High-modulus MPI flexible copper-clad plate and preparation method thereof
By using a high-modulus MPI layer of modified polyimide in flexible copper laminate, combining the proportion of fillers and specific monomers, the problem of insufficient dielectric performance and modulus in the prior art is solved, and high frequency and high frequency are achieved Stability and performance improvements in density applications.
Patent Information
- Application Number
- CN202411056507.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
The dielectric performance and modulus of existing flexible copper clad plates are insufficient, which cannot meet the needs of high-frequency and high-speed information processing. Especially in flexible circuit board designs with thin lines, narrow line spacing and high density, the low modulus of the material leads to deformation. , affects connection stability.
Using modified polyimide (MPI) flexible copper clad plate, aprotic pole is used by adding filler and a specific proportion of rigid and flexible diamine monomers to the polyimide precursor and the modified polyimide precursor. and aromatic anhydride monomers form high modulus MPI layers and improve their mechanical and dielectric properties through specific synthesis and coating processes.
It realizes flexible copper clad with excellent dielectric properties and high modulus, reduces dielectric losses, improves mechanical properties, ensures the smoothness and mechanical properties of the material, and is suitable for high-frequency and high-density flexible circuit board applications.
Smart Images

Figure CN118984530A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic materials, and in particular relates to a high modulus MPI flexible copper clad laminate and a preparation method thereof. Background Art
[0002] Flexible copper clad laminate (FCCL) is a key material for the production of flexible printed circuit boards (FPCs), with the characteristics of being soft, light, thin and bendable. With the rapid development of information science and technology, the 5G era has arrived, and information processing has begun to enter a high-frequency and high-speed stage, which has higher requirements for the loss and rate of information transmission, so there are also higher requirements for the performance of flexible copper clad laminates.
[0003] At present, the common flexible insulating materials on the market mainly include liquid crystal polymer (LCP) and polyimide (PI). Although LCP has superior performance, LCP materials have the disadvantages of insufficient production capacity, large investment, complex manufacturing process and high price. The traditional PI film has a large thermal expansion coefficient, poor heat resistance, high dielectric constant and poor mechanical properties, which can no longer meet market demand. Therefore, it has become an industry trend to modify PI to form a modified polyimide (ModifiedPolyimide, referred to as MPI) substrate to improve dielectric properties. Although the cost of MPI is lower than that of LCP, the dielectric loss of MPI flexible copper clad laminate will increase at high frequencies, and the flexible groups in its chemical structure will cause the MPI film to have a lower modulus, which reduces the modulus of the flexible copper clad laminate. Due to the design of flexible circuit boards in recent years, the lines tend to be thinner, the line spacing is narrower, the guide holes are smaller, and the density is higher, and the rigidity of MPI is required more harshly. If the modulus of the flexible copper clad laminate is too low, it means that the material is more likely to deform under external force, and this deformation may cause the connection of downstream products to be unstable, affecting the normal operation of the equipment. Therefore, it is very important to provide an MPI flexible copper clad laminate with excellent dielectric properties and high modulus. Summary of the invention
[0004] The purpose of the present invention is to provide an MPI flexible copper clad laminate with excellent dielectric properties and high modulus in view of the deficiencies in the prior art. The present invention also provides a method for preparing the high modulus MPI flexible copper clad laminate, which is easy to implement and can be mass-produced.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A high modulus MPI flexible copper clad laminate comprises a copper foil layer and an MPI layer coated on the copper foil layer; the MPI layer is prepared by mixing a modified polyimide precursor and a polyimide precursor in a weight ratio of (1-4):1; the polyimide precursor comprises a filler, an aprotic polar solvent, a rigid diamine monomer, a flexible diamine monomer and an aromatic anhydride monomer; the modified polyimide precursor comprises a filler, an aprotic polar solvent, a rigid diamine monomer, Flexible diamine monomer, diamine monomer containing ester group in the main chain and aromatic anhydride monomer; the molar ratio of the sum of the molar numbers of rigid diamine monomer and flexible diamine monomer in the polyimide precursor to the aromatic anhydride monomer is 1:(0.96-1.05); the molar ratio of the sum of the molar numbers of rigid diamine monomer, flexible diamine monomer and diamine monomer containing ester group in the main chain to the aromatic anhydride monomer in the modified polyimide precursor is 1:(0.96-1.05).
