Oxidized bacterial cellulose / carboxymethyl chitosan sponge material as well as preparation method and application thereof

By using crosslinking technology of oxidized bacterial cellulose and carboxymethyl chitosan combined with 1,4-butanediol diglycidyl ether, oxidized bacterial cellulose/carboxymethyl group with high porosity and rapid water absorption and blood absorption effect, oxidized bacterial cellulose/carboxymethyl group with high porosity and rapid water absorption and blood absorption effect was prepared by crosslinking technology of oxidized bacterial cellulose and carboxymethyl chi Chitosan sponge material solves the shortcomings of existing hemostatic materials on incompressible wounds, and achieves efficient hemostatic and simple processes.

CN118987326APending Publication Date: 2024-11-22NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411066385.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing hemostatic materials have poor hemostatic effect on incompressible wounds, and the production process is complex, making it difficult to meet the traumatic needs of deep, narrow and irregular shapes.

Method used

Three-dimensional porous oxidized bacterial cellulose and carboxymethyl chitosan as raw materials, and frozen crosslinking is carried out to prepare three-dimensional porous oxidized bacterial cellulose/carboxymethyl chitosan as raw materials. Sugar sponge material, with good biocompatibility and rapid water absorption and blood absorption effect.

Benefits of technology

It achieves high porosity, rapid water absorption and blood absorption and shape memory, significantly improves the hemostatic effect, is suitable for the treatment of incompressible wounds, and the preparation process is simple and easy to perform.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118987326A_ABST
    Figure CN118987326A_ABST
Patent Text Reader

Abstract

The invention discloses an oxidized bacterial cellulose / carboxymethyl chitosan sponge material as well as a preparation method and application thereof. The method comprises the following steps: firstly mixing oxidized bacterial cellulose and carboxymethyl chitosan in water, then adding 1, 4-butanediol diglycidyl ether for freezing and crosslinking, and finally freeze-drying to obtain the oxidized bacterial cellulose / carboxymethyl chitosan sponge material. The oxidized bacterial cellulose / carboxymethyl chitosan sponge material disclosed by the invention has good porosity, relatively large water absorption rate, excellent biocompatibility, shape memory of rapid water absorption, blood absorption and resilience and a good hemostatic effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedical materials and relates to an oxidized bacterial cellulose / carboxymethyl chitosan sponge material and a preparation method and application thereof. Background Art

[0002] Chitosan (CS) has been widely studied as a hemostatic ingredient, but pure chitosan has a weak hemostatic effect and poor water solubility, making it an undesirable hemostatic material. Carboxymethyl chitosan (CMC) is a water-soluble derivative of chitosan. Compared with CS, CMC has better biocompatibility, biodegradability, moisture retention, viscosity and other properties. More importantly, the free amino groups on the CMC molecular chain can aggregate platelets and activate red blood cells. Oxidized bacterial cellulose (OBC) has good mechanical strength, can stimulate platelet aggregation through contact activation to promote coagulation, and can be degraded in situ.

[0003] 1,4-Butanediol diglycidyl ether (BDDE) is the crosslinker for most hyaluronic acid on the market. Its crosslinking ability is attributed to the reactivity of the epoxy groups at both ends of the molecule. Under alkaline conditions (pH>10), these epoxy groups preferentially react with primary alcohols to form ether bonds. Under acidic conditions (pH<4), these epoxy groups preferentially react with carboxylic acids to form ester bonds (Leach, J., et al. "Crosslinked α-elastin biomaterials: toward a processableelastin mimetic scaffold." Acta Biomaterialia 1 (2005): 155-164.).

[0004] Non-compressible hemostatic wounds face direct challenges of being deep, narrow, and irregular in shape. Emergency hemostatic materials such as gauze, hydrogel, and powder have good hemostatic effects on shallow surface trauma, but have huge disadvantages in dealing with non-compressible wounds caused by penetrating injuries. Compared with other types of hemostatic materials, hemostatic sponges have the advantages of being compressible, easy to pack, and staying at the bleeding site to form physical pressure. Therefore, it is of great significance to develop a sponge-type hemostatic material that can quickly stop bleeding in non-compressible wounds.

