Glass for optical filter and optical filter
By adding Cu and Mo to the phosphate glass, the composition and structure are optimized, and the problem of the reduced visible light transmittance when the phosphate glass melts at high temperature is solved, and the efficient color correction filter effect is achieved in applications such as digital cameras.
Patent Information
- Application Number
- CN202380034229.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-19
AI Technical Summary
The high temperature of existing phosphate glasses during melting leads to a decrease in the light transmittance in the visible light area, and when the temperature is reduced, unmelted foreign matter may be generated, affecting the light transmittance.
Using phosphate glass containing Cu and Mo, by optimizing the component ratio, the transmittance of light in visible light is maintained high and the transmittance of light in near infrared region is suppressed. The specific components include P2O5, CuO, MoO3, Al2O3, etc., and do not contain F. Optimize the thickness and thermal expansion coefficient of the glass.
The effect of low suppression of near-infrared light transmittance while maintaining high light transmittance in visible light is achieved. It is suitable for color correction filters for solid-state imaging elements such as digital cameras, and improves the stability and weather resistance of glass.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to a filter glass and a filter which are used in a color correction filter of a solid-state imaging element such as a digital camera or a color video camera and which have excellent transmittance of light in the visible light region and absorption of light in the near infrared region. Background Art
[0002] Solid-state imaging elements such as CCD and CMOS used in digital cameras have spectral sensitivity from the visible light region to the near-infrared region near 1200nm. Therefore, solid-state imaging elements cannot directly obtain good color reproducibility, so near-infrared cutoff filter glass added with a specific substance that absorbs infrared rays is used to correct the visual sensitivity of solid-state imaging elements. As this near-infrared cutoff filter glass, in order to selectively absorb light with a wavelength in the near-infrared region, optical glass in which Cu (copper) is added to phosphate glass has been developed and used. Regarding these glasses, the composition is disclosed in Patent Document 1.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2010-008908 Summary of the invention
[0006] Problems to be solved by the invention
[0007] Phosphate glass has a tendency to have a lower transmittance to light in the visible light region (especially blue light) when the temperature of melting the glass raw material is as high as 1000°C or more. The reason is believed to be as follows. It is known that in phosphate glass containing Cu, the Cu component in the glass is Cu that absorbs light with wavelengths in the near infrared region. 2+ (Divalent) and Cu which has absorption characteristics for light with wavelengths around 300nm to 600nm + When the temperature of melting glass raw materials is high, part of the Cu component in the glass is in the form of Cu + The form of residue (Cu 2+ ), thereby reducing the transmittance of light in the visible light region (especially blue light). In addition, when the temperature when melting glass raw materials is lowered, there is a problem that unmelted foreign matter is generated in the glass, and the transmittance of light in the visible light region is significantly reduced.
[0008] The present invention has been made based on such a background, and an object of the present invention is to provide a filter glass and a filter capable of keeping the transmittance of light in the visible light region (particularly blue light) high while suppressing the transmittance of light in the near infrared region to be low.
[0009] Means used to solve problems
[0010] The present inventors have repeatedly conducted intensive studies and have found that, as a result, it is possible to obtain a filter glass and a filter that can maintain a high transmittance of light in the visible light region and suppress a low transmittance of light in the near-infrared region compared to conventional filters by using phosphate glass containing Cu and Mo (molybdenum).
[0011] That is, the optical filter glass of the present invention contains P (phosphorus), Cu, and Mo as components, and contains substantially no F (fluorine).
[0012] In a preferred embodiment of the optical filter glass of the present invention, the optical filter glass further contains 0.01% to 10% of MoO 3 in terms of mass % based on oxides.
[0013] In a preferred embodiment of the glass for optical filter of the present invention, the glass for optical filter further contains 40% or more of P2O5 in terms of mass % based on oxides.
[0014] In a preferred embodiment of the glass for optical filter of the present invention, the glass for optical filter further contains 5% or more of Al 2 O 3 in terms of mass % based on oxides.
[0015] Moreover, in a preferred embodiment of the optical filter glass of the present invention, the optical filter glass further contains more than 2.0% of CuO in terms of mass % based on oxides.
