Resin composition, pellets, and molded article

By reasonably preparing titanium oxide particles, polyolefin wax with low acid value and aromatic sulfonic acid metal salts in polycarbonate resin, the problem of insufficient impact resistance during retention of polycarbonate resin molded products is solved, and high light shading is achieved and impact resistance, impact strength retention rate reaches more than 72%.

CN118984857APending Publication Date: 2024-11-19MITSUBISHI ENG PLASTICS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033197.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-15
Filing Date
2023-04-10
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When existing polycarbonate resin molded products are mixed with large amounts of titanium oxide, the impact strength is poor, especially when retained, and the impact resistance is insufficient.

Method used

5.0 to 20.0 parts by mass of titanium oxide particles, 0.001 to 1.5 parts by mass of polyolefin wax having an acid value of less than 0.5 mgKOH/g, and 0.01 to 1.5 parts by mass of aromatic sulfonic acid metal salt were added to the polycarbonate resin, and the adjustment was made. The ratio and acid value can improve the dispersion of titanium oxide particles and the impact resistance of molded products.

Benefits of technology

The high impact resistance and light shielding properties of the molded product under retention conditions are achieved, and the impact intensity retention rate reaches more than 72%, ensuring the excellent performance of the molded product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005076316310000041
    Figure BDA0005076316310000041
  • Figure BDA0005076316310000051
    Figure BDA0005076316310000051
  • Figure BDA0005076316310000061
    Figure BDA0005076316310000061
Patent Text Reader

Abstract

Provided are a resin composition containing a polycarbonate resin (A) and containing 5.0-20.0 parts by mass of particles (B) mainly composed of titanium oxide, a polyolefin wax (C), and an aromatic sulfonic acid metal salt (D) per 100 parts by mass of the polycarbonate resin (A), the resin composition being characterized in that when the polyolefin wax (C) is a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, the polyolefin wax (C) is a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, the polyolefin wax (C) is a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, and the polyolefin wax (C) is a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g. The content of the polyolefin wax (C-1) is 0.001-1.5 parts by mass and the content of the aromatic sulfonic acid metal salt (D) is 0.01-1.5 parts by mass when the polyolefin wax (C) is a polyolefin wax (C-2) having an acid value of 0.5-150 mgKOH / g, the content of the polyolefin wax (C-2) is 0.001-1.5 parts by mass and the aromatic sulfonic acid alkali metal salt (D) is 0.2-1.5 parts by mass when the polyolefin wax (C) is a polyolefin wax (C-2) having an acid value of 0.5-150 mgKOH / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition, particles and molded products. Background Art

[0002] Conventionally, titanium oxide has been blended into polycarbonate resin for the purpose of improving the shielding properties and coloring of resin molded products (Patent Documents 1 and 2).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2019 / 172243

[0006] Patent Document 2: Japanese Patent Application Publication No. 2019-123809 Summary of the invention

[0007] Problems to be solved by the invention

[0008] As described above, in order to improve the light-shielding property of a molded product molded from a resin composition containing a polycarbonate resin, a large amount of titanium oxide particles is sometimes added to the resin composition. However, if a resin composition containing a large amount of titanium oxide is prepared, the impact strength of the molded product obtained from the resin composition tends to be poor. In particular, when the resin composition is molded and retained in a barrel, the impact resistance of the molded product tends to be poor.

[0009] The present invention aims to solve the above-mentioned problems and to provide a resin composition and a molded article which can achieve desired light-shielding properties and have excellent impact resistance, particularly, retention of impact resistance during retention.

[0010] Solutions to the problem

[0011] The present inventors have conducted studies based on the above problems and have found that the above problems can be solved by blending an aromatic sulfonic acid metal salt with a polycarbonate resin and titanium oxide particles.

[0012] Specifically, the above-mentioned problems are solved in the following manner.

[0013] <1> A resin composition, wherein

[0014] The resin composition comprises a polycarbonate resin (A), and 5.0 to 20.0 parts by mass of particles (B) containing titanium oxide as a main component, a polyolefin wax (C), and an aromatic sulfonic acid metal salt (D) based on 100 parts by mass of the polycarbonate resin (A).

[0015] When the polyolefin wax (C) is a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, the content of the polyolefin wax (C-1) is 0.001 to 1.5 parts by mass, and the content of the aromatic sulfonic acid metal salt (D) is 0.01 to 1.5 parts by mass,

[0016] When the polyolefin wax (C) is a polyolefin wax (C-2) having an acid value of 0.5 to 150 mgKOH / g, the content of the polyolefin wax (C-2) is 0.001 to 1.5 parts by mass, and the resin composition contains 0.2 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D).

[0017] <2> The resin composition according to <1>, wherein

[0018] The resin composition comprises 5.0 to 20.0 parts by mass of particles (B) containing titanium oxide as a main component, 0.001 to 1.5 parts by mass of a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, and 0.01 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D), based on 100 parts by mass of a polycarbonate resin (A).

[0019] <3> The resin composition according to <2>, wherein

[0020] The mass ratio (C-1) / (D) of the polyolefin wax (C-1) to the aromatic sulfonic acid alkali metal salt (D) is 0.15 to 20.

[0021] <4> The resin composition according to <1>, wherein

[0022] The resin composition comprises 5.0 to 20.0 parts by mass of particles (B) containing titanium oxide as a main component, 0.001 to 1.5 parts by mass of a polyolefin wax (C-2) having an acid value of 0.5 to 150 mgKOH / g, and 0.2 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D), based on 100 parts by mass of a polycarbonate resin (A).

[0023] <5> The resin composition according to <4>, wherein

[0024] The mass ratio (C-2) / (D) of the polyolefin wax (C-2) and the aromatic sulfonic acid alkali metal salt (D) is 0.15 to 10.0.

[0025] <6> The resin composition according to <4> or <5>, wherein

[0026] The molded product obtained by molding the above-mentioned resin composition under the conditions of a barrel setting temperature of 280°C and a cycle time of 1 minute was observed using an operating electron microscope. The equivalent circle diameter calculated using mathematical formula (1) based on the area of ​​the region where the particles (B) containing titanium oxide as the main component were dispersed was less than 0.165 μm.

[0027] <7> The resin composition according to any one of <1> to <6>, wherein

[0028] The polyolefin wax (C) has a carboxyl group and / or an anhydride group thereof.

[0029] <8> The resin composition according to any one of <1> to <7>, wherein

[0030] The fluorination rate of the aromatic sulfonic acid alkali metal salt (D) is less than 1%.

[0031] <9> The resin composition according to any one of <1> to <8>, wherein

[0032] The content of at least one filler selected from the group consisting of fibrous glass fillers, fibrous carbon fillers, and plate-shaped glass fillers is less than 1 part by mass based on 100 parts by mass of the polycarbonate resin.

[0033] <10> Pellets formed from the resin composition according to any one of <1> to <9>.

[0034] <11> A molded article formed from the resin composition according to any one of <1> to <9>.

[0035] <12> A molded article formed from the pellets according to <10>.

[0036] <2-1> A resin composition, wherein

[0037] The resin composition comprises a polycarbonate resin (A), and comprises 5.0 to 20.0 parts by mass of particles (B) having titanium oxide as a main component, 0.001 to 1.5 parts by mass of a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, and 0.01 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D), based on 100 parts by mass of the polycarbonate resin (A).

[0038] <2-2> The resin composition according to <2-1>, wherein

[0039] The notched Charpy impact strength obtained by molding a 3 mm thick test piece using the above resin composition at a cylinder setting temperature of 310°C and a residence time in the cylinder of 7 minutes and measuring it in accordance with ISO179-1 is compared with the notched Charpy impact strength obtained by measuring it by the same method as above when molding using the above resin composition at a cylinder setting temperature of 280°C and a cycle time of 1 minute. The impact strength retention rate is 72% or more.

[0040] <2-3> The resin composition according to <2-1> or <2-2>, wherein

[0041] The particles (B) containing titanium oxide as a main component contain TiO2: 90.0 to 98.0% by mass, Al2O3: 0.5 to 3.5% by mass, and SiO2: 0 to 6.0% by mass.

[0042] <2-4> The resin composition according to any one of <2-1> to <2-3>, wherein

[0043] The above-mentioned aromatic sulfonic acid alkali metal salt (D) is an aromatic sulfonic acid alkali metal salt having a fluorination rate of less than 1%.