[0007] In the present invention, the molar ratio of the rigid diamine monomer to the flexible diamine monomer in the polyimide precursor is (3.5-4.5):1; the molar ratio of the rigid diamine monomer, the flexible diamine monomer and the diamine monomer containing an ester group in the main chain in the modified polyimide precursor is (1.5-2.5):1:2.
[0008] The thickness of the MPI layer is 12-25 μm.
[0009] In the present invention, the solvent is an aprotic polar solvent, and the aprotic polar solvent is one or more of N,N dimethylformamide (DMF), N,N dimethylacetamide (DMAC), and N methylpyrrolidone (NMP). The mass percentage of the aprotic polar solvent in the polyimide precursor or the modified polyimide precursor is 80% to 90%.
[0010] In the present invention, the rigid diamine monomer is one or more of p-phenylenediamine (PPDA), m-phenylenediamine (MPD), 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFMB), and 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl (M-TB);
[0011] The flexible diamine monomer is one or more of 4,4'-diaminodiphenyl ether (ODA), bis(4-aminophenyl) terephthalate (BAPT), p-aminophenyl para-aminobenzoate (APAB), 1,3'-bis(4'-aminophenoxy)benzene (TPE-R), and 2,2'-bis[4-(4-aminophenoxyphenyl)propane] (BAPP);
[0012] The ester-containing diamine monomer is one or more of [4-(4-aminobenzoyl)oxyphenyl]4-aminobenzoate (ABHQ), bis(4-aminophenyl)terephthalate (BAPT), and p-aminophenyl para-aminobenzoate (APAB).
[0013] In the present invention, the aromatic anhydride monomer is selected from one or more of p-phenylene-trimethylene dianhydride (TAHQ), 4,4-oxydiphthalic anhydride (ODPA), bisphenol A diether dianhydride (BPADA), 4,4'-biphenyltetracarboxylic anhydride (BPDA), pyromellitic anhydride (PMDA), 4,4'-biphenyltetracarboxylic anhydride (BPDA), and 3,3',4,4'-benzophenonetetracarboxylic anhydride (BTDA).
[0014] In the present invention, the filler is one or more of silicon dioxide, LCP powder, modified white graphene, and talcum powder, and the mass fraction of the filler is 0 to 6% of the polyimide precursor or the modified polyimide precursor.
[0015] The particle size D of the LCP powder 50 5~10μm;
[0016] The silicon dioxide is Q029 from Suzhou Jinyi New Materials Co., Ltd.;
[0017] The method for preparing the high modulus MPI flexible copper clad laminate of the present invention mainly comprises the following steps:
[0018] S1. Prepare a polyimide precursor mother solution: add the filler to the aprotic polar solvent in proportion, disperse it evenly, add the rigid diamine monomer and the flexible diamine monomer, and stir until the diamine monomer is completely dissolved;
[0019] S2. Synthesis of polyimide precursor: under nitrogen protection, the dried aromatic anhydride monomers are sequentially added to the mother liquor prepared in S1 and stirred. Before adding each new aromatic anhydride monomer, it is necessary to confirm that the added monomer has reacted completely;
[0020] S3. Preparation of modified polyimide precursor mother solution: Add the filler in a non-protonic polar solvent in proportion, disperse evenly, add rigid diamine monomer, flexible diamine monomer and main chain ester-containing diamine monomer, and stir until the diamine monomer is completely dissolved;
[0021] S4. Synthesis of modified polyimide precursor: Under nitrogen protection, the dried aromatic anhydride monomers are sequentially added to the mother liquor prepared in S3 and stirred, and before each addition of new aromatic anhydride monomers, it is necessary to confirm that the added monomers have reacted completely;
[0022] S5. Preparation of mixed glue solution: Under nitrogen protection, the polyimide precursor synthesized in S2 and the modified polyimide precursor synthesized in S4 were added to the flask in proportion and stirred until uniformly mixed;
[0023] S6. Coating and cyclization: The mixed glue solution prepared in S5 is coated on the copper foil layer, dried at high temperature, and imidized to obtain a high modulus MPI single-sided flexible copper clad laminate.