[0016] In a preferred embodiment of the optical filter glass of the present invention, the optical filter glass further contains, in terms of mass % based on oxides:
[0017] P2O5: 40%~80%,
[0018] Al2O3: 5%~20%,
[0019] ∑R2O: 0.5% to 20% (R2O is one or more components selected from Li2O, Na2O, K2O, Rb2O and Cs2O, ∑R2O is the total amount of R2O),
[0020] ∑R'O: 0% to 15% (R'O is one or more components selected from CaO, MgO, BaO, SrO and ZnO, ∑R'O is the total amount of R'O),
[0021] CuO: 2.0% to 20% (excluding 2.0%),
[0022] MoO3: 0.01%~10%.
[0023] In a preferred embodiment of the optical filter glass of the present invention, the optical filter glass has an average transmittance of 88.5% or more for light with a wavelength of 450 nm to 500 nm and an average transmittance of 1.5% or less for light with a wavelength of 850 nm to 900 nm, calculated as a thickness of 0.3 mm.
[0024] In addition, in a preferred embodiment of the glass for filter of the present invention, the above-mentioned glass for filter further has an average transmittance ratio A / B of 1.140 to 2.000 when the average transmittance of light with a wavelength of 450nm to 500nm is set to A and the average transmittance of light with a wavelength of 350nm to 400nm is set to B.
[0025] Furthermore, the optical filter of the present invention includes the above-mentioned optical filter glass.
[0026] Effects of the Invention
[0027] According to the present invention, it is possible to provide an optical filter glass and an optical filter capable of keeping the transmittance of light in the visible light region (particularly blue light) high while suppressing the transmittance of light in the near infrared region to be low. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a graph showing the transmittance of light having a wavelength of 300 nm to 1200 nm in Example 7 (Example) and Example 1 (Comparative Example).
[0029] Figure 2 This is a graph showing the transmittance of light with a wavelength of 350 nm to 600 nm in Example 7 (Example) and Example 1 (Comparative Example). DETAILED DESCRIPTION
[0030] Hereinafter, the mode for implementing the present invention will be described in detail. It should be noted that the present invention is not limited to the embodiment described below.
[0031] In addition, in the present specification, "α to β" indicating a range means "not less than α and not more than β".
[0032] The following describes the components that can constitute the glass of this embodiment and their suitable contents. In this application specification, unless otherwise specified, the content of each component and the total content are expressed in mass % based on oxides. In addition, the transmittance of the glass of this embodiment includes the reflective properties of the glass surface (that is, it is not the internal transmittance of the glass, but the external transmittance of the glass).
[0033] P2O5 is the main component of glass and is an essential component for improving near-infrared cutoff. If the content of P2O5 is 40% or more, its effect can be fully obtained. If the content of P2O5 is 80% or less, it is not easy to cause problems such as glass becoming unstable and reduced weather resistance. Therefore, the content of P2O5 is preferably 50% to 80%, more preferably 52% to 78%, further preferably 54% to 77%, further preferably 56% to 76%, and most preferably 60% to 75%.
[0034] Al2O3 is a main component for forming glass and is a component for improving the strength of glass. If the content of Al2O3 is 5% or more, its effect can be fully obtained. If the content of Al2O3 is 20% or less, it is not easy to cause problems such as glass becoming unstable and near-infrared cutoff properties being reduced. Therefore, the content of Al2O3 is preferably 5% to 20%, more preferably 6% to 18%, further preferably 7% to 17%, further preferably 8% to 17%, and most preferably 9% to 16.5%.
[0035] R2O (wherein R2O is one or more components selected from Li2O, Na2O, K2O, Rb2O, and Cs2O) is a component used to lower the melting temperature of glass, lower the liquidus temperature of glass, stabilize glass, etc. If the total amount of R2O (ΣR2O) is 0.5% or more, its effect can be fully obtained, and if the total amount of R2O (ΣR2O) is 20% or less, the glass is less likely to become unstable, so it is preferred. Therefore, the total amount of R2O (ΣR2O) is preferably 0.5% to 20%, more preferably 1% to 20%, further preferably 2% to 20%, further preferably 3% to 20%, and most preferably 4% to 20%.
[0036] Li2O is a component used to lower the melting temperature of glass, lower the liquidus temperature of glass, stabilize glass, etc. The content of Li2O is preferably 0% to 15%. If the content of Li2O is 15% or less, it is less likely to cause problems such as glass becoming unstable and near-infrared cutoff properties being reduced, so it is preferred. The content of Li2O is more preferably 0% to 8%, further preferably 0% to 7%, further preferably 0% to 6%, and most preferably 0% to 5%.
