HSP70-targeted photo-thermal anti-tumor artificial bone and preparation method thereof
Through selective laser sintering technology of Ver155008, MoS2, MBG, and PLLA composites, the photothermal anti-tumor artificial bone targeting HSP70 is prepared to block the HSP70-mediated thermal resistance effect, and solve the problem of photothermal material in treating tumor bone defects. The thermal tolerance problem has significantly improved the anti-tumor performance and is suitable for filling treatment of bone defects after bone tumor surgery.
Patent Information
- Application Number
- CN202411206415.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
When using existing photothermal materials to treat tumor bone defects, artificial bones face the adverse situation of bone tumor cells to produce thermal tolerance/resistance. No research has been found to optimize the anti-tumor performance of photothermal artificial bones from the molecular level. Report.
Using the four components of Ver155008, MoS2, MBG and PLLA, the targeted photothermal anti-tumor artificial bone was prepared by selective laser sintering. Ver155008 acts as an HSP70 inhibitor to block the HSP70-mediated thermal resistance effect and enhance photothermal Anti-tumor properties of the material.
The artificial bone prepared has high mechanical strength, biocompatibility and stable drug release ability, which significantly improves the anti-tumor performance of photothermal materials. It is suitable for the treatment of bone tumor cells that are prone to heat tolerance/resistance, and meets clinical needs. .
Smart Images

Figure CN118987343A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biomedical materials and relates to an artificial bone for treating tumor bone defects and a preparation method thereof. Background Art
[0002] Tumor bone defects are bone defects caused by surgery for benign and malignant bone tumors and other diseases, and face the huge challenge of local tumor recurrence. Tumor artificial bone is an important choice. Among them, photothermal material artificial bone is an important type of anti-tumor artificial bone. It kills tumor cells by using the difference in temperature tolerance between tumor cells and normal cells. Photothermal killing of tumor cells has no significant effect on normal cells. Mesoporous bioglass (MBG) has good biological activity to promote bone regeneration, and it is rich in pores of 2~50nm that can absorb small molecule drugs. Molybdenum disulfide (MoS2) is a photothermal material with low toxicity and high efficiency of photothermal conversion performance that can be excited by near-infrared light. Poly-L-lactic acid (PLLA) uses organic polymers with good biocompatibility and is suitable as a matrix material for laser printing. Ver155008 is an effective HSP70 family inhibitor that inhibits HSP70-mediated thermal resistance and can enhance the anti-tumor ability of photothermal stents. The above materials are combined to prepare composite artificial bones to achieve complementary advantages. They can not only repair bone defects, but also use the photothermal effect to kill local residual tumor cells in bone defects more efficiently than conventional photothermal materials. They can be used for the repair of clinical tumor bone defects.
[0003] Chinese patent CN116355090A discloses a "nanoantibody targeting HSP70 and its preparation method and application". This patent also targets HSP70, which is an antibody, but does not involve anti-tumor artificial bone and its preparation technology.
[0004] Chinese patent CN112546299B discloses "a 3D printed artificial periosteum, artificial bone, artificial skeleton and its preparation method". The preparation method and composition of its artificial bone are of certain significance, but are not used for anti-tumor.
[0005] Photothermal anti-tumor artificial bone for repairing tumor bone defects faces the unfavorable situation of bone tumor cells developing thermal tolerance / resistance. So far, there has been no research report on optimizing the anti-tumor performance of photothermal artificial bone by blocking the thermal resistance mechanism at the molecular level. Summary of the invention
[0006] The present invention aims to provide an artificial bone for treating tumor bone defects and a preparation method thereof, to overcome the deficiencies of the above-mentioned prior art, and to provide a photothermal material artificial bone that can block the thermal tolerance / resistance intracellular molecular signal axis of bone tumor cells. The artificial bone has high strength, mechanical properties close to human bone, good osteoconductivity, biocompatibility, bone repair, anti-tumor effects and stable drug release capacity, and is suitable for filling and treating bone defects after various bone tumor surgeries, and is particularly suitable for bone tumor cells that are prone to thermal tolerance / resistance.
