MXene modified liquid evaporator as well as preparation method and application thereof
Through the 3D liquid evaporator modified by MXene-Ti4O7 composite material, the fabric matrix and rotary design are used to solve the problems of the existing liquid evaporator in terms of evaporation rate, efficiency and stability, and achieve efficient water evaporation and salt resistance. Suitable for seawater desalination and wastewater treatment.
Patent Information
- Application Number
- CN202411185505.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
AI Technical Summary
The existing liquid evaporators have shortcomings in terms of evaporation rate, evaporation efficiency and use stability, especially the heat transfer capability of the static evaporator is limited, making it difficult to achieve effective thermal management, and there is a problem of solute crystal blocking the transmission channel.
The 3D liquid evaporator modified with MXene-Ti4O7 composite material uses fabric matrix and rotation design, combined with porous structure and photothermal coating, improves the photothermal conversion efficiency and steam diffusion ability, and realizes continuous dissolution and steam generation of salt crystals.
It significantly improves the evaporation rate and stability, achieves efficient water evaporation efficiency and salt resistance, can operate continuously for a long time under high salinity conditions, and is suitable for seawater desalination and wastewater treatment.
Smart Images

Figure CN118987639A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of seawater desalination, and in particular to a MXene-modified liquid evaporator and a preparation method and application thereof. Background Art
[0002] With the rapid growth of population and the development of industry, the sustainable development of society still faces certain freshwater shortage problems. Using solar energy to produce drinking water is an emerging technology to solve the shortage of water resources. Among them, solar thermal interfacial water evaporation technology has become a research hotspot due to its advantages of energy saving, low cost and high efficiency. It has great potential for industrialization and is considered to be one of the sustainable and most promising solutions to overcome water shortage.
[0003] The pursuit of high evaporation rate and high efficiency is the focus of interfacial photothermal evaporation. The above performance is mainly affected by factors such as light absorption capacity, water transfer path, thermal management, and additional environmental energy input. In order to obtain faster evaporation rates, two strategies have been applied. One strategy is to explore excellent photothermal materials for solar energy collection as raw materials for the preparation of evaporators. The above materials include carbonaceous materials, plasma nanoparticles, organic polymers, and metal compounds. The properties of the materials determine the light absorption and photothermal conversion efficiency. Another strategy is to optimize the design of the evaporator structure, which mainly affects the energy system and evaporation efficiency. The evaporation rate of conventional two-dimensional evaporators under one-sun irradiation is usually lower than 100% solar-water vapor conversion efficiency (about 1.47 kg m -2 h -1 ) theoretical limit. Recently optimized three-dimensional evaporator structures have been innovatively equipped with strategies for energy collection and evaporation enthalpy recovery from the environment, which enables the water evaporation rate to exceed the theoretical upper limit, thereby making the evaporation efficiency exceed 100%. However, although the 3D "static evaporator" has certain advantages, it mainly relies on the molecular self-diffusion process for mass transfer, resulting in high humidity around the evaporator, making it difficult for steam to diffuse, and the evaporation rate (maximum 6kg m -2 h -1 ) is relatively slow. At the same time, the heat transfer capacity of static evaporation is limited, it is difficult to achieve effective thermal management, and there are problems such as solute crystallization blocking the transmission channel. In order to solve the above problems, some technologies have tried to develop 3D "dynamic evaporators", but they still cannot effectively improve the evaporation rate, and the stability of the evaporator is limited.
[0004] In summary, the liquid evaporator in the related art has technical problems such as poor evaporation rate, evaporation efficiency or usage stability. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a MXene-modified liquid evaporator, which can effectively improve the photothermal conversion efficiency and absorbance, increase the evaporation rate of the liquid, and enhance the long-term stability of the liquid evaporation when evaporating the liquid by photothermal method.
[0006] The invention also provides a method for preparing the liquid evaporator.
[0007] The present invention also provides application of the liquid evaporator.
[0008] According to an embodiment of the first aspect of the present invention, there is provided a MXene-modified liquid evaporator, the liquid evaporator comprising:
[0009] Support rods;
[0010] A 3D body, the 3D body includes a substrate made of fabric, and a photothermal coating attached to the surface of the substrate; the raw materials for preparing the photothermal coating include MXene-Ti4O7 composite materials; the 3D body is rotatably connected to the support rod.
[0011] The liquid evaporator according to the embodiment of the present invention has at least the following beneficial effects:
[0012] In the liquid evaporator provided by the present invention, a fabric substrate is used, and the multi-level pores formed by the yarn / fiber gaps of the fabric provide excellent conditions for steam dissipation and water transmission. One-dimensional water transmission greatly reduces heat loss; in addition, the porous structure provides sufficient evaporation surface, and the open pores of the fabric can promote effective steam diffusion and natural convection flow. Furthermore, the liquid evaporator provided by the present invention has a 3D structure, which has the advantages of a 3D liquid evaporator and can significantly improve water evaporation efficiency.