[0005] Literature 1 reports a coupling method to combine oxidized bacterial cellulose, CS and collagen. The material is used for hemostasis and has a good hemostatic effect, but the production process is complicated. (Yuan Haibin; Lin Chen; Hong Feng. Oxidized bacterial cellulose antibacterial composite sponge for rapid hemostasis and wound repair in vivo. ACS AMI 12(3):3382-3392, December 2019). Literature 2 proposes a water-triggered shape memory sodium carboxymethyl cellulose / sodium alginate / montmorillonite composite hemostatic sponge, which has a good porous structure, but its water absorption capacity needs to be improved (Liu Yeying; Yin Xiangfei; Hu Yinchun. Water-triggered shape memory cellulose / sodium alginate / montmorillonite composite sponge for rapid hemostasis. International Journal of Biomacromolecules 271(2):132679, June 2024). Summary of the invention

[0006] The purpose of the present invention is to provide an oxidized bacterial cellulose / carboxymethyl chitosan sponge material with rapid blood absorption and shape memory, and a preparation method and application thereof. The present invention mixes carboxymethyl chitosan and oxidized bacterial cellulose with good water solubility and hemostatic effect, and uses 1,4-butanediol diglycidyl ether as a cross-linking agent for ring-opening cross-linking to obtain a three-dimensional porous oxidized bacterial cellulose / carboxymethyl chitosan sponge material with good biocompatibility and hemostatic effect.

[0007] The technical solution for achieving the purpose of the present invention is as follows:

[0008] The preparation method of the oxidized bacterial cellulose / carboxymethyl chitosan three-dimensional sponge-like hemostatic material comprises the following steps:

[0009] (1) mixing oxidized bacterial cellulose and carboxymethyl chitosan in water at a mass ratio of oxidized bacterial cellulose to carboxymethyl chitosan of 4:1 to 1:4 to form a uniform solution;

[0010] (2) adding 1,4-butanediol diglycidyl ether to the solution obtained in step (1), stirring to form a uniform mixed solution, wherein the mass of 1,4-butanediol diglycidyl ether is 5% to 15% of the total mass of oxidized bacterial cellulose and carboxymethyl chitosan;

[0011] (3) freezing and cross-linking the mixed solution obtained in step (1);

[0012] (4) freeze-drying the cross-linked sample in step (3) to obtain an oxidized bacterial cellulose / carboxymethyl chitosan sponge material.

[0013] Preferably, in step (1), the oxidized bacterial cellulose is prepared by the following steps: after homogenizing the bacterial cellulose film, adding 2,2,6,6-tetramethylpiperidinyl oxide (TEMPO), sodium bromide and sodium hypochlorite solution to carry out oxidation reaction, and after the reaction is completed, dialyzing to obtain a uniformly dispersed oxidized bacterial cellulose solution with an oxidation degree of 15%.

[0014] Preferably, in step (1), the concentrations of oxidized bacterial cellulose and carboxymethyl chitosan are 10 mg / ml respectively.

[0015] Preferably, in step (2), the mass of 1,4-butanediol diglycidyl ether is 10% of the total mass of oxidized bacterial cellulose and carboxymethyl chitosan.

[0016] Preferably, in step (3), the freezing cross-linking temperature is -20°C and the freezing time is 12 to 24 hours.

[0017] The invention also provides an oxidized bacterial cellulose / carboxymethyl chitosan sponge material prepared by the preparation method.

[0018] Furthermore, the present invention provides the use of the above-mentioned oxidized bacterial cellulose / carboxymethyl chitosan sponge material as a hemostatic material.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] (1) The present invention uses oxidized bacterial cellulose and carboxymethyl chitosan as raw materials, both of which are good biomaterials, non-biotoxic, and have good biocompatibility. In addition, the preparation process of the present invention is simple and easy to operate.

