbonate (DMC): ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, and shaken evenly to obtain a basic electrolyte.
[0065] Comparative Example 2
[0066] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), lithium salts are lithium bis(oxalatoborate) (LiBOB) and lithium tetrafluoroborate (LiBF4), with concentrations of 0.8mol / L and 0.2mol / L respectively, and organic solvents are ethyl methyl carbonate (EMC):ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, and shaken evenly to obtain a basic electrolyte.
[0067] Comparative Example 3
[0068] In an inert glove box filled with argon atmosphere (water content <0.1ppm, oxygen content <0.1ppm), the lithium salt is lithium bistrifluoromethanesulfonyl imide (LiTFSI), the concentration is 1.5mol / L, and the organic solvent is dimethyl carbonate (DMC):ethylene carbonate (EC) = 7:3 (volume ratio), mixed evenly, and shaken evenly to obtain a basic electrolyte.
[0069] The electrolyte compositions of Examples 1 to 14 and Comparative Examples 1, 2, and 3 and the performance tests after assembling the batteries are shown in Table 1 below, wherein A, B, and C are trimethylsilyl acetate, acetoxymethyltrimethoxysilane, and tetrafluoroethyltetrafluoropropyl ether, respectively.
[0070] Table 1
[0071]
[0072]
[0073] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
Claims
1. A lithium manganese iron phosphate battery electrolyte, characterized in that: The additive is one or a mixture of several of trimethylsilyl acetate, acetoxymethyltrimethoxysilane, acetoxyethyltrimethoxysilane, acetoxymethyltriethoxysilane, (acetoxy)acetoxyethyldimethylchlorosilane, 2-acetoxyethyltrichlorosilane tetrafluoroethyl-trifluoroethyl ether, tetrafluoroethyl-tetrafluoropropyl ether, tetrafluoroethyl-ethyl ether, tetrafluoroethyl-methyl ether and difluoroanisole.
2. The lithium manganese iron phosphate battery electrolyte according to claim 1, characterized in that: The additive is trimethylsilyl methyl acetate, acetoxymethyl trimethoxysilane or tetrafluoroethyl-tetrafluoropropyl ether.
3. The lithium manganese iron phosphate battery electrolyte according to claim 1, characterized in that: The lithium manganese iron phosphate battery electrolyte further includes a lithium salt and a carbonate solvent.
4. The lithium manganese iron phosphate battery electrolyte according to claim 3, characterized in that: The lithium salt is one of lithium hexafluorophosphate, lithium difluorooxalatoborate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl imide), lithium difluorophosphate, lithium dioxalatoborate, lithium bis(fluorosulfonyl imide), and lithium trifluoromethanesulfonate, or a mixture of several thereof.
5. The lithium manganese iron phosphate battery electrolyte according to claim 3, characterized in that: The carbonate solvent is ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate or ethyl propyl carbonate.
6. The lithium manganese iron phosphate battery electrolyte according to claim 3, characterized in that: Based on the total weight of the electrolyte, the content of the basic solvent is 10-30%.
7. The lithium manganese iron phosphate battery electrolyte according to claim 3, characterized in that: Based on the total weight of the electrolyte, the additive may account for 0.5% to 2% of the total mass of the electrolyte.
8. A method for preparing the lithium manganese iron phosphate battery electrolyte according to any one of claims 1 to 7, comprising: In a glove box filled with argon, the water content and oxygen content are controlled below 0.1ppm, the basic solvent and the high temperature stability solvent are mixed evenly, and the mixed solvent is placed in a low temperature environment for cooling, and then the lithium salt is slowly added. After the lithium salt is completely dissolved, the basic film-forming additive and the additive described in claim 1 are added, and after stirring evenly and fully dissolved, a lithium iron manganese phosphate battery electrolyte is obtained.
9. A lithium manganese iron phosphate battery, characterized in that: The lithium iron manganese phosphate battery comprises the lithium iron manganese phosphate battery electrolyte according to any one of claims 1-7.
10. The lithium manganese iron phosphate battery according to claim 9, characterized in that: The lithium manganese iron phosphate battery further includes a positive electrode membrane; Optionally, the material of the positive electrode membrane is lithium manganese iron phosphate; Optionally, the lithium manganese iron phosphate battery further comprises a negative electrode material; Optionally, the negative electrode material may be any one selected from graphite, porous carbon, soft carbon, hard carbon, and mesophase carbon microspheres; Optionally, the lithium manganese iron phosphate battery further comprises a separator; Optionally, the separator is polyethylene, polypropylene or a polyethylene-polypropylene composite separator.
Citation Information
Patent Citations
LMFP (Li-Mn-Fe Phosphate) battery and electrolyte thereof
CN108808089A
Additive for lithium ion battery electrolyte and lithium iron manganese phosphate battery electrolyte
CN117790906A
Lithium manganese iron phosphate battery electrolyte, preparation method of lithium manganese iron phosphate battery electrolyte and lithium manganese iron phosphate battery containing lithium manganese iron phosphate battery electrolyte
CN117976975A