[0013] In order to ensure that the liquid evaporator maintains stable and excellent evaporation performance, the management of salt (solute) crystallization during liquid evaporation is also crucial. In the continuous evaporation process, it is inevitable that salt will crystallize on the surface of the liquid evaporator, which not only reduces light absorption, but also blocks the channels for water supply and steam release, greatly inhibiting the practical application of the liquid evaporator in photothermal evaporation. In the liquid evaporator provided by the present invention, under the action of salt convection and salt gravity, when the salt solution approaches the edge, the salt concentration gradually increases, and the salt crystallizes at the tip of the 3D body. Continuous steam generation and salt collection are achieved in uninterrupted operation. Under certain convection, the liquid evaporator can rotate and the salt can also be dissolved. The reason is that convection can rotate the 3D windmill, and the rotation allows the tip to contact water, so that the crystallized salt can be dissolved, which also avoids the influence of salt crystallization on the evaporation of the liquid evaporator. As a result, the liquid evaporator provided by the present invention can operate stably for a long time.
[0014] The surface of the 3D main body provided by the present invention adopts a photothermal coating made of a MXene-Ti4O7 composite material, in which MXene and Ti4O7 have a synergistic effect, and the photothermal coating has high photothermal conversion efficiency and absorbance, with a specific absorbance of up to 98.7%.
[0015] During actual use, some edges of the 3D body come into contact with the liquid to be treated, and are transmitted to all parts of the 3D body through static transmission or dynamic transmission during the rotation of the 3D body, so that the liquid evaporates. The support rod plays a supporting role. On the one hand, it can prevent the 3D body from losing its evaporation effect when immersed in water, and on the other hand, it can provide a fulcrum for the rotation of the 3D body, transforming static 3D liquid evaporation into dynamic 3D liquid evaporation, thereby improving the comprehensive performance of the liquid evaporator.
[0016] From the data, the liquid evaporator provided by the present invention has an evaporation rate of ≥2.56 kg m in a static state under the irradiation of 1 sun. -2 h -1 ; in convection 3.5ms -1 Under the irradiation of 1 sun, the liquid evaporator achieves rotary evaporation with an evaporation rate of up to 7.25 kg m -2 h -1 At the same time, it can maintain excellent stability even under high salinity (20wt% NaCl solution) conditions; specifically, continuous steam generation and salt collection were achieved in uninterrupted operation for more than 300h, and energy efficiency and water evaporation were not affected by salt accumulation, indicating that it has the potential for sustainable and practical applications in the future.
[0017] In summary, the liquid evaporator provided by the present invention has the characteristics of high photothermal conversion efficiency, stable and efficient water evaporation rate, excellent salt resistance and suitability for large-scale applications, and shows broad application prospects in the fields of seawater desalination and wastewater treatment.
[0018] According to some embodiments of the present invention, the support rod is made of iron. In actual production, the material is not strictly limited, and any material with certain strength, toughness and aging resistance can be used to prepare the support rod.
[0019] According to some embodiments of the present invention, the liquid evaporator further comprises a bearing, and the 3D body and the support rod are connected via the bearing.
[0020] According to some embodiments of the present invention, the diameter of the bearing is 4-10 mm, for example, about 5 mm, 6 mm, 7 mm, 8 mm or about 9 mm.
[0021] According to some embodiments of the present invention, the bearing comprises a copper shaft. In actual production, the material is not strictly limited as long as a smooth rotation connection can be achieved.
[0022] According to some embodiments of the present invention, the material of the matrix includes at least one of cotton, linen, wool and polyester. That is, in actual production, the yarn used to weave the matrix is pure spun yarn or blended yarn.
[0023] According to some embodiments of the present invention, the diameter of the yarn used to weave the matrix is 1-3 mm, for example, about 1.5 mm, 2.0 mm or about 2.5 mm.
[0024] According to some embodiments of the present invention, the number of strands of yarn used to weave the matrix is 2 to 6, for example, 3, 4 or 5.
[0025] According to some embodiments of the present invention, the 3D body further comprises a hydrophilic coating disposed between the substrate and the photothermal coating. The excellent hydrophilicity ensures timely water supply.
[0026] According to some embodiments of the present invention, the component of the hydrophilic coating includes at least one of polydopamine and polyethyleneimine.
[0027] According to some embodiments of the present invention, the shape of the 3D body includes a windmill shape or a disk shape.
[0028] According to some embodiments of the present invention, when the 3D body is in the shape of a windmill, the number of blades it has is 2 to 7. For example, the number of blades may be 2, 3, 4, 5 or 6.
[0029] According to some embodiments of the present invention, the diameter of the circumscribed circle of the 3D body is 4-10 cm, for example, about 4 cm, 6 cm, 7 cm, 8 cm or about 9 cm.
[0030] According to some embodiments of the present invention, the thickness of the 3D body is 0.5-1 cm. The thickness is the thickness of the thickest part of the 3D body. For example, if the 3D body is in the shape of a windmill, the thickness is the maximum vertical distance between the back and front of the windmill.