[0044] <2-5> The resin composition according to any one of <2-1> to <2-4>, wherein

[0045] The notched Charpy impact strength obtained by molding a 3 mm thick test piece using the resin composition at a cylinder setting temperature of 310° C. and a residence time in the cylinder of 7 minutes and measuring it in accordance with ISO179-1 is compared with the notched Charpy impact strength obtained by measuring it in the same manner as above when molding using the resin composition at a cylinder setting temperature of 280° C. and a cycle time of 1 minute. The impact strength retention rate is 72% or more.

[0046] The particles (B) containing titanium oxide as a main component contain TiO2: 90.0-98.0 mass %, Al2O3: 0.5-3.5 mass %, and SiO2: 0-6.0 mass %,

[0047] The above-mentioned aromatic sulfonic acid alkali metal salt (D) is an aromatic sulfonic acid alkali metal salt having a fluorination rate of less than 1%.

[0048] <2-6> A molded article formed from the resin composition according to any one of <2-1> to <2-5>.

[0049] <2-7> Pellets formed from the resin composition according to any one of <2-1> to <2-5>.

[0050] <2-8> A molded article formed from the pellets described in <2-7>.

[0051] <3-1> A resin composition, wherein

[0052] The resin composition comprises a polycarbonate resin (A), and contains 5.0 to 20.0 parts by mass of particles (B) having titanium oxide as a main component, 0.001 to 1.5 parts by mass of a polyolefin wax (C-2) having an acid value of 0.5 to 150 mgKOH / g, and 0.2 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D) based on 100 parts by mass of the polycarbonate resin (A).

[0053] <3-2> The resin composition according to <3-1>, wherein

[0054] The polyolefin wax (C-2) has a carboxyl group and / or an anhydride group thereof.

[0055] <3-3> The resin composition according to <3-1> or <3-2>, wherein

[0056] The notched Charpy impact strength obtained by molding a 3 mm thick test piece using the above resin composition at a cylinder setting temperature of 310°C and a residence time in the cylinder of 7 minutes and measuring it in accordance with ISO179-1 is compared with the notched Charpy impact strength obtained by measuring it by the same method as above when molding using the above resin composition at a cylinder setting temperature of 280°C and a cycle time of 1 minute. The impact strength retention rate is 80% or more.

[0057] <3-4> The resin composition according to <3-1> or <3-2>, wherein

[0058] The molded product obtained by molding the above-mentioned resin composition under the conditions of a barrel setting temperature of 280°C and a cycle time of 1 minute was observed using an operating electron microscope. The equivalent circle diameter calculated using mathematical formula (1) based on the area of ​​the region where particles (B) with titanium oxide as the main component were dispersed was less than 0.165 μm.

[0059] [Mathematical formula 1]

[0060]

[0061] <3-5> The resin composition according to <3-1> or <3-2>, wherein

[0062] The notched Charpy impact strength obtained by molding a 3 mm thick test piece using the resin composition at a cylinder setting temperature of 310° C. and a residence time in the cylinder of 7 minutes and measuring it in accordance with ISO179-1 is compared with the notched Charpy impact strength obtained by measuring it in the same manner as above when molding using the resin composition at a cylinder setting temperature of 280° C. and a cycle time of 1 minute, and the impact strength retention rate is 80% or more, and

[0063] The molded product obtained by molding the above-mentioned resin composition under the conditions of a barrel setting temperature of 280°C and a cycle time of 1 minute was observed using an operating electron microscope. The equivalent circle diameter calculated using mathematical formula (1) based on the area of ​​the region where particles (B) with titanium oxide as the main component were dispersed was less than 0.165 μm.

[0064] [Mathematical formula 2]

[0065]

[0066] <3-6> The resin composition according to any one of <3-1> to <3-5>, wherein

[0067] The particles (B) containing titanium oxide as a main component contain TiO2: 90.0 to 98.0% by mass, Al2O3: 0.5 to 3.5% by mass, and SiO2: 0 to 6.0% by mass.

[0068] <3-7> The resin composition according to any one of <3-1> to <3-6>, wherein

[0069] The mass ratio (C-2) / (D) of the polyolefin wax (C-2) and the aromatic sulfonic acid alkali metal salt (D) is 0.15 to 10.0.

[0070] <3-8> The resin composition according to any one of <3-1> to <3-7>, wherein

[0071] The content of at least one filler selected from the group consisting of fibrous glass fillers, fibrous carbon fillers, and plate-shaped glass fillers is less than 1 part by mass based on 100 parts by mass of the polycarbonate resin.

[0072] <3-9> The resin composition according to any one of <3-1> to <3-8>, wherein

[0073] The polyolefin wax (C-2) has a carboxyl group and / or anhydride group thereof,

[0074] The notched Charpy impact strength obtained by molding a 3 mm thick test piece using the resin composition at a cylinder setting temperature of 310° C. and a residence time in the cylinder of 7 minutes and measuring it in accordance with ISO179-1 is compared with the notched Charpy impact strength obtained by measuring it in the same manner as above when molding using the resin composition at a cylinder setting temperature of 280° C. and a cycle time of 1 minute. The impact strength retention rate is 80% or more.

[0075] The molded article obtained by molding the resin composition under the conditions of a cylinder setting temperature of 280° C. and a cycle time of 1 minute was observed by an operating electron microscope. The equivalent circle diameter calculated by using the mathematical formula (1) based on the area of ​​the region where the particles (B) containing titanium oxide as the main component were dispersed was 0.165 μm or less.

[0076] The particles (B) containing titanium oxide as a main component contain TiO2: 90.0-98.0 mass %, Al2O3: 0.5-3.5 mass %, and SiO2: 0-6.0 mass %,

[0077] The mass ratio of the polyolefin wax (C-2) to the aromatic sulfonic acid alkali metal salt (D) is (C-2) / (D) in the range of 0.15 to 10.0.

[0078] The content of at least one filler selected from the group consisting of fibrous glass fillers, fibrous carbon fillers, and plate-shaped glass fillers is less than 1 part by mass based on 100 parts by mass of the polycarbonate resin.

[0079] [Mathematical formula 3]

[0080]

[0081] <3-10> A molded article formed from the resin composition according to any one of <3-1> to <3-9>.

[0082] <3-11> Pellets formed from the resin composition according to any one of <3-1> to <3-9>.

[0083] <3-12> A molded article formed from the pellets according to <3-11>.

[0084] Effects of the Invention

[0085] According to the present invention, a resin composition and a molded article can be provided. The resin composition can provide a molded article that can achieve desired light-shielding properties and has excellent impact resistance, particularly, retention of impact resistance during retention. DETAILED DESCRIPTION

[0086] Hereinafter, a mode for implementing the present invention (hereinafter referred to as "this embodiment") will be described in detail. It should be noted that the following this embodiment is an example for explaining the present invention, and the present invention is not limited to this embodiment.

[0087] In addition, in this specification, "to" is used to mean that the numerical value described before and after it is included as a lower limit and an upper limit.

[0088] In this specification, various physical property values ​​and characteristic values ​​are values ​​at 23° C. unless otherwise specified.

[0089] When the measurement methods and the like described in the standards shown in this specification differ by year, unless otherwise specified, the standards are based on the time point of January 1, 2022.

[0090] The resin composition of the present embodiment comprises 5.0 to 20.0 parts by mass of particles (B) containing titanium oxide as a main component (hereinafter sometimes referred to as "titanium oxide particles"), a polyolefin wax (C), and an aromatic sulfonic acid metal salt (D) based on 100 parts by mass of a polycarbonate resin (A).

[0091] When the polyolefin wax (C) is a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, the content of the polyolefin wax (C-1) is 0.001 to 1.5 parts by mass, and the content of the aromatic sulfonic acid metal salt (D) is 0.01 to 1.5 parts by mass,

[0092] When the polyolefin wax (C) is a polyolefin wax (C-2) having an acid value of 0.5 to 150 mgKOH / g, the content of the polyolefin wax (C-2) is 0.001 to 1.5 parts by mass, and the resin composition contains 0.2 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D). By setting such a configuration, a resin composition that can provide a molded product having an excellent retention rate of impact resistance during retention can be provided.

[0093] In the resin composition of the first embodiment, 5.0 to 20.0 parts by mass of particles (B) having titanium oxide as a main component, 0.001 to 1.5 parts by mass of a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, and 0.01 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D) are contained relative to 100 parts by mass of a polycarbonate resin (A). By setting the above-mentioned structure, a molded product having excellent light-shielding properties and impact resistance, particularly excellent retention of impact resistance during retention, can be provided.