[0021] (2) The present invention adjusts the pH of the cross-linking system so that cross-linking is achieved under neutral conditions rather than alkaline and acidic conditions. The sponge prepared under neutral cross-linking conditions has better formability and is more suitable for biomedical applications.

[0022] (3) The present invention adopts the form of freeze-crosslinking followed by freeze-drying to ensure complete crosslinking and the final sponge material has uniform pore size and good porosity.

[0023] (4) The cross-linking process of the present invention utilizes chemical cross-linking, and the material is tightly cross-linked and will not break or fall apart after repeated compression.

[0024] (5) The oxidized bacterial cellulose / carboxymethyl chitosan sponge material prepared by the present invention has high water absorption rate, high porosity of more than 90%, excellent biocompatibility, shape memory of rapid water and blood absorption and rebound, and good hemostatic effect. When used as a hemostatic material, the hemostatic effect is significantly better than that of the gauze group. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1The alkalized oxidized bacterial cellulose sponge material of Comparative Example 1 and the oxidized bacterial cellulose / chitosan sponge material of Comparative Example 4 are physical pictures;

[0026] Figure 2 The actual pictures of the oxidized bacterial cellulose / carboxymethyl chitosan sponge materials (OBC / CMC) of Examples 1 to 3, the neutral oxidized bacterial cellulose sponge material (OBC) of Comparative Example 2 and the carboxymethyl chitosan sponge material (CMC) of Comparative Example 3 before and after dry compression and wet compression, and after water-induced rebound, wherein OBC: neutral oxidized bacterial cellulose sponge material, 4:1: oxidized bacterial cellulose / carboxymethyl chitosan sponge material prepared when the mass ratio of oxidized bacterial cellulose to carboxymethyl chitosan is 4:1, 1:1: oxidized bacterial cellulose / carboxymethyl chitosan sponge material prepared when the mass ratio of oxidized bacterial cellulose to carboxymethyl chitosan is 1:1, 1:4: oxidized bacterial cellulose / carboxymethyl chitosan sponge material prepared when the mass ratio of oxidized bacterial cellulose to carboxymethyl chitosan is 1:4, CMC: carboxymethyl chitosan sponge.

[0027] Figure 3 The scanning electron microscope images of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2, and the CMC sponge material of Comparative Example 3;

[0028] Figure 4 These are infrared spectra of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2, and the CMC sponge material of Comparative Example 3.

[0029] Figure 5 The graphs are the porosity and water absorption of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2, and the CMC sponge material of Comparative Example 3.

[0030] Figure 6 The graphs are the porosity and water absorption of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2, and the CMC sponge material of Comparative Example 3.

[0031] Figure 7 The biocompatibility (a), cell proliferation test (b) and live-death test result (c) of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2 and the CMC sponge material of Comparative Example 3 of Example 3 are shown;

[0032] Figure 8 Graphs showing in vivo liver hemostasis time and bleeding volume of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2, and the CMC sponge material of Comparative Example 3. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with specific embodiments and drawings.

[0034] In the following examples, the oxidized bacterial cellulose used was prepared by referring to the existing method, and the specific steps were as follows: after homogenizing the bacterial cellulose membrane, TEMPO, sodium bromide and sodium hypochlorite solution were added to carry out oxidation reaction, and after the reaction was completed, the membrane was placed in a dialysis bag for dialysis to obtain a uniformly dispersed oxidized bacterial cellulose solution with a solid content of 1%.