[0031] According to some embodiments of the present invention, the angle between the axis of the 3D body and the axis of the support rod is greater than 0° and less than or equal to 90°. That is, there is a certain angle between the two, so that when the support rod stands vertically in the liquid to be treated, the height of the support rod can be adjusted to ensure that part of the edge of the 3D body is in contact with the liquid to be treated.
[0032] According to an embodiment of the second aspect of the present invention, a method for preparing the liquid evaporator is provided, the method comprising the following steps:
[0033] S1. Weaving a matrix of the 3D body using yarn;
[0034] S2. Depositing the photothermal coating on the surface of the substrate;
[0035] S3. Assembly.
[0036] In the preparation method, the numbers S1, S2 and S3 are only for the convenience of expression and do not represent the actual implementation order. For example, the assembly of step S3 can be performed after step S2 or between step S2 and step S1.
[0037] Since the preparation method adopts all the technical solutions of the liquid evaporator of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.
[0038] Furthermore, the preparation method provided by the present invention is simple to operate, easy to implement, and convenient for large-scale promotion and use.
[0039] According to some embodiments of the present invention, in step S1, the weaving method of the 3D body includes at least one of knitting and crocheting. In actual production, a suitable weaving method can be selected according to experimental conditions and common sense; if there is no special explanation, the specific weaving steps can be carried out according to the method in common sense.
[0040] If the weaving method is crocheting, the simple sequence of weaving is as follows: first, create a simple loop knot on one side, which will serve as the starting point; insert the hook into the loop, pull the thread through the loop, and form a new loop; continue to repeat this step on each basic chain to form a sheet-like semi-finished product, and fold the semi-finished product to obtain the base. In actual production, the number of crocheted circles can be adjusted according to experimental requirements to prepare a series of bases with different leaf numbers and sizes.
[0041] According to some embodiments of the present invention, in step S2, the assembly connects the center point of the base to the bearing; and fixes the support rod on the other side of the bearing, so that the base can rotate dynamically under the action of the bearing. The connection method can be glue bonding. In actual production, other commonly used connection methods can also be used as long as the purpose of connection can be achieved.
[0042] According to some embodiments of the present invention, step S1 further includes cleaning the substrate, thereby removing impurities on the surface of the substrate and facilitating the subsequent deposition of the photothermal coating and the like.
[0043] The cleaning method comprises alkali cleaning, water cleaning and drying performed in sequence.
[0044] The detergent used for the alkaline washing is a sodium hydroxide aqueous solution, and the mass concentration of the sodium hydroxide aqueous solution is 5-8%, for example, about 6%.
[0045] The drying temperature is 50-70°C, for example, about 60°C.
[0046] According to some embodiments of the present invention, the preparation method further comprises depositing a hydrophilic coating on the surface of the substrate between step S1 and step S2.
[0047] According to some embodiments of the present invention, the method for depositing the hydrophilic coating comprises immersing the substrate in a solution comprising a hydrophilic component.
[0048] The hydrophilic component includes at least one of dopamine (DA) and polyethyleneimine (PEI). Specifically, it can be a mixture of dopamine and polyethyleneimine; more specifically, the mass ratio of dopamine to polyethyleneimine is 1:0.5-2.5. For example, it can be about 1:0.7, 1:0.8, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.8, 1:2 or about 1:2.2. Thus, dopamine can further form polydopamine, and the resulting hydrophilic coating has both hydrophilicity and surface cationic properties.
[0049] The solution of the hydrophilic component includes a Tris buffer as a solvent. The pH of the Tris buffer is 7.5 to 8.5, for example, it can be about 8. The concentration of the Tris buffer is 0.02 to 1.5 mol / L, for example, it can be about 0.05 mol / L, 0.1 mol / L or about 1 mol / L.
[0050] In the solution of the hydrophilic components, the concentration of each hydrophilic component is 0.6-2 mg / mL. For example, the concentration of dopamine can be 0.6-2 mg / mL; more specifically, the concentration of dopamine is 0.8 mg / mL, 1.0 mg / mL, 1.2 mg / mL, 1.4 mg / mL, 1.5 mg / mL, 1.6 mg / mL or about 1.8 mg / mL.
[0051] The duration of the immersion is 10 to 20 hours; for example, it can be about 12 hours, 13 hours, 15 hours or about 18 hours.
[0052] The immersion temperature is 20 to 30°C; for example, it can be about 25°C;
[0053] The method for depositing the hydrophilic coating further includes drying after the dipping.
[0054] The drying temperature of the hydrophilic coating is 50-70°C; for example, it can be about 55°C, 60°C or about 65°C;
[0055] The drying time for preparing the hydrophilic coating is 3 to 6 hours; for example, it can be about 4 hours, 4.5 hours or about 5 hours.
[0056] According to some embodiments of the present invention, in step S2, the deposition of the photothermal coating comprises at least one of coating and dipping. Regardless of the deposition method, the MXene-Ti4O7 composite material can be deposited on the surface of the substrate by electrostatic assembly.
[0057] According to some embodiments of the present invention, in step S2, when the deposition method of the photothermal coating is immersion;
[0058] The duration of the immersion is 2 to 4 hours, for example, about 2.5 hours, 3.0 hours or about 3.5 hours.