[0037] Na2O is a component used to lower the melting temperature of glass, lower the liquidus temperature of glass, stabilize glass, etc. The content of Na2O is preferably 0% to 15%. If the content of Na2O is 15% or less, the glass is less likely to become unstable, so it is preferred. The content of Na2O is more preferably 0.5% to 14%, further preferably 1% to 13%, and further preferably 2% to 13%.
[0038] K2O is a component that has the effect of lowering the melting temperature of glass and the liquidus temperature of glass. The content of K2O is preferably 0% to 15%. If the content of K2O is 15% or less, the glass is less likely to become unstable, so it is preferred. The content of K2O is more preferably 0.5% to 14%, further preferably 1% to 13%, and further preferably 2% to 13%.
[0039] Rb2O is a component that has the effect of lowering the melting temperature of glass and the liquidus temperature of glass. The content of Rb2O is preferably 0% to 15%. If the content of Rb2O is 15% or less, the glass is less likely to become unstable, so it is preferred. The content of Rb2O is more preferably 0.5% to 14%, further preferably 1% to 13%, and further preferably 2% to 13%.
[0040] Cs2O is a component that has the effect of lowering the melting temperature of glass and the liquidus temperature of glass. The content of Cs2O is preferably 0% to 15%. If the content of Cs2O is 15% or less, the glass is less likely to become unstable, so it is preferred. The content of Cs2O is more preferably 0.5% to 14%, further preferably 1% to 13%, and further preferably 2% to 13%.
[0041] In addition, the alkali metal component represented by R2O generates a mixed alkali effect in the glass by adding two or more components at the same time. + The mobility of ions is reduced. Therefore, when glass comes into contact with water, the H + Ions and R in Glass + The hydration reaction caused by the ion exchange of ions improves the weather resistance of the glass. Therefore, the glass of this embodiment preferably contains two or more components selected from Li2O, Na2O, K2O, Rb2O and Cs2O. In this case, the total amount (∑R2O) of R2O (wherein R2O is Li2O, Na2O, K2O, Rb2O and Cs2O) is preferably 7% to 18% (wherein 7% is not included). If the total amount of R2O is greater than 7%, its effect can be fully obtained. If the total amount of R2O is less than 18%, it is not easy to cause problems such as the glass becoming unstable, the near-infrared cutoff property being reduced, and the strength of the glass being reduced, so it is preferred. Therefore, ΣR2O is preferably greater than 7% and less than or equal to 18%, more preferably 7.5% to 17%, further preferably 8% to 16%, further preferably 8.5% to 15%, and most preferably 9% to 14%.
[0042] R'O (wherein R'O is one or more components selected from CaO, MgO, BaO, SrO and ZnO) is a component used to lower the melting temperature of glass, lower the liquidus temperature of glass, stabilize glass, increase the strength of glass, etc. The total amount of R'O (ΣR'O) is preferably 0% to 15%. If the total amount of R'O is 15% or less, it is less likely to cause problems such as glass becoming unstable, near-infrared cutoff properties being reduced, and glass strength being reduced, so it is preferred. The total amount of R'O (ΣR'O) is more preferably 0% to 13%, and more preferably 0% to 11%. It is further preferably 0% to 9%, and further preferably 0% to 8%.
[0043] CaO is a component used to lower the melting temperature of glass, lower the liquidus temperature of glass, stabilize glass, and increase the strength of glass. As the content of CaO, it is preferably 0% to 10%. If the content of CaO is less than 10%, it is not easy to cause problems such as glass becoming unstable and near-infrared cutoff properties being reduced, so it is preferred. The content of CaO is more preferably 0% to 8%, further preferably 0% to 6%, further preferably 0% to 5%, and most preferably 0% to 4%.
[0044] MgO is a component used to lower the melting temperature of glass, lower the liquidus temperature of glass, stabilize glass, and increase the strength of glass. The content of MgO is preferably 0% to 15%. If the content of MgO is 15% or less, it is less likely to cause problems such as glass becoming unstable and near-infrared cutoff properties being reduced, so it is preferred. The content of MgO is more preferably 0% to 13%, further preferably 0% to 10%, further preferably 0% to 9%, and most preferably 0% to 8%.