[0035] Example 1

[0036] (1) mixing an oxidized bacterial cellulose solution and a carboxymethyl chitosan solution each having a solid content of 1% in a volume ratio of 4:1;

[0037] (2) adding 1,4-butanediol diglycidyl ether to the solution obtained in step (1), wherein the mass of 1,4-butanediol diglycidyl ether is 10% of the total mass of oxidized bacterial cellulose and carboxymethyl chitosan, and stirring at room temperature for 1 hour;

[0038] (3) placing the mixed liquid in a -20°C refrigerator for 12 h for freeze cross-linking;

[0039] (4) freeze-drying the cross-linked material to obtain an oxidized bacterial cellulose / carboxymethyl chitosan sponge material.

[0040] Example 2

[0041] This embodiment is basically the same as the embodiment 1, except that the volume ratio of the oxidized bacterial cellulose solution with a solid content of 1% and the carboxymethyl chitosan solution is 1:1.

[0042] Example 3

[0043] This embodiment is basically the same as the embodiment 1, except that the volume ratio of the oxidized bacterial cellulose solution with a solid content of 1% and the carboxymethyl chitosan solution is 1:4.

[0044] Comparative Example 1

[0045] (1) The pH of the oxidized bacterial cellulose solution was adjusted to 10 with a 2M NaOH solution and alkalized for 30 min;

[0046] (2) adding 1,4-butanediol diglycidyl ether to the alkalized oxidized bacterial cellulose solution, wherein the mass of 1,4-butanediol diglycidyl ether is 10% of the mass of the oxidized bacterial cellulose, and stirring at room temperature for 1 hour;

[0047] (3) placing the mixed liquid in a -20°C refrigerator for 12 h for freeze cross-linking;

[0048] (4) freeze-drying the cross-linked material to obtain an alkaline oxidized bacterial cellulose sponge material.

[0049] Comparative Example 2

[0050] (1) adding 1,4-butanediol diglycidyl ether to the oxidized bacterial cellulose solution, wherein the mass of 1,4-butanediol diglycidyl ether is 10% of the mass of the oxidized bacterial cellulose, and stirring at room temperature for 1 hour;

[0051] (2) placing the mixed liquid in a -20°C refrigerator for 12 hours to perform freeze crosslinking;

[0052] (3) freeze-drying the cross-linked material to obtain a neutral oxidized bacterial cellulose sponge material.

[0053] Comparative Example 3

[0054] (1) Dissolve 1 g of carboxymethyl chitosan in 100 ml of deionized water to form a uniform solution;

[0055] (2) adding 1,4-butanediol diglycidyl ether to the carboxymethyl chitosan solution, wherein the mass of 1,4-butanediol diglycidyl ether is 10% of the mass of the carboxymethyl chitosan, and stirring at room temperature for 1 hour;

[0056] (3) placing the mixed liquid in a -20°C refrigerator for 12 h for freeze cross-linking;

[0057] (4) freeze-drying the cross-linked material to obtain a carboxymethyl chitosan sponge material.

[0058] Comparative Example 4

[0059] (1) The pH of the oxidized bacterial cellulose solution was adjusted to 12 with a 2M NaOH solution and alkalized for 30 min;

[0060] (2) first preparing a 2% (v / v) acetic acid solution, and then adding chitosan to prepare a chitosan solution with a solid content of 1%;

[0061] (3) mixing the alkalized oxidized bacterial cellulose solution and the chitosan solution in a volume ratio of 1:1, adjusting the pH of the entire solution to 10, and rapidly stirring until the precipitated chitosan is dispersed;

[0062] (4) adding 1,4-butanediol diglycidyl ether to the mixed solution, wherein the mass of 1,4-butanediol diglycidyl ether is 10% of the total mass of oxidized bacterial cellulose and chitosan, and stirring at room temperature for 1 hour;

[0063] (5) Place the mixed liquid in a -20°C refrigerator for 12 hours to perform freeze crosslinking;

[0064] (6) The cross-linked material is freeze-dried to obtain an oxidized bacterial cellulose / chitosan sponge material (OBC1 / CS1 alkaline).