[0059] According to some embodiments of the present invention, in step S2, the deposition of the photothermal coating further includes drying after the coating or dipping.
[0060] The drying temperature is 35-55°C, for example, about 40°C, 45°C or about 50°C;
[0061] The drying time is 6 to 9 hours; for example, it can be about 7 hours or about 8 hours.
[0062] According to some embodiments of the present invention, in step S2, in the deposition of the photothermal coating, the preparation raw material used is a mixed dispersion obtained by mixing a MXene dispersion and a Ti4O7 dispersion.
[0063] According to some embodiments of the present invention, in the mixed dispersion, the sum of the concentrations of MXene and Ti4O7 is 5 to 10 mg / mL, for example, about 7 mg / mL or 8 mg / mL.
[0064] According to some embodiments of the present invention, the concentration of the MXene dispersion is 1 to 15 mg / mL, for example, about 2 mg / mL, 3 mg / mL, 4 mg / mL, 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL, 10 mg / mL, 12 mg / mL or about 14 mg / mL.
[0065] According to some embodiments of the present invention, in the mixed dispersion, the mass ratio of MXene to Ti4O7 is 0.2 to 5:1. For example, it can be about 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1 or about 4.5:1.
[0066] According to some embodiments of the present invention, the preparation method of the MXene dispersion is:
[0067] S2a. The MAX phase powder was added to a mixed solution of HCl and LiF and the reaction was stirred at a constant temperature;
[0068] S2b. The resulting mixture was washed by centrifugation with deionized water until the pH of the supernatant was close to neutral; obtaining a precipitate;
[0069] S2c. The obtained precipitate is dispersed in deionized water and ultrasonicated, and centrifuged again to obtain the upper supernatant, i.e., the MXene dispersion.
[0070] According to some embodiments of the present invention, in step S2a, the particle size of the MAX phase powder is 200-600 mesh. For example, it can be about 300 mesh, 400 mesh or 500 mesh. In the present invention, particles of corresponding mesh size indicate that the particles can pass through a sieve of the mesh size, i.e., the particles under the sieve of the mesh size.
[0071] According to some embodiments of the present invention, in step S2a, the method for preparing the mixed solution of HCl and LiF comprises mixing LiF and HCl aqueous solutions. The molar ratio of LiF to HCl is 1:2 to 5, for example, about 1:3 or about 1:4. The concentration of the HCl aqueous solution is 8 to 10M, for example, about 9M.
[0072] According to some embodiments of the present invention, in step S2a, the mass volume ratio of the MAX phase powder to the mixed solution is 1 g: 15-25 mL, for example, about 1 g: 18 mL, 1 g: 20 mL or about 1 g: 22 mL.
[0073] According to some embodiments of the present invention, in step S2a, the temperature of the constant temperature stirring reaction is 30-40°C, for example, about 32°C, 34°C, 35°C or about 38°C.
[0074] According to some embodiments of the present invention, in step S2a, the constant temperature stirring reaction time is 10 to 36 hours, for example, about 12 hours, 15 hours, 18 hours, 20 hours, 22 hours, 24 hours, 28 hours, 30 hours, 32 hours or about 34 hours.
[0075] According to some embodiments of the present invention, in step S2b, the near-neutral pH is 6 to 7. For example, it may be about 6.5.
[0076] According to some embodiments of the present invention, in step S2b and step S2c, the centrifugal washing or the like has a centrifugal speed of 3500-6000 rpm, for example, about 4000 rpm, 4500 rpm, 5000 rpm or about 5500 rpm.
[0077] According to some embodiments of the present invention, in step S2b, in the centrifugal washing, the duration of each centrifugation is 3 to 8 minutes; for example, it can be specifically about 5 minutes.
[0078] According to some embodiments of the present invention, in step S2c, the ultrasonication is performed in an ice water bath. The mass volume ratio of the MAX phase powder added in step S2a to the deionized water used in this step is 1 g:45-55 mL. For example, it can be about 1 g:48 mL, 1 g:50 mL or about 1 g:52 mL.
[0079] According to some embodiments of the present invention, in step S2c, the duration of the ultrasound is 0.5 to 1.5 hours; for example, it may be about 1 hour.
[0080] According to some embodiments of the present invention, in step S2c, the duration of the re-centrifugation is 5 min to 1.5 h; for example, it may be about 10 min, 30 min or about 1 h.
[0081] According to some embodiments of the present invention, the mass of MXene in the mixed dispersion is 3-25% of the mass of the matrix, for example, about 4%, 5%, 6%, 8%, 10%, 12%, 15%, 18%, 20% or about 23%.
[0082] According to some embodiments of the present invention, in step S3, the assembling includes assembling and connecting the 3D body, the bearing and the support rod obtained in step S2.
[0083] If step S3 is performed before step S2, the assembling includes assembling and connecting the base, bearing and support rod obtained in step S1.
[0084] According to an embodiment of the third aspect of the present invention, there is provided an application of the liquid evaporator in seawater desalination or wastewater treatment.