[0094] That is, in the first embodiment, titanium oxide particles (B) are added to achieve shielding properties. In addition, in the first embodiment, polyolefin wax is added to achieve impact resistance. However, it is known that if an acid-modified polyolefin wax is used as the polyolefin wax, there is a tendency to easily attract the hydroxyl groups on the surface of the titanium oxide particles (B) and cause the titanium oxide particles (B) to condense. It can be inferred that in the first embodiment, by using a polyolefin wax with a low acid value (acid-unmodified or acid-slightly modified polyolefin wax (C-1)), the reduction in the dispersibility of the titanium oxide particles (B) can be effectively suppressed. In addition, it can be inferred that in the first embodiment, by using an aromatic sulfonic acid alkali metal salt (D), the dispersibility of the titanium oxide particles (B) is improved.

[0095] In particular, by adopting the configuration of the first embodiment, it is possible to provide a resin composition capable of obtaining a molded article having an excellent retention rate of impact resistance during retention.

[0096] [Details of the resin composition of the second embodiment]

[0097] <Polycarbonate resin (A)>

[0098] The resin composition of the first embodiment contains a polycarbonate resin (A).

[0099] Specifically, the polycarbonate resin (A) is not particularly limited as long as it contains a -[OR-OC(=O)]- unit containing a carbonate bond in the main chain of the molecule (R contains an organic group, preferably a hydrocarbon group, more preferably an aliphatic group, an aromatic group, or both an aliphatic group and an aromatic group and has a straight-chain structure or a branched structure). In the first embodiment, the polycarbonate resin (A) is preferably an aromatic polycarbonate resin, and more preferably a polycarbonate resin having a bisphenol skeleton. By using such a polycarbonate resin, better heat resistance and toughness can be achieved. In the first embodiment, preferably more than 90 mol% of all structural units of the polycarbonate resin having a bisphenol skeleton are structural units having a bisphenol skeleton, and more preferably more than 90 mol% of all structural units are structural units derived from bisphenol A.

[0100] In addition, the viscosity average molecular weight (Mv) of the polycarbonate resin (A) is preferably 10,000 or more, more preferably 12,000 or more, and further preferably 15,000 or more. By setting it to be above the above lower limit, there is a tendency that the durability of the obtained molded article is further improved. The upper limit value of the viscosity average molecular weight (Mv) of the polycarbonate resin (A) is preferably 50,000 or less, more preferably 40,000 or less, and further preferably 30,000 or less. By setting it to be below the above upper limit, there is a tendency that the molding processability of the molded article is further improved.

[0101] The viscosity average molecular weight (Mv) is the limiting viscosity [η] (unit: dL / g) at 25°C obtained by using an Ubbelohde viscometer using dichloromethane as a solvent. According to Schnell's viscosity formula, η = 1.23 × 10 -4 ×Mv 0.83 The calculated value.

[0102] When two or more polycarbonate resins are used, the viscosity average molecular weight is set to the mixture.

[0103] The method for producing the polycarbonate resin (A) is not particularly limited, and polycarbonate resins (A) produced by the conventionally known phosgene method (interfacial polymerization method) or melt method (ester exchange method) can be used. In addition, when the melt method is used, a polycarbonate resin in which the amount of OH groups at the terminal group is adjusted can be used.

[0104] The polycarbonate resin (A) used in the first embodiment may be a recycled product (including a recovered product, a material recycled product, a chemically recycled product, etc.), a defective product, or an end product of a thermoplastic resin.

[0105] In addition to the above, details of the polycarbonate resin (A) can be referred to the description in paragraphs 0013 to 0041 of Japanese Patent Application Laid-Open No. 2021-084942 and paragraphs 0030 to 0035 of Japanese Patent Application Laid-Open No. 2021-119211, the contents of which are incorporated into the present specification.

[0106] The ratio of the polycarbonate resin (A) in the resin composition of the first embodiment is preferably 83% by mass or more, more preferably 85% by mass or more, and further preferably 87% by mass or more. By setting it to more than the above-mentioned lower limit, there is a tendency that the impact resistance of the obtained molded product is further improved. In addition, the ratio of the polycarbonate resin (A) in the resin composition of the first embodiment is preferably less than 95% by mass, more preferably less than 93% by mass. By setting it to less than the above-mentioned upper limit, there is a tendency that the light-shielding property of the obtained molded product is further improved.

[0107] The resin composition of the first embodiment may contain only one polycarbonate resin (A) or two or more polycarbonate resins (A). When containing two or more polycarbonate resins (A), the total amount is preferably within the above range.

[0108] <Particles containing titanium oxide as a main component (B)>

[0109] The resin composition of the first embodiment contains particles (titanium oxide particles) (B) containing titanium oxide as a main component. By containing the titanium oxide particles (B), the light shielding property of the obtained molded article can be improved.

[0110] The main component is titanium oxide, which is the largest component in the titanium oxide particles (B). Usually, the proportion of titanium oxide (preferably titanium dioxide) in the titanium oxide particles (B) is 85.0% by mass or more, preferably 90.0% by mass or more.

[0111] The titanium oxide particles (B) preferably contain TiO2: 90.0-98.0 mass%, Al2O3: 0.5-3.5 mass%, and SiO2: 0-6.0 mass%. In addition to the above components, the titanium oxide particles (B) may also contain SO3: 0-0.1 mass%, Na2O: 0-0.15 mass%, and Cl: 0-0.01 mass%. In addition, the titanium oxide particles (B) may also contain other components, and the total of these components is 100 mass%.

[0112] In the first embodiment, the titanium oxide particles (B) can be rutile titanium oxide particles or anatase titanium oxide particles. In addition, the surface of the titanium oxide particles (B) is preferably treated with a surface treatment agent. That is, it is preferred that the surface of the titanium oxide particles (B) has a layer (particularly an organic layer) formed by a surface treatment agent. By setting such a structure, it is easier to disperse titanium oxide in the polycarbonate resin (A) to obtain a molded product with a better appearance. The surface treatment agent can exemplify a polymer, preferably a siloxane compound, particularly preferably hydrogen methyl siloxane, dimethyl siloxane, etc. The surface treatment agent can be physically adsorbed on the titanium oxide surface or chemically bonded to the titanium oxide surface.

[0113] The titanium oxide is typically titanium dioxide.

[0114] In the first embodiment, the resin composition contains 5.0 to 20.0 parts by mass of titanium oxide particles (B) relative to 100 parts by mass of the polycarbonate resin (A). By setting it to be above the above lower limit, there is a tendency for the shielding property to be improved. In addition, by setting it to be below the above upper limit, there is a tendency for higher impact resistance to be obtained during retention molding.

[0115] In the first embodiment, the content of the titanium oxide particles (B) is preferably 6.0 parts by mass or more, more preferably 8.0 parts by mass or more, and even more preferably 9.0 parts by mass or more, relative to 100 parts by mass of the polycarbonate resin (A). In the first embodiment, the content of the titanium oxide particles (B) is preferably 18.0 parts by mass or less, more preferably 16.0 parts by mass or less, even more preferably 14.0 parts by mass or less, and even more preferably 12.0 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin (A).

[0116] The resin composition of the first embodiment may contain only one type of titanium oxide particles (B) or two or more types. When containing two or more types, the total amount is preferably within the above range.

[0117] <Polyolefin wax having an acid value of less than 0.5 mgKOH / g (C-1)>

[0118] The resin composition of the first embodiment contains a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g (acid-unmodified or acid-slightly modified polyolefin wax (C-1)). By containing the acid-unmodified or acid-slightly modified polyolefin wax (C-1), the aggregation of the titanium oxide particles (B) can be suppressed and the impact resistance can be improved.

[0119] The acid value of the acid-unmodified or acid-slightly modified polyolefin wax (C-1) is preferably 0.4 mgKOH / g or less, more preferably 0.3 mgKOH / g or less, further preferably 0.2 mgKOH / g or less, further preferably 0.1 mgKOH / g or less, further more preferably 0.01 mgKOH / g or less, and particularly preferably 0 mgKOH / g or less than the detection limit.

[0120] The acid value of the acid-unmodified or acid-slightly modified polyolefin wax (C-1) can be measured according to the description in the Examples described below.

[0121] The viscosity average molecular weight of the acid-unmodified or acid-slightly modified polyolefin wax (C-1) used in the first embodiment is preferably 1000 or more, more preferably 2000 or more, and further preferably 3000 or more, and preferably 6000 or less, and more preferably 5000 or less. By setting it to be above the lower limit, there is a tendency that the impact properties of the obtained molded article are improved. In addition, by setting it to be below the upper limit, there is a tendency that the dispersibility of titanium oxide in the obtained molded article is further improved.