[0045] BaO is a component used to lower the melting temperature of glass, lower the liquidus temperature of glass, stabilize glass, etc. The content of BaO is preferably 0.1% to 10%. If the content of BaO is 10% or less, it is not easy to cause problems such as glass becoming unstable and near-infrared cutoff properties being reduced, so it is preferred. The content of BaO is more preferably 0% to 8%, further preferably 0% to 6%, further preferably 0% to 5%, and most preferably 0% to 4%.
[0046] SrO is a component used to lower the melting temperature of glass, lower the liquidus temperature of glass, stabilize glass, etc. The content of SrO is preferably 0% to 10%. If the content of SrO is 10% or less, it is less likely to cause problems such as glass becoming unstable and near-infrared cutoff properties being reduced, so it is preferred. The content of SrO is more preferably 0% to 8%, further preferably 0% to 7%, and most preferably 0% to 6%.
[0047] ZnO has the effect of lowering the melting temperature of glass and the liquidus temperature of glass. The content of ZnO is preferably 0% to 15%. If the content of ZnO is 15% or less, it is not easy to produce problems such as poor solubility of glass and reduced near-infrared cutoff, so it is preferred. The content of ZnO is more preferably 0% to 13%, further preferably 0% to 10%, further preferably 0% to 9%, and most preferably 0% to 8%.
[0048] In the glass of this embodiment, it is preferred that divalent cations of elements other than Cu are substantially not contained. The reason for this is as follows. It should be noted that as an element other than Cu, the above-mentioned R' can be cited. Therefore, ΣR'O is preferably 0%.
[0049] When the glass of this embodiment contains CuO, 2+ The light absorption of the ions blocks the light in the near infrared region. 2- The electric field of the ions splits the Cu 2+ It is produced by the electron transition between the d orbitals of the ions. 2+ O around the ions 2- When the symmetry of the ion is reduced, the splitting of the d orbitals is promoted. 2- When there are cations around the ion, O 2- The ions are attracted by the electric field of the cations, O 2- The symmetry of the ions is reduced. As a result, the splitting of the d orbital is promoted, and light absorption caused by the electron transition between the split d orbitals occurs, so the light absorption capacity in the near-infrared region (wavelength: greater than or equal to 750nm and less than 1000nm) is weakened, and the light absorption capacity in the short-wavelength infrared region (wavelength: greater than or equal to 1000nm and less than 2500nm) is enhanced. When the valence of the ion is large, the intensity of the electric field of the cation becomes stronger, so especially when an oxide containing a divalent cation of an element other than Cu is added to the glass, there is a possibility that the near-infrared cutoff property is reduced and the transmittance of the short-wavelength infrared is reduced.
[0050] MoO3 is an essential component for improving the transmittance of light in the visible light region of glass. The inventors prepared a phosphate glass containing Cu (which does not contain a fluorine component) and a phosphate glass containing only Mo added to the glass, and confirmed their optical properties. As a result, the following phenomenon was confirmed: the transmittance of light with a wavelength of 400nm to 540nm in the latter glass was greatly increased compared to the former glass. This phenomenon is believed to be attributed to the following reasons, but the following reasons are hypothetical.
[0051] It is known that Mo exists in glass as Mo 6+ However, when Mo and Cu are added to phosphoric acid glass at the same time, the Cu+ Releases electrons and becomes Cu 2+ (Cu + →Cu 2+ +e - ), Mo 6+ Accept Cu + The released electrons become Mo 5+ (Mo 6+ +e - →Mo 5+ ). Therefore, Cu, which has absorption characteristics near the wavelength of 300nm to 600nm, + The existence ratio of (monovalent) decreases, and the transmittance of light with a wavelength of 400nm to 540nm increases. It is believed that Mo ions have the characteristic of absorbing light with a wavelength of about 400nm, so the transmittance of light with a wavelength of about 400nm does not increase. In the past, phosphate glass containing Cu and Mo was not known, and the above content is considered to be a new insight discovered by the inventors of the present application.
[0052] If the content of MoO3 is 0.01% or more, the effect of improving the transmittance of light in the visible light region of the glass can be fully obtained. In addition, if the content of MoO3 is 10% or less, it is not easy to produce problems such as reduced near-infrared cutoff and loss of transparency in the glass, so it is preferred. The content of MoO3 is more preferably 0.02% to 9%, further preferably 0.03% to 8%, further preferably 0.04% to 7%, and most preferably 0.05% to 6%.