[0085] Since the application adopts all the technical solutions of the liquid evaporator of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment. Specifically, the seawater desalination and wastewater treatment performed by the liquid evaporator are simpler and less costly.
[0086] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 100 is actually 100±2%×100.
[0087] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values 2 and 3.
[0088] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0089] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0090] Figure 1 This is the crocheting process of the substrate in step S1 of embodiment 1 of the present invention (taking substrate C as an example).
[0091] Figure 2 This is the apparent morphology of substrates A to F obtained in Example 1 of the present invention.
[0092] Figure 3 It is a schematic structural diagram of the liquid evaporator obtained in Example 1 of the present invention (the substrate is taken as substrate C as an example).
[0093] Figure 4 These are SEM images of the mixed dispersion obtained in step S3d of Example 1 of the present invention (a-d), the matrix C obtained in step S1 (e-f), and the obtained 3D body (taking matrix C as an example) (g-h).
[0094] Figure 5 This is the hydrophilicity test result of the 3D body (taking the base C as an example) in the liquid evaporator obtained in Example 1 of the present invention.
[0095] Figure 6 The light absorption performance of Example 1 of the present invention, Comparative Examples 1-2 (the substrate is substrate C as an example) and substrate C are shown.
[0096] Figure 7 Schematic diagram of application scenario of the liquid evaporator obtained in the embodiment of the present invention (the substrate is taken as substrate C as an example).
[0097] Figure 8 It is the wet temperature of the liquid evaporator obtained in Example 1 of the present invention (the substrate is taken as substrate C as an example) under different light illumination.
[0098] Fig. 9 These are the dry state (a) and wet state (b) temperatures of the liquid evaporator obtained in Example 1 of the present invention (the substrate is substrate C as an example) under light and air convection.
[0099] Fig.10 It is the water evaporation rate (a) of the liquid evaporator obtained in Example 1 of the present invention (the substrate is taken as substrate C as an example) under different light illumination, and the water evaporation rate (b) of different liquid evaporators obtained in Example 1 of the present invention under the same light illumination.
[0100] Fig.11 This is a comparison of the apparent changes over time in the evaporation effect of seawater on the liquid evaporator obtained in Example 1 of the present invention (the substrate is taken as substrate C as an example).
[0101] Fig.12 It is the salt crystals precipitated at the tip of the blade when the liquid evaporator obtained in Example 1 of the present invention (the substrate is taken as substrate C as an example) evaporates seawater and its weight. DETAILED DESCRIPTION
[0102] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0103] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0104] Example 1
[0105] In this example, a liquid evaporator is prepared, and the specific steps are as follows:
[0106] S1. The base for weaving the 3D body:
[0107] First, use four strands of cotton yarn (about 2mm in diameter) as the raw material and crochet with a crochet hook. Specifically: create a simple loop on one side, which will serve as the starting point. Insert the crochet hook into the loop, pull the thread through the loop, and form a new loop. Continue to repeat this step on each basic chain until a sheet-like semi-finished product is hooked, folded to form a series of bases; among them,
[0108] Base A is in the shape of a pinwheel, with three blades and a circumscribed circle diameter of 4 cm;
[0109] Base B is in the shape of a pinwheel, with 4 blades and a circumscribed circle with a diameter of 4 cm;
[0110] Base C is in the shape of a pinwheel, with 5 blades and a circumscribed circle diameter of 4 cm;
[0111] The base D is in the shape of a windmill, with 7 blades and a circumscribed circle diameter of 4 cm;
[0112] Substrate E is disc-shaped with a diameter of 4 cm;
[0113] The base F is in the shape of a windmill, with 5 blades and a circumscribed circle with a diameter of 10 cm;
[0114] The appearance of matrix A~F is as follows Figure 2 As shown; thickness is approximately 10mm.
[0115] Taking the matrix C as an example, the crochet process of the matrix is as follows: Figure 1 shown.
[0116] Cleaning the substrate: Clean with sodium hydroxide aqueous solution (mass concentration of 6%) and distilled water in sequence and dry (about 60° C.) to remove impurities on the surface of the fabric.
[0117] S2. Preparation of hydrophilic coating:
[0118] Prepare a mixed solution of dopamine (DA) and polyethyleneimine (PEI); immerse the substrate obtained in step S1 in the mixed solution at room temperature (about 25°C) for 12 hours and then dry.
[0119] The solvent of the mixed solution used to prepare the hydrophilic coating is Tris buffer (pH about 8, concentration about 0.05 mol / L); the mass ratio of dopamine (DA) and polyethyleneimine (PEI) is 1:1.2; the concentration of dopamine is 1 mg / mL. During the immersion and drying process, dopamine undergoes a certain degree of polymerization to form polydopamine.
[0120] The drying temperature was 60°C and the drying time was 4.5 h.
[0121] Preparation of photothermal coating:
[0122] S2a. 2.5 g of MAX phase powder (particle size of 200 mesh, i.e., can pass through a 200 mesh sieve, but cannot pass through a 400 mesh sieve) was added to a mixed solution of HCl and LiF, and the mixture was stirred at a constant temperature of about 35°C for 30 h;
[0123] The mixed solution was prepared by mixing 50 mL of 9 mol / L HCl aqueous solution and 3.0 g of LiF.