[0122] When the acid-unmodified or slightly acid-modified polyolefin wax (C-1) has an acid group, it is preferably a carboxyl group and / or anhydride thereof, more preferably a maleic acid group and / or a maleic anhydride group, and further preferably a maleic anhydride group.

[0123] Examples of the acid-unmodified or acid-slightly modified polyolefin wax (C-1) include polyethylene, polypropylene, polybutene, α-olefin polymers, ethylene-propylene copolymers, ethylene-butene copolymers and the like waxes, preferably polyethylene waxes, more preferably low-density polyethylene waxes.

[0124] The density of the acid-unmodified or acid-slightly modified polyolefin wax (C-1) is preferably 700 kg / m 3 More preferably 800 kg / m 3 More preferably, 900 kg / m 3More than, preferably 1100kg / m 3 Less than, more preferably 1000kg / m 3 the following.

[0125] The melting point of the acid-unmodified or acid-slightly modified polyolefin wax (C-1) is preferably 60 to 145°C.

[0126] As commercially available products of the acid-unmodified or slightly acid-modified polyolefin wax (C-1), for example, Mitsui Hi-WAX 100P, 200P, 400P, 800P, 110P, 210P, 220P, 320P, 410P, 420P, 720P and the like manufactured by Mitsui Chemicals, Inc. can be used.

[0127] Relative to 100 parts by mass of polycarbonate resin (A), the content of the acid unmodified or slightly acid modified polyolefin wax (C-1) in the resin composition of the first embodiment is 0.001 parts by mass or more, preferably 0.005 parts by mass or more, more preferably 0.01 parts by mass or more, further preferably 0.05 parts by mass or more, further preferably 0.1 parts by mass or more, further more preferably 0.2 parts by mass or more. By being set to more than the above-mentioned lower limit, there is a tendency that the retention rate of impact resistance when it is retained during molding is further improved. In addition, relative to 100 parts by mass of polycarbonate resin (A), the content of the acid unmodified or slightly acid modified polyolefin wax (C-1) in the resin composition of the first embodiment is 1.5 parts by mass or less, preferably 1.3 parts by mass or less, more preferably 1.1 parts by mass or less, further preferably 0.9 parts by mass or less, further preferably 0.7 parts by mass or less, further more preferably 0.6 parts by mass or less. By being set to less than the above-mentioned upper limit, there is a tendency that the dispersibility of titanium oxide is improved.

[0128] The resin composition of the first embodiment may contain only one type of acid-unmodified or acid-slightly-modified polyolefin wax (C-1), or may contain two or more types. When containing two or more types, the total amount is preferably within the above range.

[0129] The resin composition of the first embodiment may contain a polyolefin wax having an acid value of 0.5 mgKOH / g or more (polyolefin wax (C-2) described later, etc.), or may not contain it. In the first embodiment, it is preferred that the polyolefin wax having an acid value of 0.5 mgKOH / g or more is substantially not contained. Substantially not contained means that the content of the polyolefin wax having an acid value of 0.5 mgKOH / g or more is 10% by mass or less of the content of the acid-unmodified or acid-slightly modified polyolefin wax (C-1), preferably 5% by mass or less, more preferably 3% by mass or less, and further preferably 1% by mass or less.

[0130] <Alkali metal salt of aromatic sulfonic acid (D)>

[0131] In the resin composition of the first embodiment, 0.01 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D) is contained relative to 100 parts by mass of the polycarbonate resin (A). By containing the aromatic sulfonic acid alkali metal salt (D), the aggregation of the titanium oxide particles (B) can be effectively suppressed, and the impact resistance of the obtained molded article, especially the retention rate of the impact resistance during retention, can be improved.

[0132] The aromatic sulfonic acid alkali metal salt (D) is generally a component used as a flame retardant for polycarbonate resin. In the first embodiment, the titanium oxide particles (B) are successfully dispersed efficiently by using the aromatic sulfonic acid alkali metal salt (D).

[0133] Aromatic sulfonic acid alkali metal salt (D) refers to an alkali metal salt of a sulfonic acid containing an aromatic ring, and more preferably an alkali metal salt of a sulfonic acid containing one or two benzene rings. The alkali metal constituting the alkali metal salt is preferably lithium, sodium, potassium and rubidium, more preferably sodium or potassium, and further preferably sodium. In addition, the aromatic sulfonic acid alkali metal salt (D) may contain fluorine atoms, preferably a fluorine content of less than 1%, more preferably less than 0.5%, and further preferably no fluorine atoms. In addition, the aromatic sulfonic acid alkali metal salt (D) may contain halogen atoms, preferably a halogen content of less than 1%, more preferably less than 0.5%, and further preferably no halogen atoms. It should be noted that when the number of hydrogen atoms bonded to the carbon atoms possessed by the aromatic sulfonic acid alkali metal salt (D) is set to A and the number of fluorine atoms or halogen atoms is set to B, the fluorine content and the halogen content are each independently a value represented by B / (A+B).

[0134] The aromatic sulfonic acid alkali metal salt (D) is preferably a compound represented by the formula (D1).

[0135] Formula (D1)

[0136] [Chemical formula 1]

[0137]

[0138] (In formula (D1), M is an alkali metal and R is a substituent.)

[0139] M is preferably lithium, sodium, potassium, and rubidium, more preferably sodium or potassium, and further preferably sodium.

[0140] The formula weight of R is preferably 70-300.

[0141] R is preferably a hydrocarbon group, or R 1 -S(=O)2-, where R 1 It is a hydrocarbon group.

[0142] The hydrocarbon group as R is preferably an alkyl group having 1 to 10 carbon atoms, more preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and still more preferably a methyl group.

[0143] As R 1 The hydrocarbon group is preferably a substituted or unsubstituted phenyl group. The substituent in this case is preferably an alkyl group having 1 to 10 carbon atoms, more preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and still more preferably a methyl group.

[0144] In formula (D1), R is preferably an alkyl group having 1 to 10 carbon atoms, more preferably a methyl group, an ethyl group, a propyl group or a butyl group, and further preferably a methyl group.

[0145] The molecular weight of the aromatic sulfonic acid alkali metal salt (D) used in the first embodiment is preferably 100 to 900, more preferably 100 to 500.

[0146] Specific examples of the aromatic sulfonic acid alkali metal salt (D) used in the first embodiment are shown below. Of course, in the first embodiment, the aromatic sulfonic acid alkali metal salt (D) is not limited thereto.

[0147] [Chemical formula 2]

[0148]

[0149] As the aromatic sulfonic acid alkali metal salt (D), commercially available products such as CHEMGUARD-NATS manufactured by Sun Chemical Co., Ltd. and KSS-FR manufactured by Arichem Co., Ltd. can be used.

[0150] Relative to 100 parts by mass of polycarbonate resin (A), the content of the aromatic sulfonic acid alkali metal salt (D) in the resin composition of the first embodiment is 0.01 parts by mass or more, preferably more than 0.1 parts by mass, more preferably more than 0.15 parts by mass, more preferably more than 0.2 parts by mass, more preferably more than 0.24 parts by mass, and more preferably more than 0.26 parts by mass. By setting it to above the above lower limit, there is a tendency that the impact resistance, especially the retention rate of the impact resistance during retention, is further improved. In addition, relative to 100 parts by mass of polycarbonate resin (A), the upper limit of the content of the aromatic sulfonic acid alkali metal salt (D) is 1.5 parts by mass or less, preferably 1.3 parts by mass or less, more preferably 1.2 parts by mass or less, more preferably 1.0 parts by mass or less, more preferably 0.8 parts by mass or less, more preferably 0.7 parts by mass or less, and more preferably 0.6 parts by mass or less. By setting it to above the above lower limit, there is a tendency that the impact resistance, especially the retention rate of the impact resistance during retention, is further improved.

[0151] The resin composition of the first embodiment may contain only one kind of aromatic sulfonic acid alkali metal salt (D), or may contain two or more kinds. When containing two or more kinds, the total amount is preferably within the above range.

[0152] The resin composition of the first embodiment may or may not contain an alkali metal salt other than the aromatic sulfonic acid alkali metal salt (D). As alkali metal salts other than the aromatic sulfonic acid alkali metal salt (D), reference may be made to paragraphs 0069 to 0078 of JP-A-2015-117298, the contents of which are incorporated herein.

[0153] The resin composition of the first embodiment preferably contains substantially no alkali metal salts other than the aromatic sulfonic acid alkali metal salt (D). Substantially containing no alkali metal salts means that the content of alkali metal salts other than the aromatic sulfonic acid alkali metal salt (D) is 10% by mass or less, preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less of the content of the aromatic sulfonic acid alkali metal salt (D) contained in the resin composition.