[0007] In order to achieve the above object, the technical solution provided by the present invention is: A photothermal anti-tumor artificial bone targeting HSP70, the artificial bone is composed of Ver155008, MoS2, MBG, and PLLA in a mass ratio of (0.1~1): (0.5~1.5): (5~10): 100; the mesoporous bioglass MBG is reacted with aminopropyltriethoxysilane APTES in toluene to achieve the amino modification of the pore wall of MBG; Ver155008@MBG-NH2 nanoparticles are obtained by ultrasonically dispersing HSP70 blocker Ver155008 and MBG-NH2, self-assembling and freeze-drying in sequence, wherein MBG is mainly combined with Ver155008 by physical adsorption and amide covalent bonds, the particle diameter is between 100~1000nm, and the mass ratio of Ver155008 to MBG-NH2 is (0.08~0.12): 1.
[0008] Furthermore, the optimal component mass ratio of Ver155008 and MBG-NH2 (0.09~0.11):1.
[0009] Furthermore, the particle size of Ver155008@MBG is 100~300nm, the Zeta potential is positive, the aqueous solution is colloid, and the pH value of the solution is between 7.0~7.7; the particle size of the MBG powder is less than 300nm; and the Ver155008 is of biopharmaceutical grade.
[0010] Furthermore, in the construction of Ver155008@MBG nanoparticles, the PLLA powder is smaller than 200 mesh, the MoS2 particle size is 50-300 nm; and the pore size of the mesoporous bioglass is 2-50 nm.
[0011] The above method for preparing HSP70-targeted photothermal anti-tumor artificial bone comprises the following steps: (1) Mixing: After physically mixing 0.11-0.22 g of the Ver155008@MBG nanoparticles prepared in claim 1 with 0.1-0.15 g of molybdenum disulfide powder and 2 g of PLLA powder, the mixture is added into 100 ml of ultrapure water and stirred evenly using a constant temperature magnetic stirrer for 30-60 min at a temperature of 30-37°C; the mass percentage content of MoS2 in the suspension is 0.5%-1.5%, the mass percentage content of MBG is 5%-10%, and the mass percentage content of Ver155008 is 0.1%-1%; (2) Filtration and freeze drying: The suspension obtained in step (1) is injected into a filter to obtain a precipitate, which is then placed in a cold trap of a vacuum freeze dryer and pre-frozen at -20°C for 1 to 2 hours. The cold trap gas is then pumped to a vacuum, and finally freeze-dried for 12 to 24 hours. (3) Laser sintering: The freeze-dried samples are collected and packaged. According to the preset cross-sectional shape of the artificial bone, the first layer of mixed powder laid on the laser sintering template is selectively scanned and sintered. After one layer is sintered, the next layer of powder is laid and scanned and sintered again. The latter layer and the previous layer are sintered together, and the cycle is repeated. The laser sintering conditions set during laser sintering are marking speed 100~400mm / s, laser power 2~3W, laser frequency 2~10kHz, and duty cycle 1.5~2.5, and artificial bone for repairing bone defects after bone tumor surgery is obtained.
[0012] Furthermore, in step (2) of filtering and freeze drying, the freeze drying conditions set during freeze drying are temperature -20°C, power 850W, vacuum degree <10Pa, and water replenishment capacity 4kg / 24h.
[0013] Principle of the invention: In order to solve the problem of difficulty in repairing tumor-induced bone defects, the present invention compounds four components, Ver155008, MoS2, MBG and PLLA, and prepares artificial bones by selective laser sintering. The artificial bones have good mechanical strength, good biological activity and uniform drug distribution. The drugs are gradually released as the matrix material degrades, thus avoiding the sudden drug release caused by the coating method. HSP70 is a key molecule that induces the thermal resistance effect of bone tumor cells during the tumor killing process of photothermal materials. HSP70 can mediate the expression of a series of signal molecules in bone tumor cells, leading to thermal tolerance / resistance. Ver155008 is an HSP70 inhibitor with high biological targeting. The photothermal artificial bones loaded with Ver155008 will block the thermal resistance effect mediated by HSP70, thereby indicating the anti-tumor activity of the photothermal scaffold.