[0124] S2b. The resulting mixture was repeatedly washed by centrifugation with deionized water (centrifugation rate of about 5000 rpm, single centrifugation time of about 5 min) until the pH of the supernatant was close to neutral (pH of about 6); obtaining a precipitate;
[0125] S2c. The obtained precipitate is dispersed in deionized water and ultrasonicated (carried out in a water bath, the volume of deionized water used is 100 mL, and the ultrasonication time is about 30 min), and centrifuged again (the centrifugal speed is about 5000 rpm, and the centrifugal time is 5 min) to take the upper supernatant, i.e., the MXene dispersion; wherein the concentration of MXene is 5 mg / mL.
[0126] S2d. Mix the MXene dispersion and the Ti4O7 dispersion to obtain a mixed dispersion; wherein the mass ratio of MXene to Ti4O7 is about 2:1, and the sum of the concentrations of MXene and Ti4O7 is 7 mg / mL.
[0127] S2e. Immerse the substrate coated with the hydrophilic coating (soak it in water) in the mixed dispersion obtained in step S2d, and then dry it (at about 50°C). The mass of MXene in the mixed dispersion is 15% of the mass of the substrate. During the immersion process, the MXene-Ti4O7 composite material is deposited on the surface of the substrate with the hydrophilic coating in the form of electrostatic assembly.
[0128] S3. Use glue to connect the center point of the 3D body obtained in step S2 and the bearing (about 8mm in diameter, copper shaft), and fix the support rod (made of iron) on the other side of the bearing. Taking the base C as an example, the structure of the product obtained in this step is as follows: Figure 3 shown.
[0129] Example 2
[0130] This example prepares a liquid evaporator, which differs from Example 1 in that:
[0131] (1) In step S1, the parameter difference is:
[0132] The diameter of the bearing used is 5mm;
[0133] (2) In step S2, the parameter differences in the preparation process of the hydrophilic coating are:
[0134] The mass ratio of dopamine (DA) and polyethyleneimine (PEI) was 1:2;
[0135] (3) In step S2, the parameter differences in the photothermal coating preparation process are:
[0136] In step S2a, the particle size of the MAX phase powder used is 400 mesh (400 mesh sieve under); the temperature of the constant temperature stirring reaction is 32° C., and the reaction time is 12 h;
[0137] The centrifugal speed in steps S2b to S2c is 4000 rpm;
[0138] The concentration of the MXene dispersion obtained in step S2c is 3 mg / mL.
[0139] In step S2e, the mass of MXene in the mixed dispersion is 4% of the mass of the matrix.
[0140] Example 3
[0141] This example prepares a liquid evaporator, and the specific steps are different from those in Example 1 in that:
[0142] (1) In step S1, the parameter difference is:
[0143] In step S1, the diameter of the yarn used is 3 mm;
[0144] In step S3, the diameter of the bearing used is 10 mm;
[0145] (2) In step S2, the parameter differences in the preparation process of the hydrophilic coating are:
[0146] The mass ratio of dopamine (DA) to polyethyleneimine (PEI) was 1.5:1; the concentration of dopamine was 1.5 mg / mL;
[0147] (3) In step S2, the parameter differences in the photothermal coating preparation process are:
[0148] In step S2a, the particle size of the MAX phase powder used is 600 mesh (600 mesh sieve undersize); the temperature of the constant temperature stirring reaction is 42° C., and the reaction time is 28 hours;
[0149] The centrifugal speed in steps S2b to S2c is 6600 rpm;
[0150] The concentration of the MXene dispersion obtained in step S2c is 12 mg / mL.
[0151] In step S2e, the mass of MXene in the mixed dispersion is 25% of the mass of the matrix.
[0152] Example 4
[0153] This example prepares a liquid evaporator, which differs from Example 1 in that:
[0154] (1) In step S2, the parameter differences in the process of preparing the hydrophilic coating are:
[0155] The duration of immersion is 18h;
[0156] The solvent used was Tris buffer with a pH of 8.5 and a concentration of 1.5 mol / L;
[0157] The mass ratio of dopamine (DA) and polyethyleneimine (PEI) was 1:1;
[0158] (2) In step S2, the parameter differences in the process of preparing the photothermal coating are:
[0159] In step S2a, the mixed solution of HCl and LiF is prepared by slowly adding 2.5 g of LiF into 50 mL of 9 M HCl solution.
[0160] In step S2a, the temperature of the constant temperature stirring reaction is 40° C. and the duration is 21 h;
[0161] The centrifugal speed in step S2b is 3500 rpm; the duration of each centrifugation is 5 min;
[0162] In step S2c, the conditions for dispersion, ultrasonication and centrifugation are:
[0163] The duration of ultrasonic dispersion was 1 h;
[0164] The centrifugation time was 1 h and the speed was 3500 rpm.
[0165] In step S2c, the concentration of MXene in the obtained MXene dispersion is 4 mg / mL.