[0053] CuO is an essential component for cutting off near infrared rays. If the content of CuO is greater than 2.0%, its effect and the effect of increasing the transmittance of light in the visible light region of the glass obtained when added simultaneously with MoO3 can be fully obtained. In addition, if the content of CuO is less than 20%, it is not easy to produce problems such as devitrified foreign matter in the glass and reduced transmittance of light in the visible light region, so it is preferred. The content of CuO is more preferably 4% to 19.5%, further preferably 5% to 19%, further preferably 6% to 18.5%, and most preferably 7% to 18% (excluding 7%).
[0054] In the glass of this embodiment, F is a component effective for improving weather resistance, but since it is an environmental load substance and there is a possibility that near-infrared cutoff properties may be reduced, F is not substantially contained.
[0055] In the present invention, substantially not containing a specific component means that the specific component is not intentionally added, and does not exclude the inclusion of a specific component to the extent that the specific component is inevitably mixed from raw materials etc. but does not affect the desired properties.
[0056] In order to stabilize the glass, B2O3 may be contained within a range of 10% or less. If the content of B2O3 is 10% or less, it is not easy to cause problems such as poor weather resistance of the glass and reduced near-infrared cutoff properties, so it is preferred. The content of B2O3 is preferably 9% or less, more preferably 8% or less, further preferably 7% or less, further preferably 6% or less, and most preferably 5% or less.
[0057] In the glass of the present embodiment, in order to improve the weather resistance of the glass, SiO2, GeO2, ZrO2, SnO2, TiO2, CeO2, WO3, Y2O3, La2O3, Gd2O3, Yb2O3, Nb2O5 can be contained within a range of 5% or less. If the content of these components is 5% or less, it is not easy to produce problems such as devitrification foreign matter in the glass and reduction of near-infrared cutoff, so it is preferred. The content of these components is preferably 4% or less, more preferably 3% or less, further preferably 2% or less, and further preferably 1% or less.
[0058] Fe2O3, Cr2O3, Bi2O3, NiO, V2O5, MnO2, and CoO are components that reduce the transmittance of light in the visible light region by being present in the glass. Therefore, it is preferred that these components are not substantially contained in the glass.
[0059] The glass of this embodiment preferably has a thermal expansion coefficient of 60×10 -7 / ℃~180×10 -7 / ℃.
[0060] When the glass of this embodiment is used as a color correction filter (near infrared cut filter glass) of a solid-state imaging element, it also functions as a protective glass for airtightly sealing the solid-state imaging element, and therefore is sometimes directly bonded to a packaging material. In this case, if the difference in thermal expansion coefficients between the near infrared cut filter glass and the packaging material is large, there is a possibility that peeling or breakage may occur at the bonded portion, and the airtight state cannot be maintained.
[0061] Usually, as a packaging material, glass, crystallized glass, ceramic, alumina and other materials are used in consideration of heat resistance, and it is preferable to reduce the difference in thermal expansion coefficient between these packaging materials and the near-infrared cutoff filter glass. Therefore, for the glass of this embodiment, it is preferable to adjust the thermal expansion coefficient in the temperature range of 30°C to 300°C to the above range. In the case where the thermal expansion coefficient of the glass of this embodiment is outside the above range, the difference with the thermal expansion coefficient of the packaging material is large, and it is possible that the airtight state cannot be maintained due to peeling or breakage. The more preferred range of the thermal expansion coefficient is 65×10 -7 / ℃~175×10 -7 / ℃, and the further preferred range is 70×10-7 / ℃~170×10 -7 / ℃.
[0062] For the glass of this embodiment, the average transmittance at a wavelength of 450nm to 500nm, measured when light is incident from the normal direction toward the main surface and converted to a thickness of 0.3mm, is 88.5% or more, and the average transmittance at a wavelength of 850nm to 900nm is 1.5% or less. The glass of this embodiment has such optical properties, and can be obtained as a glass suitable for a filter that can maintain a high transmittance of light in the visible light region while suppressing a low transmittance of light in the near infrared region.
[0063] The average transmittance of the glass of this embodiment for light of wavelength 450 nm to 500 nm converted at a thickness of 0.3 mm is preferably 88.6% or more, more preferably 88.7% or more, further preferably 88.8% or more, further preferably 88.9% or more, and most preferably 89% or more.
[0064] The average transmittance of the glass of this embodiment at a wavelength of 850 nm to 900 nm converted to a thickness of 0.3 mm is preferably 1.4% or less, more preferably 1.3% or less, further preferably 1.1% or less, further preferably 0.9% or less, and most preferably 0.7% or less.