[0065] Figure 1 The alkalized oxidized bacterial cellulose sponge material of Comparative Example 1 and the oxidized bacterial cellulose / chitosan sponge material of Comparative Example 4 show that in Comparative Example 1, the oxidized bacterial cellulose with an oxidation degree of 15% was not successfully cross-linked under alkaline conditions. In Comparative Example 2, the sponge obtained by cross-linking oxidized bacterial cellulose and chitosan under alkaline conditions had a low degree of cross-linking and could not return to its original shape after being compressed and absorbing water.

[0066] Figure 2 The actual pictures of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2 and the CMC sponge material of Comparative Example 3 before and after dry compression and wet compression and after water-induced rebound. It can be seen from the figures that each material has been successfully cross-linked without any loosening phenomenon, and has good resilience after water absorption.

[0067] Figure 3 The SEM images of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2, and the CMC sponge material of Comparative Example 3 show that the materials have a rich lamellar porous structure inside. The rich porous structure is conducive to the full contact between the OBC / CMC material and the blood and promotes the coagulation cascade.

[0068] Figure 4 The mechanical properties of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge materials of Comparative Example 2, and the CMC sponge materials of Comparative Example 3 are shown in the figure. Each material is soaked and subjected to 10 cycles of compression with a deformation of 95%. It can be seen from the figure that the CMC material is softer than the OBC material and is easy to collapse after being compressed. The OBC / CMC sponge materials, due to the high mechanical strength of oxidized bacterial cellulose, show excellent resilience and can recover their original shape after being compressed without falling apart.

[0069] Figure 5 The FT-IR graphs of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2, and the CMC sponge material of Comparative Example 3 are shown in Figure 1, where OBC represents oxidized bacterial cellulose, C-OBC represents cross-linked oxidized bacterial cellulose, and other materials are named using the same rules. -1 The broad peak at 2900 cm corresponds to the -OH stretching vibration band, -NH2 stretching vibration band (amide II) and CO-NH stretching vibration band. -1 The weak absorption peak at 1600cm in the material spectrum is related to the -OH stretching vibration and CH stretching vibration of CMC. -1 The 1050 cm-1 corresponds to the -NH2 angular vibration band and the CO-OH stretching vibration band. The C=O stretching vibration band of amide (amide I) overlaps with them and is difficult to distinguish in ordinary light.-1 The absorption peaks at 1735cm-1 correspond to the CO and CC stretching vibration peaks. The absorption peak at 1735cm-1 is the C=O stretching vibration peak of the ester, indicating that the epoxy ring can be opened and reacted with the carboxyl group under neutral conditions, and there is no need to stimulate its ring opening under alkaline or acidic conditions.

[0070] Figure 6 The porosity and water absorption rate of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2, and the CMC sponge material of Comparative Example 3 are shown in Figure 1. The porosity is measured by the ethanol saturation method. First, the width and thickness of the sponge are measured to obtain its volume V. Then, the dry sponge is weighed as m0. Then, the dry sponge is soaked in anhydrous ethanol and vacuumed for 5 minutes to obtain the wet sponge m1. The calculation formula is: OBC / CMC sponge materials both have high water absorption and high porosity of more than 90%, which is conducive to rapid hemostasis and can promote coagulation by concentrating blood and activating intrinsic pathways in the body.