[0154] In the resin composition of the first embodiment, the mass ratio of acid unmodified or acid slightly modified polyolefin wax (C-1) / aromatic sulfonic acid alkali metal salt (D) is preferably more than 0.15, more preferably more than 0.3, more preferably more than 0.5, more preferably more than 0.7, and more preferably more than 1.0. By being set to more than the above-mentioned lower limit, there is a tendency that the dispersibility of titanium oxide is further improved. In addition, the mass ratio of acid unmodified or acid slightly modified polyolefin wax (C-1) / aromatic sulfonic acid alkali metal salt (D) is preferably less than 20, more preferably less than 10, more preferably less than 5, more preferably less than 3, further more preferably less than 2, and more preferably less than 1.5. By being set to less than the above-mentioned upper limit, there is a tendency that the retention rate of impact resistance when staying during molding is further improved.

[0155] <Filling material (E)>

[0156] The resin composition of the first embodiment may or may not contain a filler. In the resin composition of the first embodiment, the content of at least one filler selected from fibrous glass fillers, fibrous carbon fillers, and plate-shaped glass fillers is preferably less than 1 mass part relative to 100 mass parts of polycarbonate resin (A). In addition, in the resin composition of the first embodiment, the content of the filler is preferably less than 1 mass part relative to 100 mass parts of polycarbonate resin (A).

[0157] As for the filler, the description in paragraphs 0052 to 0066 of Japanese Patent Application Laid-Open No. 2006-249286 can be referred to, and the contents are incorporated into this specification.

[0158] <Other ingredients>

[0159] The resin combination of the first embodiment may further include other components in addition to the above. As other components, reinforcing materials (except filler (E)), mold release agents, colorants (such as carbon black, etc.) except titanium oxide, stabilizers (heat stabilizers, antioxidants, etc.), flame retardants except alkali metal salts, flame retardant aids, anti-drip agents, ultraviolet light absorbers, fluorescent whitening agents, impact resistance modifiers, epoxy compounds, antifogging agents, flow modifiers, plasticizers, dispersants, antibacterial agents, antiviral agents, etc. can be exemplified. Reinforcing materials include at least one filling material selected from fibrous glass filling materials, fibrous carbon filling materials and plate-shaped glass filling materials, and these filling materials are preferably less than 1 mass part relative to 100 mass parts of polycarbonate resin. For details of these components, reference can be made to paragraphs 0107 to 0115 of Japanese Patent Application Publication No. 2014-136710, paragraphs 0106 to 0128 of Japanese Patent Application Publication No. 2015-117298, and paragraphs 0055 to 0061 of Japanese Patent Application Publication No. 2018-095706, and the contents thereof are incorporated into this specification.

[0160] The content of the other components is, if contained, for example, 0.001 mass % or more, and for example, 5.0 mass % or less, preferably 3.0 mass % or less, and more preferably 1.0 mass % or less, based on the mass of the resin composition.

[0161] [Details of the resin composition of the second embodiment]

[0162] In the resin composition of the second embodiment, 5.0 to 20.0 parts by mass of particles (B) containing titanium oxide as a main component, 0.001 to 1.5 parts by mass of a polyolefin wax (C-2) having an acid value of 0.5 to 150 mgKOH / g (hereinafter, sometimes referred to as "acidic polyolefin wax (C-2)"), and 0.2 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D) are contained relative to 100 parts by mass of a polycarbonate resin (A). By setting the above-mentioned structure, a molded product can be provided which can achieve the desired light-shielding property, has excellent surface appearance, and has excellent impact resistance, especially excellent retention rate of impact resistance during retention.

[0163] That is, in the second embodiment, titanium oxide particles (B) are added to achieve shielding properties. In addition, in the second embodiment, acid-modified polyolefin wax is added to achieve impact resistance. However, it can be inferred that if acid-modified polyolefin wax is used as polyolefin wax, there is a tendency that the acid-modified polyolefin wax easily attracts hydroxyl groups on the surface of titanium oxide particles and causes the first embodiment of the acid-unmodified or acid-slightly modified polyolefin wax (C-1) of titanium oxide particles (B) to agglomerate. It can be inferred that in the second embodiment, if a large amount of aromatic sulfonic acid alkali metal salt (D) is used, the dispersibility of titanium oxide particles (B) can be improved.

[0164] In particular, by adopting the configuration of the second embodiment, a molded product can be obtained that is excellent in the retention rate of impact resistance when the resin composition is allowed to remain during molding.

[0165] <Polycarbonate resin (A)>

[0166] The resin composition of the second embodiment contains a polycarbonate resin (A). The details of the polycarbonate resin (A) in the resin composition of the second embodiment are the same as those of the polycarbonate resin (A) in the resin composition of the first embodiment, and the preferred range is also the same.

[0167] <Particles containing titanium oxide as a main component (B)>

[0168] The resin composition of the second embodiment includes particles (titanium oxide particles) (B) with titanium oxide as the main component. By including the titanium oxide particles (B), the light-shielding property of the obtained molded product can be achieved. The details of the titanium oxide particles (B) in the resin composition of the second embodiment are the same as the titanium oxide particles (B) in the resin composition of the first embodiment, and the preferred range is also the same.

[0169] <Polyolefin wax having an acid value of 0.5 to 150 mgKOH / g (C-2)>

[0170] The resin composition of the second embodiment contains polyolefin wax (C-2) having an acid value of 0.5 to 150 mgKOH / g (acid-modified polyolefin wax (C-2)). By containing the acid-modified polyolefin wax (C-2), a molded article having excellent surface appearance and excellent impact resistance can be obtained.

[0171] The acid value of the acid-modified polyolefin wax (C-2) is preferably 0.8 mgKOH / g or more, more preferably 1.2 mgKOH / g or more, further preferably 5 mgKOH / g or more, further preferably 10 mgKOH / g or more, further more preferably 20 mgKOH / g or more, still further preferably 30 mgKOH / g or more, particularly preferably 40 mgKOH / g or more, further particularly preferably 50 mgKOH / g or more, and may be 70 mgKOH / g or more. The upper limit of the acid value of the acid-modified polyolefin wax (C-2) is practically 150 mgKOH / g or less, and may be 110 mgKOH / g or less.

[0172] The acid value of the acid-modified polyolefin wax (C-2) can be measured according to the description in the Examples described below.

[0173] The viscosity average molecular weight of the acid-modified polyolefin wax (C-2) used in the second embodiment is preferably 1000 or more, and preferably 20000 or less, and more preferably 15000 or less. When the viscosity average molecular weight is set to be equal to or greater than the above lower limit, the impact properties of the obtained molded article tend to be improved. In addition, when the viscosity average molecular weight is set to be equal to or less than the above upper limit, the dispersibility of titanium oxide in the obtained molded article tends to be improved.

[0174] The acid-modified polyolefin wax (C-2) preferably has a carboxyl group and / or an anhydride group thereof, more preferably has a maleic acid group and / or a maleic anhydride group, and further preferably has a maleic anhydride group.

[0175] Examples of the acid-modified polyolefin wax (C-2) include polyethylene, polypropylene, polybutene, α-olefin polymer, ethylene-propylene copolymer, ethylene-butene copolymer and the like waxes, and polyethylene wax is preferred, and low-density polyethylene wax is more preferred.

[0176] The density of the acid-modified polyolefin wax (C-2) is preferably 700 kg / m 3 More preferably 800 kg / m 3 More preferably, 900 kg / m 3 More than 1100 kg / m 3 Less than, more preferably 1000kg / m 3 the following.

[0177] The melting point of the acid-modified polyolefin wax (C-2) is preferably 60 to 145°C.

[0178] As commercially available products of the acid-modified polyolefin wax (C-2), for example, 210MP, 220MP, 310MP, 320MP, 405MP, 405MPF, 4051E, 4052E, 4202E, 4252E, 1105A, 2203A manufactured by Mitsui Chemicals, Inc., and DIACARNA 30M manufactured by Mitsubishi Chemical, etc. can be used.

[0179] Relative to 100 parts by mass of polycarbonate resin (A), the content of the acid-modified polyolefin wax (C-2) in the resin composition of the second embodiment is more than 0.001 parts by mass, preferably more than 0.005 parts by mass, more preferably more than 0.01 parts by mass, further preferably more than 0.06 parts by mass, further preferably more than 0.1 parts by mass, further more preferably more than 0.2 parts by mass. By being set to more than the above-mentioned lower limit, there is a tendency that the retention rate of impact resistance when retained during molding is further improved. In addition, relative to 100 parts by mass of polycarbonate resin (A), the content of the acid-modified polyolefin wax (C-2) in the resin composition of the second embodiment is less than 1.5 parts by mass, preferably less than 1.3 parts by mass, more preferably less than 1.1 parts by mass, further preferably less than 0.9 parts by mass, further preferably less than 0.7 parts by mass, further more preferably less than 0.5 parts by mass. By being set to less than the above-mentioned upper limit, there is a tendency that the dispersibility of titanium oxide is further improved.