[0014] Compared with the prior art, the present invention proposes for the first time to use the compound Ver155008 to enhance the anti-tumor efficacy of artificial bone made of photothermal materials; the present invention uses Ver155008 as the main synergistic component of artificial bone to further enhance the anti-tumor performance of existing photothermal materials, mainly by blocking the thermal tolerance / resistance molecular signaling pathway mediated by HSP70. The beneficial effects of the present invention are: 1) The photothermal effect of the artificial bone prepared by the present invention has anti-tumor function, but the effective ingredient Ver155008 can block the HSP70-mediated thermal tolerance / resistance effect generated during the photothermal anti-tumor process of the existing photothermal material artificial bone (such as MoS2 composite artificial bone), further enhancing the anti-tumor performance of the photothermal material artificial bone; 2) The bone repair material prepared by the present invention is most suitable for filling treatment of tumor bone defects, the preparation method is simple, the biomechanical properties are close to normal bones, the degradation rate is basically matched with the bone repair rate, the drug is stably released, it meets the needs of clinical use, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a schematic diagram of the preparation of HSP70-targeted photothermal anti-tumor artificial bone and the blocking of the heat resistance signal axis. MoS2 nanoparticles activated the SLC7A11 / GSH / GPX4 signal axis under NIR irradiation, which can promote ferroptosis of osteosarcoma cells. At the same time, the thermal effect of the MoS2 composite bone scaffold caused the increase of HSP70 expression in osteosarcoma cells. HSP70 activated downstream AKT, which entered the cell nucleus from the cytoplasm to enhance the activity of GPX4 transcription factor, and finally promoted the upregulation of GPX4 expression, inhibited the ferroptosis effect of tumor cells, and produced heat resistance. The HSP70 blocker Ver155008 can reverse this phenomenon.
[0016] Figure 2 This is an in vitro NIR irradiation image. Live and dead cell staining was used in an in vitro experiment to evaluate the tumor inhibition effect of the HSP70-targeted photothermal anti-tumor artificial bone Ver155008@MBG / MoS2 / PLLA (V@M / M / P) under NIR irradiation. The experimental results showed that the tumor inhibition effect of the V@M / M / P + NIR group was higher than that of the control group (M / M / P + NIR). DETAILED DESCRIPTION Example 1
[0017] A method for preparing HSP70-targeted photothermal anti-tumor artificial bone, wherein the chemical components of the artificial bone are MoS2=1.29%, MBG=8.58%, Ver155008=4.29%, and PLLA=85.84% by weight; the preparation method comprises the following steps (1) Mixing: First, react an appropriate amount of mesoporous bioglass MBG with 2.5 mmol aminopropyltriethoxysilane APTES in toluene to chemically modify the pore wall of MBG. Take 0.1g of HSP70 blocker Ver155008 powder and 0.2g of MBG-NH2 and mix them physically. Add deionized water for ultrasonic stirring and mix well. Freeze-dry to obtain Ver155008@MBG nanoparticles. After 0.3g of the prepared Ver155008@MBG nanoparticles is physically mixed with 0.03g of molybdenum disulfide (MoS2) powder and 2g of PLLA powder, add them to 100ml of ultrapure water and stir evenly with a constant temperature magnetic stirrer. The stirring time is 30~60min and the temperature is 30~37℃. (2) Filtration and freeze drying: The suspension obtained by mixing in step (1) is injected into a filter to obtain a precipitate, which is placed in a cold trap of a vacuum freeze dryer and pre-frozen at -20°C for 1-2 hours. The cold trap gas is then pumped to a vacuum, and finally freeze-dried for 12 hours to 24 hours. (3) Selective laser sintering: The freeze-dried samples are collected and packaged. According to the preset cross-sectional shape of the artificial bone, the first layer of mixed powder laid on the laser sintering template is selectively scanned and sintered. After one layer is sintered, the next layer of powder is laid and scanned and sintered again. The latter layer and the previous layer are sintered together, and the cycle is repeated. The laser sintering conditions set during laser sintering are marking speed 100~400mm / s, laser power 2~3W, laser frequency 2~10kHz, and duty cycle 1.5~2.5, thus obtaining artificial bone for repairing bone defects after bone tumor surgery.