[0065] For the glass of this embodiment, when the average transmittance of light with a wavelength of 450nm to 500nm converted by a thickness of 0.3mm is set to A, and the average transmittance of light with a wavelength of 350nm to 400nm converted by a thickness of 0.3mm is set to B, the average transmittance ratio A / B is 1.140 to 2.000. The glass of this embodiment has such optical properties that it is possible to cut off ultraviolet rays while maintaining a high transmittance in the visible light region, especially blue light. When the average transmittance ratio A / B is less than 1.140, it may not be possible to fully obtain the above-mentioned effect, so it is not preferred. When the average transmittance ratio A / B is greater than 2.000, it is possible that the absorption of light in the ultraviolet region extends to the visible light region, and the transmittance of light in the visible light region decreases, so it is not preferred. The average transmittance ratio A / B of the glass of the present embodiment is preferably 1.145 to 2.000, more preferably 1.150 to 1.900, further preferably 1.160 to 1.800, further preferably 1.170 to 1.700, and most preferably 1.180 to 1.600.
[0066] When the glass of the present embodiment is used as a color correction filter of a solid-state imaging element, for example, it is usually used with a thickness of 2 mm or less. From the viewpoint of lightweight components, it is preferably 1 mm or less, more preferably 0.5 mm or less, further preferably 0.3 mm or less, and further preferably 0.2 mm or less. In addition, from the viewpoint of ensuring the strength of the glass, it is preferably 0.05 mm or more.
[0067] The glass of this embodiment can be produced as follows, for example.
[0068] First, the raw materials are weighed and mixed so as to be within the above composition range (mixing step). The raw material mixture is placed in a platinum crucible and heated and melted in an electric furnace at a temperature of 950°C to 1300°C (melting step). After being fully stirred and clarified, it is cast into a mold, cut, and ground to form a flat plate of a specified thickness (forming step).
[0069] In the melting step of the manufacturing method, the maximum temperature of the glass during the glass melting is preferably adjusted to 1300° C. or less. When the maximum temperature of the glass during the glass melting exceeds 1300° C., the transmittance characteristics deteriorate. The temperature is more preferably 1250° C. or less, further preferably 1200° C. or less, and further preferably 1150° C. or less.
[0070] If the temperature in the melting step is too low, problems such as devitrification during melting and time-consuming complete melting may occur. Therefore, the temperature is preferably 1000° C. or higher, and more preferably 1025° C. or higher.
[0071] The glass of this embodiment can be formed into a predetermined shape, and then an optical multilayer film can be provided on at least one side of the glass, thereby obtaining an optical filter having the above-mentioned optical filter glass. Examples of the optical multilayer film include: IR cut-off film (film reflecting near infrared rays), UV / IR cut-off film (film reflecting ultraviolet rays and near infrared rays), UV cut-off film (film reflecting ultraviolet rays), anti-reflection film, etc. These optical thin films can be formed by known methods such as evaporation method or sputtering method.
[0072] An adhesion enhancing film may also be provided between the glass and the optical multilayer film of the present embodiment. By providing the adhesion enhancing film, the adhesion between the glass and the optical multilayer film is improved, and film peeling can be suppressed. Examples of adhesion enhancing films include silicon oxide (SiO2), titanium oxide (TiO2), lanthanum titanate (La2Ti2O7), aluminum oxide (Al2O3), a mixture of aluminum oxide and zirconium oxide (ZrO2), magnesium fluoride (MgF2), calcium fluoride (CaF2), strontium fluoride (SrF2), fluorine-containing organosilicon, and the like. If the substance contains fluorine or oxygen, the adhesion is higher, and in particular, the adhesion of magnesium fluoride and titanium oxide to glass or film becomes higher, so it is preferably used as an adhesion enhancing film. The adhesion enhancing film may be a single layer or may be two or more layers. In the case of two or more layers, a variety of substances may be combined.
[0073] The optical filter of this embodiment includes the glass of this embodiment described above. The optical filter of this embodiment may include the following configuration in addition to the glass of this embodiment.
[0074] The optical filter of this embodiment may include an absorption layer on at least one main surface of the glass of this embodiment, wherein the absorption layer includes a near-infrared absorption material having a maximum absorption wavelength in the near-infrared region. By making such a structure, a filter can be obtained in which the transmittance of light in the near-infrared region is suppressed to a lower level.