[0180] The resin composition of the second embodiment may contain only one type of acid-modified polyolefin wax (C-2), or may contain two or more types. When containing two or more types, the total amount is preferably within the above range.

[0181] The resin composition of the second embodiment may contain a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, or may not contain it. In the second embodiment, it is preferred that the polyolefin wax having an acid value of less than 0.5 mgKOH / g is not substantially contained. Substantially not contained means that the content of the polyolefin wax having an acid value of less than 0.5 mgKOH / g is 10% by mass or less of the content of the acid-modified polyolefin wax (C-2), preferably 5% by mass or less, more preferably 3% by mass or less, and further preferably 1% by mass or less.

[0182] <Alkali metal salt of aromatic sulfonic acid (D)>

[0183] In the resin composition of the second embodiment, 0.2 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D) is contained relative to 100 parts by mass of the polycarbonate resin (A). By containing the aromatic sulfonic acid alkali metal salt (D), the aggregation of the titanium oxide particles (B) can be effectively suppressed, and the impact resistance of the obtained molded article, especially the retention rate of the impact resistance during retention, can be improved.

[0184] Aromatic sulfonic acid alkali metal salt (D) is generally used as a flame retardant for polycarbonate resin. In the second embodiment, the titanium oxide particles (B) are successfully dispersed effectively by using an aromatic sulfonic acid alkali metal salt (D) in an amount larger than the amount usually blended as a flame retardant.

[0185] The details of the aromatic sulfonic acid alkali metal salt (D) are the same as the preferred range of the aromatic sulfonic acid alkali metal salt (D) in the first embodiment except for the content.

[0186] Relative to 100 parts by mass of polycarbonate resin (A), the content of the aromatic sulfonic acid alkali metal salt (D) in the resin composition of the second embodiment is 0.2 parts by mass or more, preferably 0.24 parts by mass or more, more preferably 0.26 parts by mass or more. By setting it to above the above lower limit, there is a tendency that the impact resistance, especially the retention rate of the impact resistance during retention, is further improved. In addition, relative to 100 parts by mass of polycarbonate resin (A), the upper limit of the content of the aromatic sulfonic acid alkali metal salt (D) is 1.5 parts by mass or less, preferably 1.3 parts by mass or less, more preferably 1.2 parts by mass or less, further preferably 1.0 parts by mass or less, further preferably 0.8 parts by mass or less, further more preferably 0.7 parts by mass or less, and further preferably 0.6 parts by mass or less. By setting it to above the above lower limit, there is a tendency that the impact resistance, especially the retention rate of the impact resistance during retention, is further improved.

[0187] The resin composition of the second embodiment may contain only one kind of aromatic sulfonic acid alkali metal salt (D), or may contain two or more kinds. When containing two or more kinds, the total amount is preferably within the above range.

[0188] The resin composition of the second embodiment may or may not contain an alkali metal salt other than the aromatic sulfonic acid alkali metal salt (D). As alkali metal salts other than the aromatic sulfonic acid alkali metal salt (D), reference may be made to paragraphs 0069 to 0078 of JP-A-2015-117298, the contents of which are incorporated herein.

[0189] The resin composition of the second embodiment preferably contains substantially no alkali metal salts other than the aromatic sulfonic acid alkali metal salt (D). Substantially containing no alkali metal salts means that the content of alkali metal salts other than the aromatic sulfonic acid alkali metal salt (D) is 10% by mass or less, preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less of the content of the aromatic sulfonic acid alkali metal salt (D) contained in the resin composition.

[0190] In the resin composition of the second embodiment, the mass ratio (C-2) / (D) of acid-modified polyolefin wax (C-2) / aromatic sulfonic acid alkali metal salt (D) is preferably more than 0.15, and may be more than 0.5, more than 0.7, or more than 0.9. By being set to more than the above-mentioned lower limit, there is a tendency that the impact resistance, particularly the impact characteristics after high temperature retention, are improved. In addition, the mass ratio (C-2) / (D) of acid-modified polyolefin wax (C-2) / aromatic sulfonic acid alkali metal salt (D) is preferably less than 10.0, more preferably less than 8.0, further preferably less than 5.0, further preferably less than 3.0, further more preferably less than 2.0, further preferably less than 1.5, and may be less than 0.9. By being set to less than the above-mentioned upper limit, there is a tendency that the dispersibility of titanium oxide is improved.

[0191] <Filling material (E)>

[0192] The resin composition of the second embodiment may or may not contain a filler. In the resin composition of the second embodiment, the content of at least one filler selected from fibrous glass fillers, fibrous carbon fillers, and plate-shaped glass fillers is preferably less than 1 mass part relative to 100 mass parts of polycarbonate resin (A). In addition, in the resin composition of the second embodiment, the content of the filler is preferably less than 1 mass part relative to 100 mass parts of polycarbonate resin (A).

[0193] As for the filler, the description in paragraphs 0052 to 0066 of Japanese Patent Application Laid-Open No. 2006-249286 can be referred to, and the contents are incorporated into this specification.

[0194] <Other ingredients>

[0195] The resin composition of the second embodiment may further include other components other than the above. As other components, reinforcing materials (except filler (E)), mold release agents, colorants other than titanium oxide (for example, carbon black, etc.), stabilizers (thermal stabilizers, antioxidants, etc.), flame retardants other than alkali metal salts, flame retardant aids, anti-drip agents, ultraviolet light absorbers, fluorescent whitening agents, impact resistance modifiers, epoxy compounds, antifogging agents, flowability modifiers, plasticizers, dispersants, antibacterial agents, antiviral agents, etc. can be exemplified.

[0196] For details of these components, reference can be made to paragraphs 0107 to 0115 of Japanese Patent Application Publication No. 2014-136710, paragraphs 0106 to 0128 of Japanese Patent Application Publication No. 2015-117298, and paragraphs 0055 to 0061 of Japanese Patent Application Publication No. 2018-095706, and the contents thereof are incorporated into this specification.

[0197] The content of the other components is, if contained, for example, 0.001 mass % or more, and for example, 5.0 mass % or less, preferably 3.0 mass % or less, and more preferably 1.0 mass % or less, based on the mass of the resin composition.

[0198] [Physical properties of resin composition]

[0199] The resin composition of the present embodiment (the resin composition of the first embodiment and the resin composition of the second embodiment) can provide a molded product with high shielding properties. In particular, the total light transmittance when the resin composition of the present embodiment is molded into a thickness of 1.0 mm is preferably 0.04% or less, more preferably less than 0.02%, and further preferably 0.015% or less. The lower limit of the total light transmittance may be 0%, but even if it is 0.001% or more, the required performance can be fully met.

[0200] The total light transmittance can be measured according to the description in the Examples described later.

[0201] In addition, the resin composition of the present embodiment can provide a molded product with excellent impact resistance. In particular, a 3 mm thick test piece is molded using the above resin composition at a cylinder temperature of 280° C. and a cycle time of 1 minute, and the notched Charpy impact strength obtained by measurement based on ISO179-1 is preferably 40 kJ / m 2 More preferably 42 kJ / m 2 More preferably, 44 kJ / m 2 More preferably, 46 kJ / m 2 More preferably, 47 kJ / m 2 The upper limit of the notched Charpy impact strength is not particularly limited, but is practically 70 kJ / m 2 the following.

[0202] The resin composition of the present embodiment can achieve high impact resistance even when it is retained in the barrel during molding. Specifically, a 3 mm thick test piece is molded using the resin composition of the present embodiment under the conditions of a barrel setting temperature of 310° C. and a retention time in the barrel of 7 minutes, and the notched Charpy impact strength obtained by measurement based on ISO179-1 is preferably 30 kJ / m 2 More preferably 32 kJ / m 2 More preferably, 34 kJ / m 2 More preferably, 39 kJ / m 2 More preferably, 40 kJ / m 2 The upper limit of the notched Charpy impact strength is not particularly limited, but is practically 60 kJ / m2 the following.

[0203] The resin composition of the present embodiment can maintain high impact resistance even when it remains in the cylinder during molding.