[0018] Performance evaluation: mainly evaluate the physical and chemical characteristics, mechanical properties, biological toxicity and anti-tumor properties of artificial bones: 1) Physical and chemical characterization: X-ray diffraction (XRD), Fourier transform infrared spectroscopy (FTIR) and other phase detection methods can detect the presence of specific peaks of the bone scaffold, indicating that the scaffold is composed of Ver155008, MBG, MoS2, and PLLA; 2) Mechanical properties and cytotoxicity: The elastic modulus of the composite bone scaffold was measured to be 2 GPa by the compression test, and the CCK-8 cytotoxicity test showed that the scaffold had no significant effect on the cell viability of bone marrow mesenchymal stem cells compared with the cell group not inoculated into the scaffold (p>0.05); 3) Anti-tumor performance: The bone tumor cell death rate was 90.28% (p < 0.05) counted by live and dead cell staining, which was significantly higher than that in the blank group (p < 0.05).
[0019] Example 2 The preparation method of HSP70-targeted photothermal anti-tumor artificial bone has a chemical composition mass percentage of: 0.89% by mass of MoS2, 8.92% by mass of MBG, 0.89% by mass of Ver155008, and 89.3% by mass of PLLA; the preparation method comprises the following steps (1) Mixing: First, react an appropriate amount of mesoporous bioglass (MBG) with 2.5 mmol aminopropyltriethoxysilane APTES in toluene to chemically modify the pore wall of MBG. Take 0.02g of HSP70 blocker Ver155008 powder and 0.2g of MBG-NH2 and mix them physically. Add deionized water for ultrasonic stirring and mix well. Freeze-dry to obtain Ver155008@MBG nanoparticles. After 0.22g of the prepared Ver155008@MBG nanoparticles are physically mixed with 0.02g of molybdenum disulfide MoS2 powder and 2g of PLLA powder, add them to 100ml of ultrapure water and stir evenly with a constant temperature magnetic stirrer. The stirring time is 30-60min and the temperature is 30~37℃. (2) Filtration and freeze drying: The suspension obtained by mixing in step (1) is injected into a filter to obtain a precipitate, which is placed in a cold trap of a vacuum freeze dryer and pre-frozen at -20°C for 1 to 2 hours. The cold trap gas is then pumped to a vacuum, and finally freeze-dried for 12 to 24 hours. (3) Laser sintering: The freeze-dried samples are collected and packaged. According to the preset cross-sectional shape of the artificial bone, the first layer of mixed powder laid on the laser sintering template is selectively scanned and sintered. After one layer is sintered, the next layer of powder is laid and scanned and sintered again. The latter layer and the previous layer are sintered together, and the cycle is repeated. The laser sintering conditions set during laser sintering are marking speed 100~400mm / s, laser power 2~3W, laser frequency 2~10kHz, and duty cycle 1.5~2.5, and artificial bone for repairing bone defects after bone tumor surgery is obtained.
[0020] Performance evaluation: mainly evaluate the physical and chemical characteristics, mechanical properties, biological toxicity and anti-tumor properties of artificial bones: 1) Phase structure: X-ray diffraction (XRD), Fourier transform infrared spectroscopy (FTIR) and other phase detection and analysis can detect the presence of specific peaks in the bone scaffold, indicating that the scaffold is composed of Ver155008, MBG, MoS2 and PLLA; 2) Mechanical properties and cytotoxicity: The elastic modulus of the composite bone scaffold was measured to be 2 GPa by the compression test, and the CCK-8 cytotoxicity test showed that the scaffold had no significant effect on the cell viability of bone marrow mesenchymal stem cells compared with the cell group not inoculated into the scaffold (p>0.05); 3) Anti-tumor performance: The bone tumor cell death rate was 90.28% (p < 0.05) counted by live and dead cell staining, which was significantly higher than that in the blank group (p < 0.05).