[0071] Figure 7 The biocompatibility (a) of the OBC / CMC sponge material of Examples 1 to 3, the OBC sponge material of Comparative Example 2, and the CMC sponge material of Comparative Example 3, the cell proliferation test (b), and the live-death test result (c) are shown. The sample was soaked in 75% ethanol for 30 minutes, sterilized and irradiated with ultraviolet light for 30 minutes, and then washed 3 times with PBS solution. The sterilized sample was placed in an immersion fluid prepared with pure DMEM, incubated at 37°C for 2 hours, filtered, and added with 10% FBS and 1% P / S to prepare a complete culture medium of 5 mg / mL. HL-1 cells were inoculated in a 96-well plate (1500 cells / well) and cultured. After cell adhesion, it was changed into the sample extract and cultured for 1, 3, 5, and 7 days respectively. The cell compatibility of the sponge material was detected by the CCK-8 method. 10 μL CCK-8 reagent was added to each well of 100 μL basal culture medium, incubated at 37°C for 2 hours, and the absorbance at 450nm was measured by an enzyme marker. The cell proliferation rate (CPR) was calculated as follows: In the formula, As and Ac are the absorbance values ​​of the sample group and the control group, respectively. In addition, live-dead staining was used to further detect cytotoxicity, in which AML-12 cells were measured at 1×10 4 The density of cells / well was implanted into a 24-well plate. The culture medium was the immersion fluid of each sample. After incubation at 37°C for 3 days, the cells were stained with live and dead dyes and observed under a fluorescence microscope. The results showed that OBC / CMC sponge materials were non-toxic to cells and had good biocompatibility.

[0072] Figure 8The graphs are the hemostasis time and bleeding volume of the liver in vivo of the OBC / CMC sponge materials of Examples 1 to 3, the OBC sponge material of Comparative Example 2, and the CMC sponge material of Comparative Example 3. The mice were anesthetized for 3 min with 3% (w / v) sodium pentobarbital (intraperitoneal injection, 30 mg / kg). After successful anesthesia, the mice were placed in a supine position and fixed on an operating table. The mouse skin and endothelium were cut open along the midline of the abdomen to expose the liver, and a perforator with a diameter of 2 mm was used to puncture the lower lobe of the liver. Then a prepared sponge was pressed into the wound. The hemostasis time and hemostasis volume were recorded. At the same time, a blank group without any treatment and a control group using gauze bandage for hemostasis were set up. It can be clearly seen from the figure that the hemostasis time and bleeding volume of the OBC / CMC sponge material are lower than those of the gauze, proving that the OBC / CMC sponge material has a good hemostatic effect.

Claims

1. A method for preparing a three-dimensional sponge-like hemostatic material of oxidized bacterial cellulose / carboxymethyl chitosan, characterized in that: The following steps are involved: (1) mixing oxidized bacterial cellulose and carboxymethyl chitosan in water at a mass ratio of 4:1 to 1:4 to form a uniform solution; (2) adding 1,4-butanediol diglycidyl ether to the solution obtained in step (1), stirring to form a uniform mixed solution, wherein the mass of 1,4-butanediol diglycidyl ether is 5% to 15% of the total mass of oxidized bacterial cellulose and carboxymethyl chitosan; (3) freezing and cross-linking the mixed solution obtained in step (1); (4) freeze-drying the cross-linked sample in step (3) to obtain an oxidized bacterial cellulose / carboxymethyl chitosan sponge material.

2. The preparation method according to claim 1, characterized in that: In step (1), the oxidized bacterial cellulose is prepared by the following steps: after homogenizing the bacterial cellulose film, TEMPO, sodium bromide and sodium hypochlorite solution are added to carry out oxidation reaction, and after the reaction is completed, dialyze to obtain a uniformly dispersed oxidized bacterial cellulose solution with an oxidation degree of 15%.

3. The preparation method according to claim 1, characterized in that: In step (1), the concentrations of oxidized bacterial cellulose and carboxymethyl chitosan are 10 mg / ml, respectively.

4. The preparation method according to claim 1, characterized in that: In step (2), the mass of 1,4-butanediol diglycidyl ether is 10% of the total mass of oxidized bacterial cellulose and carboxymethyl chitosan.

5. The preparation method according to claim 1, characterized in that: In step (3), the freezing cross-linking temperature is -20°C and the freezing time is 12 to 24 hours.

6. The oxidized bacterial cellulose / carboxymethyl chitosan sponge material obtained according to the preparation method described in any one of claims 1 to 5.

7. Use of the oxidized bacterial cellulose / carboxymethyl chitosan sponge material according to claim 6 as a hemostatic material.