[0204] Specifically, the notched Charpy impact strength obtained by molding a 3 mm thick test piece using the resin composition of the first embodiment under the conditions of a barrel setting temperature of 310° C. and a residence time in the barrel of 7 minutes and measuring it based on ISO179-1 is compared with the notched Charpy impact strength obtained by measuring it by the same method as above when molding using the resin composition of the first embodiment at a barrel setting temperature of 280° C. and a cycle time of 1 minute. The impact strength retention rate is preferably 72% or more, more preferably 73% or more, further preferably 75% or more, further preferably 80% or more, further more preferably 83% or more, further preferably 85% or more, and particularly preferably 90% or more. The upper limit of the above impact strength retention rate is not particularly limited, and is actually 99% or less.

[0205] In addition, the notched Charpy impact strength obtained by molding a 3 mm thick test piece using the resin composition of the second embodiment under the conditions of a barrel setting temperature of 310° C. and a residence time in the barrel of 7 minutes and measuring it based on ISO179-1 is compared with the notched Charpy impact strength obtained by measuring it by the same method as above when molding using the resin composition of the second embodiment at a barrel setting temperature of 280° C. and a cycle time of 1 minute. The impact strength retention rate is preferably 80% or more, more preferably 82% or more, further preferably 84% or more, further preferably 86% or more, and further more preferably 88% or more. The upper limit of the above impact strength retention rate is not particularly limited, and is actually 99% or less.

[0206] The notched Charpy impact strength can be measured according to the description in the examples described later.

[0207] The resin composition of the present embodiment (particularly the resin composition of the second embodiment) can effectively suppress aggregation of the titanium oxide particles (B) in a molded article.

[0208] Specifically, the molded product obtained by molding the resin composition of the present embodiment under the conditions of a barrel setting temperature of 280° C. and a cycle time of 1 minute is observed by an operating electron microscope, and the equivalent circle diameter calculated using mathematical formula (1) based on the area of ​​the region of the dispersed particles (B) with titanium oxide as the main component is preferably 0.165 μm or less. Here, π is the pi. Such a small equivalent circle diameter can be achieved by adjusting the amount of titanium oxide particles (B), adding potassium diphenylsulfonate, and adjusting the amount of potassium diphenylsulfonate.

[0209] [Formula 4]

[0210]

[0211] The smaller the equivalent circle diameter in this embodiment, the less aggregation of the titanium oxide particles (B) in the molded article. In addition, by suppressing the aggregation of the titanium oxide particles (B), the surface appearance of the molded article is also improved.

[0212] The equivalent circle diameter is preferably 0.164 μm or less, more preferably 0.163 μm or less, further preferably 0.162 μm or less, and further preferably 0.160 μm or less. The lower limit of the equivalent circle diameter is not particularly limited, but is practically 0.050 μm or more.

[0213] The equivalent circle diameter in this embodiment can be measured according to the description in the examples described later.

[0214] [Manufacturing of resin composition]

[0215] The method for producing the resin composition of the present embodiment is not particularly limited, and a known method for producing the resin composition can be widely adopted, and the following method can be cited: using various mixers such as a tumble mixer and a Henschel mixer, polycarbonate resin (A), titanium oxide particles (B), polyolefin wax (C-1, C-2), and aromatic sulfonic acid alkali metal salt (D), and other components prepared as required, are pre-mixed, and then melt-kneaded using a mixer such as a Banbury mixer, a roll, a Brabender extruder, a single-screw mixing extruder, a twin-screw mixing extruder, and a kneader. It should be noted that the temperature of the melt-kneading is not particularly limited, and is usually in the range of 240 to 320°C.

[0216] One embodiment of the resin composition of the present embodiment is a pellet.

[0217] The resin composition or particles of the present embodiment can be formed into various molded products. That is, the molded product of the present embodiment is a molded product formed by the resin composition or particles of the present embodiment. The molding method of the molded product is not particularly limited, and examples thereof are given, and hollow molding methods such as injection molding, ultra-high-speed injection molding, injection compression molding, two-color molding, gas-assisted, etc., molding methods using heat-insulating molds, molding methods using rapid heating molds, foam molding (also including supercritical fluids), embedded molding, IMC (in-mold coating molding, In-mold coating molding) molding methods, extrusion molding, sheet molding, thermoforming, rotational molding, stacking molding, compression molding, blow molding, etc. can be cited, wherein preferably injection molding.

[0218] In addition, the shape of the molded product of this embodiment is not particularly limited and can be appropriately selected according to the use and purpose of the molded product. For example, there can be various shapes of molded products such as plate-shaped, disk-shaped, rod-shaped, sheet-shaped, film-shaped, cylindrical, ring-shaped, circular, elliptical, polygonal, irregular, hollow, frame-shaped, box-shaped, panel-shaped molded products, and molded products of special shapes.

[0219] The molded article of this embodiment is preferably used as parts of structural members, parts of portable electronic devices, parts of vehicles and medical devices, other electronic parts including circuits, containers for food and medicines, and composite materials for forming these parts.

[0220] In particular, the molded article of the present embodiment can be preferably used as a vehicle-mounted component, specifically, a headlight, and in particular, a light guide base.

[0221] Example

[0222] Below, enumerate embodiment and the present invention is described more specifically.As long as do not depart from the gist of the present invention, the material, dosage, ratio, processing content, processing procedure etc. shown in the following examples can be appropriately changed.Therefore, the scope of the present invention is not limited to the specific examples shown below.

[0223] When the measuring equipment used in the examples is difficult to obtain due to discontinuation of production or the like, other equipment having equivalent performance may be used for the measurement.

[0224] 1. Raw materials

[0225] As raw materials, the raw materials shown in the following table were used.

[0226] [Table 1]

[0227]

[0228] The titanium oxide particles contain TiO2: 90.0 to 98.0 mass %, Al2O3: 0.5 to 3.5 mass %, and SiO2: 0 to 6.0 mass %.

[0229] The metal salts (D1) and (D3) are alkali metal salts of aromatic sulfonic acids containing no fluorine atoms (fluorination rate 0%), and the metal salt (D2) is a sulfonic acid salt containing fluorine atoms (fluorination rate 100%).

[0230] In addition, 0.1 mass % of S-100A manufactured by Riken Vitamin Co., Ltd. and 0.3 mass % of VPG861 manufactured by Emery Oleochemicals Co., Ltd. were added to all samples examined in Examples and Comparative Examples as release agents, and 0.03 mass % of ADK STAB 2112 manufactured by ADEKA Industries Co., Ltd. was added as a stabilizer.

[0231] In Tables 2 to 5, for "polycarbonate resin (A1) / (A2)", the polycarbonate resin (A1) and the polycarbonate resin (A2) were adjusted to have a melt volume flow rate (MVR, 300°C,

[0232] 1.2kgf) becomes 17.5cm 3 The mass ratio of the polycarbonate resin (A1) to the polycarbonate resin (A2) in "polycarbonate resin (A1) / (A2)" was about 77:13.

[0233] <Determination of acid value of polyolefin wax>

[0234] The acid value of the polyolefin wax was measured in accordance with JIS K0070.

[0235] <Measurement of viscosity average molecular weight (Mv) of polyolefin wax>

[0236] The intrinsic viscosity (η) was determined according to ASTM D445, and Mv (viscosity average molecular weight) was calculated from the viscosity formula [η].

[0237] 2. Examples 1-1 to 1-13, Comparative Examples 1-1 to 1-9

[0238] <Preparation of resin pellets>

[0239] The components described in Table 1 were mixed in the proportions shown in Tables 2 to 6 (each component is in parts by mass), uniformly mixed by a tumble mixer to prepare a mixture, and the mixture was supplied to a twin-screw extruder ("TEX25αIII" manufactured by Nippon Steel Works, Ltd.), kneaded under the conditions of a screw speed of 700 rpm, a discharge amount of 20 kg / hour, and a drum temperature of 260°C, and extruded from the front end of the nozzle in the form of strands. The extrudate was rapidly cooled in a water tank, cut and pelletized using a pelletizer, and pellets of a resin composition were obtained.

[0240] <Mold deposite>

[0241] The pellets obtained above were dried at 120°C for 5 hours and then molded 200 times using an injection molding machine (SE7M-C12 manufactured by Sumitomo Heavy Industries, Ltd.) at a barrel temperature of 280°C, a mold temperature of 40°C, a screw speed of 300 rpm, and an injection speed of 4 mm / s. During this process, the mold contamination status was evaluated based on the following criteria. Five experts confirmed and judged by majority vote.

[0242] A: The degree of mold contamination is the same as that of metal salts and wax without additives.