[0024] The temperature of the high-temperature drying in S6 is 150-180° C., and the imidization is carried out in an IR furnace or a non-oxidizing high-temperature oven.
[0025] Furthermore, a nitrogen atmosphere protection is provided in the IR furnace, and the front section, the middle section and the rear section are a baking section, a cyclization section and a cooling section in sequence, the temperature of the cyclization section is 330-380° C., and the processing line speed of the IR furnace is 0.5-4 m / min.
[0026] In the present invention, the material of the copper foil layer is high-frequency copper foil, and further the high-frequency copper foil is one of electrolytic copper and rolled copper. The surface roughness (Rz value) of the copper foil is 1.2-1.5 μm.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The present invention reduces the difference in thermal expansion coefficients between the copper foil and the polyimide layer without sacrificing peel strength by adding a small amount of filler to the polyimide precursor and the modified polyimide precursor, thereby improving the flatness of the board; the filler can limit the movement of the polyimide molecular chain, reduce the slippage and creep between the molecular chains, and thus improve the modulus of the polyimide.
[0029] (2) The present invention blends a polyimide precursor and a modified polyimide precursor, and utilizes the relatively rigid structure of the polyimide precursor to reduce the dielectric constant of the polyimide while slightly increasing the dielectric loss, thereby greatly improving the mechanical properties of the MPI flexible copper clad laminate. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic structural diagram of the high modulus MPI flexible copper clad laminate of the present invention. DETAILED DESCRIPTION
[0031] The present invention will be further described below with reference to specific embodiments, but is not limited thereto.
[0032] The copper foil in the embodiments of the present invention and the comparative examples is 3EC-M2S-THE-SP3, electrolytic copper with a thickness of 1 / 3 oz and a basis weight of 100 g / cm 2The surface roughness (Rz value) is 1.2-1.5 μm. The imidization equipment is an automatic continuous cyclization equipment for flexible copper clad laminates, with a brand name of Fl-cyc-03.
[0033] LCP powder, model LF-31P, particle size 5μm; modified white graphene, model BNS01, flake size 1~5μm; talcum powder, model FKSUSS, particle size 1~2μm.
[0034] In a specific embodiment of the present invention, a method for preparing a high modulus MPI flexible copper clad laminate comprises the following steps:
[0035] S1. Prepare a polyimide precursor mother solution: add the filler to the aprotic polar solvent in proportion, disperse it evenly, add the rigid diamine monomer and the flexible diamine monomer, and stir until the diamine monomer is completely dissolved;
[0036] S2. Synthesis of polyimide precursor: under nitrogen protection, the dried aromatic anhydride monomers are sequentially added to the mother liquor prepared in S1 and stirred. Before adding each new aromatic anhydride monomer, it is necessary to confirm that the added monomer has reacted completely;
[0037] S3. Preparation of modified polyimide precursor mother solution: Add the filler to the aprotic polar aprotic polar solvent in proportion, and after uniform dispersion, add the rigid diamine monomer, the flexible diamine monomer and the main chain ester-containing diamine monomer, and stir until the diamine monomer is completely dissolved;
[0038] S4. Synthesis of modified polyimide precursor: Under nitrogen protection, the dried aromatic anhydride monomers are sequentially added to the mother liquor prepared in S3 and stirred, and before each addition of new aromatic anhydride monomers, it is necessary to confirm that the added monomers have reacted completely;
[0039] S5. Preparation of mixed glue solution: Under nitrogen protection, the polyimide precursor synthesized in S2 and the modified polyimide precursor synthesized in S4 were added to the flask in proportion and stirred until uniformly mixed;
[0040] S6. Coating and cyclization: The mixed glue solution prepared in S5 is coated on the copper foil layer, dried at high temperature, and imidized to obtain a high modulus MPI single-sided flexible copper clad laminate.