[0021] Comparative Example: The preparation method of HSP70-targeted photothermal anti-tumor artificial bone, the chemical composition mass percentage is: the mass percentage of MoS2 is 0.89%, the mass percentage of MBG is 9%, the mass percentage of Ver155008 is 0.9%, and the mass percentage of PLLA is 90.1%; preparation method: (1) Mixing: First, react an appropriate amount of mesoporous bioglass (MBG) with 2.5 mmol aminopropyltriethoxysilane APTES in toluene to chemically modify the pore wall of MBG and dry it. Take an appropriate amount of aminated MBG nanoparticles 0.2g and physically mix them with molybdenum disulfide MoS2 powder (0.02g) and PLLA powder 2g, add them to 100ml ultrapure water, and stir them evenly using a constant temperature magnetic stirrer for 30-60min at a temperature of 30-37℃; (2) Filtration and freeze drying: The suspension obtained in step (1) is injected into a filter to obtain a precipitate, which is placed in a cold trap of a vacuum freeze dryer and pre-frozen at -20°C for 1-2 hours, followed by vacuuming the cold trap gas, and finally freeze drying for 12 hours to 24 hours; (3) Laser sintering: The freeze-dried samples are collected and packaged. According to the preset cross-sectional shape of the artificial bone, the first layer of mixed powder laid on the laser sintering template is selectively scanned and sintered. After one layer is sintered, the next layer of powder is laid and scanned and sintered again. The latter layer and the previous layer are sintered together, and the cycle is repeated. The laser sintering conditions set during laser sintering are marking speed 100~400mm / s, laser power 2~3W, laser frequency 2~10kHz, and duty cycle 1.5-2.5, and artificial bone for repairing bone defects after bone tumor surgery is obtained.
[0022] Performance evaluation: mainly evaluate the physical and chemical characteristics, mechanical properties, biological toxicity and anti-tumor properties of artificial bones: 1) Physical and chemical characterization: X-ray diffraction (XRD), Fourier transform infrared spectroscopy (FTIR) and other phase detection and analysis can detect the presence of specific peaks of the bone scaffold, indicating that the scaffold is composed of MBG, MoS2 and PLLA; 2) Mechanical properties and cytotoxicity: The elastic modulus of the composite bone scaffold was measured to be 2 GPa by the compression test. The CCK-8 cytotoxicity test showed that the scaffold had no significant effect on the cell viability of bone marrow mesenchymal stem cells compared with the cell group not inoculated into the scaffold (p>0.05). 3) Anti-tumor performance: The bone tumor cell mortality rate was approximately 70.34% (p < 0.05) counted by live and dead cell staining, and the tumor cell mortality rate effect experimental group (p < 0.05), indicating that the addition of Ver155008 improved the anti-tumor performance of photothermal material artificial bone.
[0023] The comparative example did not add the HSP70 blocker Ver155008 and can be used as the control group. The process parameters reduced the step of loading MBG nanoparticles with Ver155008. Because the example was loaded with Ver155008, releasing it into the bone defect microenvironment could block the photothermal resistance phenomenon. Therefore, the anti-tumor performance of the example was more outstanding than that of the comparative example.
[0024] The experimental data of the experimental group and the control group are compared in Table 1. As shown in Table 1: The experimental group (MoS2 / MBG / PLLA scaffold + NIR irradiation for 10 min) and the control group (MoS2 / MBG / PLLA scaffold) were co-cultured with osteosarcoma Sao2 cell line, and 3vs 3 RNA-Seq analysis was performed. The differentially expressed genes in osteosarcoma cells were screened with log2Fold change>2 and FDR<0.05 as the standard, among which HSP6A (HSP70) had the most significant difference.