[0243] B: Other than A above (for example, the degree of mold contamination is worse than that of metal salt and Wax without additives)

[0244] <Total light transmittance (1.0mm thickness)>

[0245] The pellets obtained by the above method were dried at 120°C for 5 hours, and then a test piece with a thickness of 1.0 mm was produced by an injection molding machine ("EC75" manufactured by Shibaura Machine Co., Ltd.) under the conditions of a barrel temperature of 280°C, a mold temperature of 80°C, a screw speed of 100 rpm, and an injection speed of 30 mm / s.

[0246] About the obtained test piece, the total light transmittance (unit: %) was measured using a haze meter.

[0247] As the haze meter, a model NDH-2000 manufactured by Nippon Denshoku Industries Co., Ltd. was used.

[0248] <Charpy impact strength (molding temperature 280℃, 1 minute cycle)>

[0249] The obtained pellets were dried at 120°C for 5 hours and then injection molded by an injection molding machine ("EC75" manufactured by Shibaura Machine Co., Ltd.) at a barrel temperature of 280°C, a mold temperature of 80°C, a screw speed of 80 rpm, and an injection speed of 30 mm / s (cycle time 1 minute) to produce ISO multi-purpose test pieces (3.0 mmt).

[0250] The obtained ISO multi-purpose test piece (3.0 mmt) was used to measure the notched Charpy impact strength (unit: kJ / m 2 ).

[0251] <Charpy impact strength (molding temperature 310℃, 7 minutes retention)>

[0252] The obtained pellets were dried at 120°C for 5 hours and then metered by an injection molding machine ("EC75" manufactured by Shibaura Machine Co., Ltd.) at a barrel temperature of 310°C, a mold temperature of 80°C, and a screw speed of 80 rpm. After being retained in the barrel for 7 minutes, injection molding was performed at an injection speed of 30 mm / s to produce ISO multi-purpose test pieces (3.0 mmt).

[0253] The obtained ISO multi-purpose test piece (3.0 mmt) was used to measure the notched Charpy impact strength (unit: kJ / m 2 ).

[0254] <Impact strength retention rate (%)>

[0255] The impact strength retention rate was calculated from the values ​​of the Charpy impact strength (molding temperature 310°C, 7-minute retention) and the Charpy impact strength (molding temperature 280°C, 1-minute cycle) as [Charpy impact strength (molding temperature 310°C, 7-minute retention) / Charpy impact strength (molding temperature 280°C, 1-minute cycle)] × 100 (unit: %).

[0256] [Table 2]

[0257]

[0258] [Table 3]

[0259]

[0260] [Table 4]

[0261]

[0262] [Table 5]

[0263]

[0264] [Table 6]

[0265]

[0266] In Tables 2 to 6 above, "(C-1) / (D)" represents the mass ratio of the acid-unmodified or slightly acid-modified polyolefin wax (C-1) / the aromatic sulfonic acid alkali metal salt (D).

[0267] From the above results, it is clear that the molded article obtained from the resin composition of the first embodiment can achieve desired light-shielding properties and is excellent in impact resistance, particularly, in retention of impact resistance during retention.

[0268] 3. Examples 2-1 to 2-11, Comparative Examples 2-1 to 2-10

[0269] Pellets of the resin composition were obtained in the same manner as in Example 1-1. Mold deposit, total light transmittance, Charpy impact strength (molding temperature 280°C, 1-minute cycle, molding temperature 310°C, 7-minute retention), and impact strength retention (%) were measured in the same manner as in Example 1-1. In addition, the equivalent circle mean diameter was measured for Examples 2-1 to 2-11, Comparative Examples 2-1 to 2-10, and Comparative Example 1-5.

[0270] <Equivalent circle average diameter>

[0271] After drying the obtained pellets at 120°C for 5 hours, they were injection molded by an injection molding machine ("EC75" manufactured by Shibaura Machine Co., Ltd.) at a barrel temperature of 280°C, a mold temperature of 80°C, a screw speed of 80 rpm, and an injection speed of 30 mm / s to produce an ISO multi-purpose test piece (3.0 mmt). The obtained test piece was ultrasonically cleaned with methanol for 5 minutes, and the surface of the central part of the dumbbell was observed using an operating electron microscope (SEM) S-4800 (manufactured by Hitachi High-Technologies) at an acceleration voltage of 3.0 kv, a current of 10 μA, and 3000 times. The obtained image was passed through a Gaussian 3×3 filter and automatically binarized to display 0.001 μm. 2 The area below is deleted as noise. Based on the area of ​​each titanium oxide scattered on the obtained image data, the particle size (diameter) equivalent to a circle is calculated using the following mathematical formula, and the average value is used as the equivalent circle diameter of the sample (unit: μm). If the equivalent circle diameter is less than 0.165 μm, the appearance can be considered good, and if it is less than 0.160 μm, the appearance can be considered even better.

[0272] [Formula 5]

[0273]

[0274] [Table 7]

[0275]

[0276] [Table 8]

[0277]

[0278] [Table 9]

[0279]

[0280] [Table 10]

[0281]

[0282] [Table 11]

[0283]

[0284] [Table 12]

[0285]

[0286] In the above Tables 7 to 12, "(C) / (D)" represents the mass ratio of the acid-modified polyolefin wax (C-2) / the aromatic sulfonic acid alkali metal salt (D).

[0287] The above results clearly show that the molded article obtained from the resin composition of the second embodiment can achieve desired light-shielding properties, has excellent appearance, and has excellent impact resistance, particularly excellent retention rate of impact resistance during retention.

Claims

1. A resin composition, wherein The resin composition comprises a polycarbonate resin (A), and 5.0 to 20.0 parts by mass of particles (B) containing titanium oxide as a main component, a polyolefin wax (C), and an aromatic sulfonic acid metal salt (D) based on 100 parts by mass of the polycarbonate resin (A). When the polyolefin wax (C) is a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, the content of the polyolefin wax (C-1) is 0.001 to 1.5 parts by mass, and the content of the aromatic sulfonic acid metal salt (D) is 0.01 to 1.5 parts by mass, When the polyolefin wax (C) is a polyolefin wax (C-2) having an acid value of 0.5 to 150 mgKOH / g, the content of the polyolefin wax (C-2) is 0.001 to 1.5 parts by mass, and the resin composition contains 0.2 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D).

2. The resin composition according to claim 1, wherein The resin composition comprises 5.0 to 20.0 parts by mass of particles (B) containing titanium oxide as a main component, 0.001 to 1.5 parts by mass of a polyolefin wax (C-1) having an acid value of less than 0.5 mgKOH / g, and 0.01 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D), based on 100 parts by mass of a polycarbonate resin (A).

3. The resin composition according to claim 2, wherein The mass ratio of the polyolefin wax (C-1) to the aromatic sulfonic acid alkali metal salt (D), (C-1) / (D), is 0.15 to 20.

4. The resin composition according to claim 1, wherein The resin composition comprises 5.0 to 20.0 parts by mass of particles (B) containing titanium oxide as a main component, 0.001 to 1.5 parts by mass of a polyolefin wax (C-2) having an acid value of 0.5 to 150 mgKOH / g, and 0.2 to 1.5 parts by mass of an aromatic sulfonic acid alkali metal salt (D), based on 100 parts by mass of a polycarbonate resin (A).

5. The resin composition according to claim 4, wherein The mass ratio of the polyolefin wax (C-2) to the aromatic sulfonic acid alkali metal salt (D), (C-2) / (D), is 0.15 to 10.

0.

6. The resin composition according to claim 4 or 5, wherein The molded product obtained by molding the resin composition with a barrel setting temperature of 280°C and a cycle time of 1 minute was observed using an operating electron microscope, and the equivalent circle diameter calculated using mathematical formula (1) based on the area of ​​the region where particles (B) with titanium oxide as the main component were dispersed was less than 0.165 μm.

7. The resin composition according to any one of claims 1 to 6, wherein The polyolefin wax (C) has a carboxyl group and / or anhydride group thereof.

8. The resin composition according to any one of claims 1 to 7, wherein The fluorination rate of the aromatic sulfonic acid alkali metal salt (D) is less than 1%.

9. The resin composition according to any one of claims 1 to 8, wherein The content of at least one filler selected from the group consisting of fibrous glass fillers, fibrous carbon fillers, and plate-shaped glass fillers is less than 1 part by mass based on 100 parts by mass of the polycarbonate resin. 10 . Pellets formed from the resin composition according to claim 1 . 11 . A molded article formed from the resin composition according to claim 1 .

12. A molded article formed from the pellets according to claim 10.