[0075] In the optical filter of this embodiment, it is preferred that a near-infrared absorbing pigment is added to a transparent resin selected from acrylic resins, epoxy resins, ene-thiol resins, polycarbonate resins, polyether resins, polyarylate resins, polysulfone resins, polyethersulfone resins, polyparaphenylene resins, polyarylene ether phosphine oxide resins, polyimide resins, polyamide-imide resins, polyolefin resins, cyclic olefin resins and polyester resins, and is contained in the absorbing layer.
[0076] In addition, as the near infrared absorbing pigment, it is preferable to use a pigment containing A near infrared absorbing material of at least one kind selected from the group consisting of a pigment, a phthalocyanine pigment, a cyanine pigment and a diimmonium pigment.
[0077] Example
[0078] Hereinafter, although an Example is demonstrated, this invention is not limited to these Examples.
[0079] Examples and comparative examples of the optical filter glass of the present invention are shown in Tables 1 to 2 and 5. Examples 1, 13 and 16 are comparative examples, and Examples 2 to 12, 14, 15 and 17 are examples.
[0080] [Glass production]
[0081] For these glasses, the raw materials were weighed and mixed so as to have the composition shown in Tables 1 to 2 and 5 (mass % of oxides, all glasses substantially containing no fluorine), and the mixture was placed in a crucible with an internal volume of about 400 cc and melted in an atmospheric atmosphere for 2 hours. It should be noted that the melting temperature of the glass raw materials was 1100°C for Examples 3, 6 and 16, 1050°C for Examples 1, 2, 4, 5 and 7 to 12, 1150°C for Examples 13 to 15, and 1125°C for Example 17. Then, the glass raw materials were clarified and stirred, and cast into a rectangular mold of 100 mm in length × 80 mm in width × 20 mm in height preheated to about 300°C to about 500°C, and then slowly cooled at about 1°C / min, thereby obtaining a glass sample of a plate-shaped body of 40 mm in length × 30 mm in width × about 0.3 mm in thickness, both sides of which were optically polished.
[0082] In addition, regarding the raw materials of each glass, in the case of P2O5, any one or more of H3PO4, Al(PO3)3, NaPO3 and KPO3 is used.
[0083] In the case of Al2O3, Al(PO3)3 is used.
[0084] In the case of Li2O, any one or more of LiPO3, LiNO3 and Li2CO3 is used.
[0085] In the case of Na2O, any one or more of NaPO3, NaNO3 and Na2CO3 are used.
[0086] In the case of K2O, any one or more of KPO3, KNO3 and K2CO3 is used.
[0087] In the case of CuO, at least one of CuO and Cu(PO 3 ) 2 is used.
[0088] In the case of MoO3, at least one of MoO3 and Na2MoO4 is used.
[0089] In addition, the raw materials of glass are not limited to the above substances, and well-known raw materials can be used.
[0090] [evaluate]
[0091] For the glass sample prepared as above, the transmittance of light with a wavelength of 350nm to 1200nm was measured using a spectrophotometer (manufactured by JASCO Corporation, V-570), and converted to a value of 0.3mm in thickness. Based on the converted transmittance, the average transmittance B of light with a wavelength of 350nm to 400nm, the average transmittance A of light with a wavelength of 450nm to 500nm, and the average transmittance of light with a wavelength of 850nm to 900nm were obtained. In addition, the average transmittance ratio A / B was calculated from the above average transmittance A and average transmittance B.
[0092] The results are shown in Tables 3 to 4 and Table 6. In addition, the transmittance of light with a wavelength of 300 nm to 1200 nm in Example 1 (Comparative Example) and Example 7 (Example) is shown in Figure 1 The transmittance of light with a wavelength of 350nm to 600nm is shown in Figure 2 middle.
[0093] [Table 1]
[0094] Unit: Mass%
[0095]
[0096] [Table 2]
[0097] Unit: Mass%
[0098]
[0099] [Table 3]
[0100]
[0101] [Table 4]
[0102]
[0103] [Table 5]
[0104] Unit: Mass%
[0105]
[0106] [Table 6]
[0107]
[0108] In the embodiments of the present invention (Examples 2 to 12), by containing Mo in the glass, the average transmittance at wavelengths of 450nm to 500nm is 88.5% or more, and the average transmittance at wavelengths of 850nm to 900nm is 1.5% or less, thereby maintaining the transmittance of light in the visible light region at a high level while suppressing the transmittance of light in the near-infrared region at a low level. In particular, compared with the glass of the comparative example (Example 1) that does not contain Mo, the average transmittance of light in the visible light region (especially blue light) of the glass of the embodiments (Examples 2 to 12) containing Mo is improved. It is speculated that this is because the inclusion of Mo makes the Cu in the glass + The effect produced by reducing the presence ratio of the ingredient.