[0041] The temperature of the high temperature drying is 150-180°C, and the imidization is carried out in an IR furnace or a non-oxidizing high temperature oven. A nitrogen atmosphere is set in the IR furnace for protection, and the front section, middle section, and rear section are a baking section, a cyclization section, and a cooling section in sequence. The temperature of the cyclization section is 330-380°C, and the processing line speed of the IR furnace is 0.5-4 m / min.
[0042] Example
[0043] Example 1
[0044] like Figure 1 As shown, this embodiment is a high modulus MPI flexible copper clad laminate, comprising a copper foil layer 1 and an MPI layer 2 coated on the copper foil layer 1; the MPI layer 2 is made by mixing a modified polyimide precursor and a polyimide precursor at a weight ratio of 1.5:1;
[0045] The polyimide precursor includes a filler, an aprotic polar solvent, a rigid diamine monomer, a flexible diamine monomer and an aromatic anhydride monomer;
[0046] The molar ratio of the sum of the moles of the rigid diamine monomer and the flexible diamine monomer to the aromatic anhydride monomer is 1:0.99; and the molar ratio of the rigid diamine monomer to the flexible diamine monomer is 4:1.
[0047] The modified polyimide precursor includes a filler, a non-protonic polar solvent, a rigid diamine monomer, a flexible diamine monomer, a diamine monomer containing an ester group in the main chain, and an aromatic anhydride monomer;
[0048] Among them, the molar ratio of the sum of the moles of the rigid diamine monomer, the flexible diamine monomer, and the diamine monomer containing an ester group in the main chain to the aromatic anhydride monomer is 1:0.99; and the molar ratio of the rigid diamine monomer, the flexible diamine monomer, and the diamine monomer containing an ester group in the main chain is 2:1:2.
[0049] The mass percentage of the non-protonic polar solvent in the polyimide precursor or the modified polyimide precursor is 84-85%.
[0050] The thickness of the MPI layer in the copper clad laminate is 12 μm.
[0051] The method for preparing the above-mentioned high modulus MPI flexible copper clad laminate comprises the following steps:
[0052] S1. Prepare polyimide precursor mother liquor: add 0.5wt% modified white graphene BNS01 into 85% non-protonic polar solvent N,N-dimethylformamide (NMP), disperse evenly, add 4,4'-diaminodiphenyl ether (ODA) and p-phenylenediamine (PPDA), stir for 1 to 3 hours until the monomers are completely dissolved, wherein the molar ratio of p-phenylenediamine (PPDA) to 4,4'-diaminodiphenyl ether (ODA) is 4:1;
[0053] S2. Synthesis of polyimide precursor: under nitrogen protection, add dried pyromellitic anhydride (PMDA) and 4,4'-biphenyltetracarboxylic dianhydride (BPDA) to the mother liquor in sequence and stir (before adding each new anhydride monomer, it is necessary to confirm that the added anhydride monomer has reacted completely), the obtained modified polyimide precursor has a solid content of 15-16% and a viscosity of 30000-50000 cps, wherein the molar ratio of pyromellitic anhydride (PMDA) to 4,4'-biphenyltetracarboxylic dianhydride (BPDA) is 1:4;
[0054] S3. Prepare a modified polyimide precursor mother liquor: add 0.5wt% of modified white graphene BNS01 to the non-protonic polar solvent NMP, and after uniform dispersion, add 4,4'-diaminodiphenyl ether (ODA), p-phenylenediamine (PPDA), and bis(4-aminophenyl) terephthalate (BAPT), and stir for 1 to 3 hours until the monomers are completely dissolved, wherein the molar ratio of p-phenylenediamine (PPDA), 4,4'-diaminodiphenyl ether (ODA), and bis(4-aminophenyl) terephthalate (BAPT) is 2:1:2;
[0055] S4. Synthesis of modified polyimide precursor: Under nitrogen protection, the dried p-phenylene-bis(triphenyl)amine dianhydride (TAHQ) and 4,4'-biphenyltetracarboxylic acid dianhydride (BPDA) are sequentially added to the mother liquor and stirred (before adding each new anhydride monomer, it is necessary to confirm that the added anhydride monomer has reacted completely). The obtained modified polyimide precursor has a solid content of 15-16% and a viscosity of 30000-50000 cps, wherein the molar ratio of p-phenylene-bis(triphenyl)amine dianhydride (TAHQ) to 4,4'-biphenyltetracarboxylic acid dianhydride (BPDA) is 2:3;
[0056] S5. Preparation of mixed glue solution: Under nitrogen protection, the modified polyimide precursor synthesized in S4 and the polyimide precursor synthesized in S2 were added to the flask in a ratio of 1.5:1 and stirred for 16 to 20 hours until the mixture was completely mixed;
[0057] S6. Coating and cyclization: The mixed glue solution prepared in S5 is coated on the copper foil layer and baked at 160°C for 5 minutes, and then imidized in an online automatic continuous cyclization machine (IR furnace) to obtain a high modulus MPI single-sided flexible copper clad laminate. Among them, a nitrogen atmosphere protection is set in the IR furnace, and the front section-middle section-back section are baking section, cyclization section, and cooling section in sequence. The temperature of the cyclization section is 360°C, and the processing line speed of the IR furnace is 2m / min.