[0166] In step S2d, the mass ratio of MXene and Ti4O7 is about 1:1.
[0167] In step S2e, the immersion time is 3 hours;
[0168] In step S2e, the drying temperature is 40° C. and the drying time is 7 h.
[0169] Comparative Example 1
[0170] This example prepares a liquid evaporator, which differs from Example 1 in that:
[0171] Step S3d is not included, i.e., the substrate portion is directly impregnated with the MXene dispersion;
[0172] In step S3e, the mass of MXene in the MXene dispersion accounts for 22.5% of the mass of the matrix (consistent with the amount of MXene+Ti4O7 in Example 1).
[0173] Comparative Example 2
[0174] This example prepares a liquid evaporator, which differs from Example 1 in that:
[0175] Excluding steps S3a to S3d, in step S3e, the impregnation is directly carried out with Ti4O7 dispersion, and the mass of Ti4O7 in the Ti4O7 dispersion accounts for 22.5% of the mass of the matrix (consistent with the amount of MXene+Ti4O7 in Example 1).
[0176] Test Case
[0177] In the first aspect of this example, the morphology of the mixed dispersion obtained in step S3d and the 3D body in step S3e was tested by SEM. The results showed that
[0178] In the mixed solution, the MXene-Ti4O7 composite material is an integral structure, specifically MXene wraps Ti4O7; the morphology of the 3D body shows that the MXene-Ti4O7 composite material is deposited on the surface of the yarn fiber, forming a photothermal coating. Compared with the yarn without photothermal coating modification, its roughness is significantly improved, which is helpful for capturing light; the morphology of the 3D body obtained in different embodiments is similar. Specifically, the morphology test results of the mixed dispersion in Example 1 and the substrate C after the photothermal coating is set are as follows Figure 4 As shown, Figure 4 In the figure, (a) to (d) are SEM images of MXene-Ti4O7 composite materials in the mixed solution, (e) to (f) are the morphologies of yarn fibers in the matrix C; (g) to (h) are the morphologies of the 3D body deposited with hydrophilic coating and photothermal coating.
[0179] In the second aspect of this example, the hydrophilicity of the 3D body in the liquid evaporator obtained in the embodiment and the comparative example was tested. The test method was to place the 3D body on a water contact angle measuring instrument and squeeze 4 μL of water on its surface. The time required for the water droplets to wetting the fabric surface was observed, and an image was taken with a high-speed camera. The results showed that in the liquid evaporators obtained in the embodiment and the comparative example, the wetting process of the water droplets was <1s; this indicates that the liquid evaporator provided by the present invention exhibits super hydrophilic properties by providing a hydrophilic coating. Taking the 3D body in which the substrate is substrate C in Example 1 as an example, its hydrophilicity effect diagram is as shown in the figure below. Figure 5 shown.
[0180] The third aspect of this example tests the light absorption performance of the liquid evaporator (mainly the 3D body) whose 3D main body shape is the shape of the matrix C and the matrix C in Example 1 and Comparative Examples 1 to 2. The specific test method is: use a UV-vis-NIR ultraviolet spectrometer to test the light absorption performance of the 3D bodies obtained in Example 1 and Comparative Examples 1 to 2 within the wavelength range of 280 to 2500 nm. The results show that within the test range, the absorbance of Example 1 (shown as MXene / Ti4O7 modified fabric in the figure) is close to 98.7%, which is greater than the absorbance of the original windmill fabric of 58.5% (matrix C), the absorbance of MXene modified fabric of 93.3% (Comparative Example 1) and the absorbance of Ti4O7 modified fabric of 95.3% (Comparative Example 2). It can be seen that in the photothermal coating used in the present invention, a significant synergistic effect occurs between MXene and Ti4O7. The specific test results are as follows: Figure 6 shown.
[0181] The fourth aspect of this example tests the light-to-heat conversion performance of the liquid evaporator obtained in the embodiment and the comparative example, and specifically tests the temperature of the 3D body under different convection and illumination; the test method is:
[0182] refer to Figure 7 The liquid evaporator (substrate C in Example 1) is fixedly placed in a glass container filled with 300 mL of water. There is a liquid contact point between the liquid evaporator and the water, and the water is transported to the 3D body through this contact point. A xenon lamp is used to simulate a solar light source to perform a lighting experiment. Different solar light intensities are used to irradiate the wet or dry surface of the 3D body, and an infrared thermal imager is used to monitor the surface temperature changes in real time.
[0183] The results show that the temperature of the wet 3D body is 31.2°C under 0.5 suns (static, non-convective, stable temperature); 36.9°C under 1 sun; 41.8°C under 1.5 suns; and 45.1°C under 2 suns. The liquid evaporator exhibits excellent light-to-heat conversion performance. Figure 8 shown.
[0184] In the case of 3.5m / s air convection (air blowing towards the 3D body), under 1 sun, the surface temperature of the dry 3D body does not change much. In the wet state, the surface temperature of the 3D body drops significantly, from 38°C to 30°C at the center, indicating that convection can help to quickly evaporate water. Since water evaporation requires heat energy, the temperature is reduced. The specific test results are as follows Fig. 9 As shown, Fig. 9 Figure a in the middle represents the dry state, and figure b corresponds to the wet state. Each group of figures is a thermal imaging image at different times and conditions.