[0025] Table 1 Comparison of experimental data between the experimental group and the control group
[0026] The molecular mechanism of heat resistance produced by NIR irradiation in the experimental group and the control group is shown in Figure 2 Under NIR irradiation, MoS2 nanoparticles activated the SLC7A11 / GSH / GPX4 signaling axis to promote ferroptosis of osteosarcoma cells. At the same time, the thermal effect of the MoS2 composite bone scaffold caused the increase of HSP70 expression in osteosarcoma cells. HSP70 activated downstream AKT, which entered the cell nucleus from the cytoplasm to enhance the activity of GPX4 transcription factor, and finally promoted the upregulation of GPX4 expression, inhibited the ferroptosis effect of tumor cells, and produced heat resistance. The HSP70 blocker Ver155008 can reverse this phenomenon.
Claims
1. A photothermal anti-tumor artificial bone targeting HSP70, characterized by: The artificial bone is composed of Ver155008, MoS2, MBG, and PLLA in a mass ratio of (0.1~1): (0.5~1.5): (5~10): 100; the mesoporous bioglass MBG is reacted with aminopropyltriethoxysilane APTES in toluene to achieve the amino modification of the pore wall of MBG; Ver155008@MBG-NH2 nanoparticles are obtained by ultrasonic dispersion, self-assembly and freeze-drying of HSP70 blocker Ver155008 and MBG-NH2 in sequence, in which MBG is mainly bound to Ver155008 through physical adsorption and amide covalent bonds, and the particle diameter is between 100~1000nm. The mass ratio of Ver155008 to MBG-NH2 is (0.08~0.12):
1.
2. The HSP70 targeted photothermal anti-tumor artificial bone according to claim 1, characterized in that: The mass ratio of Ver155008 and MBG-NH2 components is (0.09~0.11):
1.
3. The HSP70 targeted photothermal anti-tumor artificial bone according to claim 1, characterized in that: The particle size of Ver155008@MBG is 100-300nm, the Zeta potential is positive, the aqueous solution is colloid, and the pH value of the solution is between 7.0 and 7.7; the particle size of the MBG powder is less than 300nm; and the Ver155008 is of biopharmaceutical grade.
4. The HSP70 targeted photothermal anti-tumor artificial bone according to claim 1, characterized in that: The Ver155008@MBG nanoparticles are constructed with PLLA powder smaller than 200 mesh, MoS2 particle size of 50-300 nm, and mesoporous bioglass pore size of 2-50 nm.
5. The method for preparing a HSP70-targeted photothermal anti-tumor artificial bone according to claims 1 to 3, characterized in that The steps include: (1) Mixing: After physically mixing 0.11-0.22 g of the Ver155008@MBG nanoparticles prepared in claim 1 with 0.1-0.15 g of molybdenum disulfide powder and 2 g of PLLA powder, the mixture is added into 100 ml of ultrapure water and stirred evenly using a constant temperature magnetic stirrer for 30-60 min at a temperature of 30-37°C; the mass percentage content of MoS2 in the suspension is 0.5%-1.5%, the mass percentage content of MBG is 5%-10%, and the mass percentage content of Ver155008 is 0.1%-1%; (2) Filtration and freeze drying: The suspension obtained in step (1) is injected into a filter to obtain a precipitate, which is then placed in a cold trap of a vacuum freeze dryer and pre-frozen at -20°C for 1 to 2 hours. The cold trap gas is then pumped to a vacuum, and finally freeze-dried for 12 to 24 hours. (3) Laser sintering: The freeze-dried samples are collected and packaged. According to the preset cross-sectional shape of the artificial bone, the first layer of mixed powder laid on the laser sintering template is selectively scanned and sintered. After one layer is sintered, the next layer of powder is laid and scanned and sintered again. The latter layer and the previous layer are sintered together, and the cycle is repeated. The laser sintering conditions set during laser sintering are marking speed 100~400mm / s, laser power 2~3W, laser frequency 2~10kHz, and duty cycle 1.5~2.5, and artificial bone for repairing bone defects after bone tumor surgery is obtained.
6. The method for preparing a HSP70-targeted photothermal anti-tumor artificial bone according to claim 5, characterized in that: In step (2) of filtering and freeze drying, the freeze drying conditions set during freeze drying are temperature -20°C, power 850W, vacuum degree <10Pa, and water replenishment capacity 4kg / 24h.