[0058] Example 2
[0059] The difference between Example 2 and Example 1 is that:
[0060] In steps S1 and S3, the filler is 0.2wt% of modified white graphene BNS01, 3wt% of talc powder, and 2wt% of LCP powder. In step S5, the weight ratio of the modified polyimide precursor to the polyimide precursor is 4:1;
[0061] The other compositions and preparation methods are the same as those in Example 1.
[0062] Example 3
[0063] The difference between Example 3 and Example 1 is that:
[0064] In step S3, a modified polyimide precursor mother liquor is prepared: 0.5wt% of modified white graphene BNS01 is added to 84% of aprotic polar solvent N,N dimethylformamide (DMF), and after uniform dispersion, 4,4'-diaminodiphenyl ether (ODA), p-phenylenediamine (PPDA), and [4-(4-aminobenzoyl)oxyphenyl] 4-aminobenzoate (ABHQ) are added, and stirred for 1 to 3 hours until the monomers are completely dissolved. The molar ratio of p-phenylenediamine (PPDA), 4,4'-diaminodiphenyl ether (ODA), and [4-(4-aminobenzoyl)oxyphenyl] 4-aminobenzoate (ABHQ) is 2.5:1:2;
[0065] The thickness of the MPI layer in the copper clad laminate is 25 um; other compositions and preparation methods are the same as those in Example 1.
[0066] Example 4
[0067] The difference between Example 4 and Example 1 is that:
[0068] In step S3, a modified polyimide precursor mother liquor is prepared: 0.5wt% of modified white graphene BNS01 is added to 85% of aprotic polar solvent N,N-dimethylacetamide (DMAC), and after uniform dispersion, 4,4'-diaminodiphenyl ether (ODA), p-phenylenediamine (PPDA), bis(4-aminophenyl) terephthalate (BAPT), and [4-(4-aminobenzoyl)oxyphenyl]4-aminobenzoate (ABHQ) are added, and stirred for 1 to 3 hours until the monomers are completely dissolved; wherein the molar ratio of p-phenylenediamine (PPDA), 4,4'-diaminodiphenyl ether (ODA), bis(4-aminophenyl) terephthalate (BAPT), and [4-(4-aminobenzoyl)oxyphenyl]4-aminobenzoate (ABHQ) is 1.5:0.5:0.5:2.
[0069] In step S5, the weight ratio of the modified polyimide precursor to the polyimide precursor is 1:1; other compositions and preparation methods are the same as those in Example 1.
[0070] Comparative Example
[0071] Comparative Example 1
[0072] The difference between Comparative Example 1 and Example 1 is that in steps S1 and S3, no filler is added to the aprotic polar solvent NMP, and the rest of the composition and preparation method are the same as those of Example 1.
[0073] Comparative Example 2
[0074] The difference between Comparative Example 2 and Example 1 is that steps S1, S2 and S5 are deleted, and the rest of the composition and preparation method are the same as those of Example 1.
[0075] Comparative Example 3
[0076] The difference between Comparative Example 3 and Example 1 is that steps S3, S4 and S5 are deleted, and the rest of the composition and preparation method are the same as those of Example 1.