[0109] In addition, the glasses of the examples (Example 14 and Example 15) of the present invention are obtained by adding only Mo to the glass of the comparative example (Example 13) that does not contain Mo. The glass of the example (Example 17) of the present invention is obtained by adding only Mo to the glass of the comparative example (Example 16) that does not contain Mo. From the optical properties of these glasses, the average transmittance of light (especially blue light) in the visible light region of the glass of the example containing Mo is improved compared with the glass of the comparative example that does not contain Mo. It is speculated that this is because the inclusion of Mo increases the Cu in the glass. + The effect produced by reducing the presence ratio of the ingredient.
[0110] In addition, Examples 3 and 6 are examples in which the glass compositions are the same as those of Examples 2 and 5, respectively, and only the temperature at which the glass raw materials are melted is changed (increased by 50° C.). According to the results of the optical properties in Table 3, the glasses of Examples 3 and 6 can maintain a high average transmittance in the visible light region (particularly blue light) compared to the comparative example (Example 1) containing no Mo, even when the melting temperature of the glass raw materials is increased.
[0111] The embodiments of the present invention have been described above, but the present invention is not limited to the above embodiments, etc. Various changes, corrections, substitutions, additions, deletions and combinations can be made within the scope of the claims, which of course also belong to the technical scope of the present invention.
[0112] This application claims the priority based on Japanese Patent Application No. 2022-074100 filed with the Japan Patent Office on April 28, 2022, and all the contents of Japanese Patent Application No. 2022-074100 are incorporated herein by reference.
Claims
1. A glass for a filter, in, The optical filter glass contains P, Cu, and Mo as components, and contains substantially no F.
2. The optical filter glass according to claim 1, in, The filter glass contains 0.01% to 10% of MoO in terms of mass % based on oxides. 3 .
3. The optical filter glass according to claim 1, in, The filter glass contains 40% or more of P in terms of mass % based on oxides. 2 O 5 .
4. The optical filter glass according to claim 1, in, The filter glass contains 5% or more of Al in terms of mass % based on oxides. 2 O 3 .
5. The optical filter glass according to claim 1, in, The optical filter glass contains more than 2.0% of CuO in terms of mass % based on oxide.
6. The optical filter glass according to claim 1, in, The optical filter glass contains, in terms of mass % based on oxides: P 2 O 5 :40%~80%、 <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> :5%~20%、 ∑R 2 O: 0.5%~20%(R 2 O is selected from Li 2 O、Na 2 O.K 2 O、Rb 2 O and Cs 2 One or more components in O, ∑R 2 O is R 2 O), ∑R'O: 0% to 15% (R'O is one or more components selected from CaO, MgO, BaO, SrO and ZnO, ∑R'O is the total amount of R'O), CuO: 2.0% to 20% (excluding 2.0%), MoO 3 :0.01%~10%.
7. The optical filter glass according to claim 1, in, When converted to a thickness of 0.3 mm, the average transmittance of light with a wavelength of 450nm to 500nm is 88.5% or more, and the average transmittance of light with a wavelength of 850nm to 900nm is 1.5% or less.
8. The optical filter glass according to claim 1, in, When the average transmittance of light with a wavelength of 450 nm to 500 nm converted to a thickness of 0.3 mm is A and the average transmittance of light with a wavelength of 350 nm to 400 nm converted to a thickness of 0.3 mm is B, the average transmittance ratio A / B is 1.140 to 2.
000.
9. A filter, in, The optical filter comprises the optical filter glass according to any one of claims 1 to 8.
Citation Information
Patent Citations
Near infrared cut-off filter glass
CN107531557A
Phosphate optical glass, preparation method of phosphate optical glass, optical element and optical filter thereof
CN108675631A
Ultraviolet, visible and near-infrared light absorbing glass as well as preparation method and application thereof
CN110156317A
Ultraviolet-transmitting glass
CN113045199A
Aluminophosphate glass containing copper (II) oxide, and use thereof for optical filtering
JP2007290886A