[0077] Comparative Example 4
[0078] The difference between Comparative Example 4 and Example 1 is that the MPI layer in Comparative Example 4 is prepared by mixing a modified polyimide precursor and a polyimide precursor in a weight ratio of 4.5:1.
[0079] Comparative Example 5
[0080] The difference between Comparative Example 5 and Example 1 is that in Comparative Example 5, the mass fraction of the modified white graphene BNS01 of the MPI layer-modified polyimide precursor and the mass fraction of the modified white graphene BNS01 of the polyimide precursor are changed to 7 wt %.
[0081] Performance Testing
[0082] The performance tests were performed on the flexible copper clad laminates of Examples 1-4 and Comparative Examples 1-5.
[0083] Test method:
[0084] The performance tests such as peel strength, dielectric constant (Dk), dielectric loss (Df), tensile strength, elongation, water absorption and dimensional stability are carried out according to the test methods specified in IPC-TM-650, JIS C6471 and SPDR.
[0085] The test results are shown in Table 1.
[0086] Table 1 Performance results of flexible copper clad laminate
[0087]
[0088]
[0089] According to Table 1, it can be seen that the various properties of the flexible copper-clad laminates prepared in Examples 1-4 are excellent, not only having a small dielectric constant, but also having a good Young's modulus and a large tensile strength. In Comparative Example 1, no filler is added to the non-protonic polar solvent NMP. Compared with Example 1, although the peel strength of the flexible copper-clad laminate prepared therefrom has not changed, the Young's modulus has been significantly reduced; in Comparative Example 2, due to the lack of modified polyimide precursor and polyimide precursor blending, although the dielectric loss has not decreased, the flexible copper-clad laminate prepared therefrom has not only a poor Young's modulus, but also a large dielectric constant and a small tensile strength compared with Example 1, which cannot meet the needs of actual use; in Comparative Example 3, there is a lack of polyimide precursor and polyimide precursor blending, although the tensile strength and modulus are improved. The dielectric constant and dielectric loss increased significantly; in comparison column 4, the MPI layer was prepared by mixing the modified polyimide precursor and the polyimide precursor at a weight ratio of 4.5:1, which increased the mass fraction of the modified polyimide precursor in the mixed glue, the dielectric constant and dielectric loss decreased, and the tensile strength and modulus decreased. Although the dielectric properties were improved, the mechanical properties decreased; in comparison column 5, the mass fraction of the modified white graphene BNS01 of the modified polyimide precursor and the polyimide precursor was 7wt%, the modulus was greatly improved, and the tensile strength and peel strength were small. The MPI flexible copper-clad laminate prepared in the embodiment of the present invention has a higher Young's modulus and a lower dielectric constant, while also ensuring the mechanical properties of the copper-clad laminate, and has good application prospects.
Claims
1. A high modulus MPI flexible copper clad laminate, Features The invention comprises a copper foil layer (1) and an MPI layer (2) coated on the copper foil layer (1); the MPI layer (2) is prepared by mixing a modified polyimide precursor and a polyimide precursor in a weight ratio of (1 to 4):1; the polyimide precursor comprises a filler, an aprotic polar solvent, a rigid diamine monomer, a flexible diamine monomer and an aromatic anhydride monomer; the modified polyimide precursor comprises a filler, an aprotic polar solvent, a rigid diamine monomer, a flexible diamine monomer, a diamine monomer containing an ester group in the main chain and an aromatic anhydride monomer; the molar ratio of the rigid diamine monomer, the flexible diamine monomer and the aromatic anhydride monomer in the polyimide precursor is 1:(0.96 to 1.05); the molar ratio of the sum of the molar numbers of the rigid diamine monomer, the flexible diamine monomer and the diamine monomer containing an ester group in the main chain to the aromatic anhydride monomer in the modified polyimide precursor is 1:(0.96 to 1.05).
2. The high modulus MPI flexible copper clad laminate according to claim 1, Features The molar ratio of the rigid diamine monomer to the flexible diamine monomer in the polyimide precursor is (3.5-4.5):1; the molar ratio of the rigid diamine monomer, the flexible diamine monomer and the diamine monomer containing an ester group in the main chain in the modified polyimide precursor is (1.5-2.5):1:
2.
3. The high modulus MPI flexible copper clad laminate according to claim 1, Features The thickness of the MPI layer (2) is 12 to 25 um.
4. The high modulus MPI flexible copper clad laminate according to claim 1, Features The rigid diamine monomer is one or more of p-phenylenediamine, m-phenylenediamine, 2,2'-bis(trifluoromethyl)diaminobiphenyl, and 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl; The flexible diamine monomer is one or more of 4,4'-diaminodiphenyl ether, bis(4-aminophenyl) terephthalate, p-aminophenyl para-aminobenzoate, 1,3'-bis(4'-aminophenoxy)benzene, and 2,2'-bis[4-(4-aminophenoxyphenyl)propane]; The ester-containing diamine monomer is one or more of [4-(4-aminobenzoyl)oxyphenyl]4-aminobenzoate, bis(4-aminophenyl)terephthalate, and p-aminophenyl para-aminobenzoate.
5. The high modulus MPI flexible copper clad laminate according to claim 1, Features The aromatic anhydride monomer is selected from one or more of p-phenylene-diphthalic acid dianhydride, 4,4-oxydiphthalic anhydride, bisphenol A type diether dianhydride, 4,4'-biphenyltetracarboxylic acid dianhydride, pyromellitic acid anhydride, 4,4'-biphenyltetracarboxylic acid dianhydride, and 3,3',4,4'-dibenzophenonetetracarboxylic acid dianhydride.
6. The high modulus MPI flexible copper clad laminate according to claim 1, Features The filler is one or more of silicon dioxide, LCP powder, modified white graphene, and talcum powder, and the mass fraction of the filler is 0-6% of the polyimide precursor or the modified polyimide precursor.
7. The high modulus MPI flexible copper clad laminate according to claim 1, Features The non-protonic polar solvent is one or more of N,N dimethylformamide, N,N dimethylacetamide and N methylpyrrolidone, and the mass percentage of the non-protonic polar solvent in the polyimide precursor or the modified polyimide precursor is 80% to 90%.
8. A method for preparing the high modulus MPI flexible copper clad laminate according to any one of claims 1 to 7, Features The following steps are involved: S1. Prepare a polyimide precursor mother solution: add the filler to the aprotic polar solvent in proportion, disperse it evenly, add the rigid diamine monomer and the flexible diamine monomer, and stir until the diamine monomer is completely dissolved; S2. Synthesis of polyimide precursor: under nitrogen protection, the dried aromatic anhydride monomers are sequentially added to the mother liquor prepared in S1 and stirred. Before adding each new aromatic anhydride monomer, it is necessary to confirm that the added monomer has reacted completely; S3. Preparation of modified polyimide precursor mother solution: Add the filler in a non-protonic polar solvent in proportion, disperse evenly, add rigid diamine monomer, flexible diamine monomer and main chain ester-containing diamine monomer, and stir until the diamine monomer is completely dissolved; S4. Synthesis of modified polyimide precursor: Under nitrogen protection, the dried aromatic anhydride monomers are sequentially added to the mother liquor prepared in S3 and stirred, and before each addition of new aromatic anhydride monomers, it is necessary to confirm that the added monomers have reacted completely; S5. Preparation of mixed glue solution: Under nitrogen protection, the polyimide precursor synthesized in S2 and the modified polyimide precursor synthesized in S4 were added to the flask in proportion and stirred until uniformly mixed; S6. Coating and cyclization: The mixed glue solution prepared in S5 is coated on the copper foil layer, dried at high temperature, and imidized to obtain a high modulus MPI single-sided flexible copper clad laminate.
9. The method for preparing the high modulus MPI flexible copper clad laminate according to claim 8, Features The temperature of the high-temperature drying is 150-180° C., and the imidization is carried out in an IR furnace or a non-oxidizing high-temperature oven.
10. The method for preparing the high modulus MPI flexible copper clad laminate according to claim 9, Features The IR furnace is provided with nitrogen atmosphere protection, and the front section, the middle section and the rear section are respectively a baking section, a cyclization section and a cooling section, the temperature of the cyclization section is 330-380° C., and the processing line speed of the IR furnace is 0.5-4 m / min.