[0185] The fifth aspect of this example tests the light-to-heat conversion performance of the liquid evaporator obtained in the embodiment and the comparative example, and specifically tests the evaporation performance of seawater and the salt crystallization performance; wherein,
[0186] The test method for seawater evaporation performance is:
[0187] refer to Figure 7 The liquid evaporator prepared in the embodiment or comparative example is fixedly placed in a beaker filled with seawater, a lighting experiment is carried out using a simulated solar light source, and the change in the evaporation mass of the water body is monitored using an electronic balance; the test is a static test.
[0188] The test results show that the evaporation rate of water increases with the light intensity. The evaporation rate of the liquid evaporator obtained in Example 1 (the 3D main body adopts the shape of the substrate C) is as high as 4.25 kg m under 2 suns. -2 h -1 The liquid evaporators with different numbers of blades in Example 1 also exhibit different evaporation rates. It can be seen that the evaporation rate first increases and then decreases as the number of blades increases. The specific test results are as follows: Fig.10 As shown, (a) shows the performance of the liquid evaporator in the shape of substrate C in Example 1, and (b) shows the performance of the liquid evaporators of different shapes obtained in Example 1, and Figure (b) uses 1 sun intensity.
[0189] The test method for salt crystallization performance is:
[0190] refer to Figure 7 The liquid evaporator prepared in the embodiment or comparative example was fixedly placed in a beaker filled with a 5% salt concentration aqueous solution, and an evaporation test was carried out for 84 hours under the irradiation of one sun (static test, without air convection).
[0191] The results showed that precipitated salt crystals were observed at the apex of the liquid evaporator blades but not on the surface of the evaporator. The reason is that under the action of salt convection and salt gravity, when the salt solution approaches the edge, the salt concentration gradually increases, and the salt crystallizes at the tip of the 3D body. Continuous steam generation and salt collection are achieved during uninterrupted operation. Under certain convection, the liquid evaporator can rotate and the salt can be dissolved. The reason is that convection can cause the 3D windmill to rotate, and the rotation allows the tip to contact the water, so that the crystallized salt can be dissolved, thus avoiding the influence of salt crystallization on the evaporation of the liquid evaporator. Taking the liquid evaporator obtained by using substrate C as the substrate in Example 1 as an example, the specific test process and results are as follows. Figures 11-12 shown.
[0192] In summary, the liquid evaporator provided by the present invention, due to its unique structure and material design, plus the synergistic effect of the components in the photothermal coating, can significantly improve the utilization of light and the evaporation rate of the liquid, and can operate stably for a long time; in order to overcome the fresh water crisis, it provides a low-cost, efficient, scalable, salt-resistant and green reuse technical solution, and also provides new ideas for wastewater treatment.
[0193] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A MXene-modified liquid evaporator, characterized in that: The liquid evaporator comprises: Support rods; A 3D body, the 3D body includes a substrate made of fabric, and a photothermal coating attached to the surface of the substrate; the raw materials for preparing the photothermal coating include MXene-Ti4O7 composite materials; the 3D body is rotatably connected to the support rod.
2. The liquid evaporator according to claim 1, characterized in that: The liquid evaporator further includes a bearing, and the 3D body and the support rod are connected via the bearing; and / or, the 3D body further includes a hydrophilic coating disposed between the substrate and the photothermal coating.
3. The liquid evaporator according to claim 2, characterized in that: The components of the hydrophilic coating include at least one of polydopamine and polyethyleneimine.
4. The liquid evaporator according to any one of claims 1 to 3, characterized in that: The shape of the 3D body includes a windmill shape or a disk shape.
5. The liquid evaporator according to claim 4, characterized in that: The diameter of the circumscribed circle of the 3D body is 4 to 10 cm.
6. A method for preparing a liquid evaporator according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: S1. Weaving a matrix of the 3D body using yarn; S2. Depositing the photothermal coating on the surface of the substrate; S3. Assembly.
7. The preparation method according to claim 6, characterized in that: The preparation method further comprises depositing a hydrophilic coating on the surface of the substrate between step S1 and step S2.
8. The preparation method according to claim 6 or 7, characterized in that: In step S2, the deposition method of the photothermal coating includes at least one of coating and dipping.
9. The preparation method according to claim 8, characterized in that: In step S2, in the deposition of the photothermal coating, the raw material used for preparation is a mixed dispersion obtained by mixing a MXene dispersion and a Ti4O7 dispersion.
10. Use of the liquid evaporator according to any one of claims 1 to 5 in seawater desalination or wastewater treatment.
Citation Information
Patent Citations
Thin film based on two-dimensional trititanium dicarbide / titanium dioxide heterojunction and preparation method and application of thin film
CN113816455A
Gear-shaped self-rotating solar interface evaporator and preparation method thereof
CN116495817A
Desulfurization wastewater treatment-oriented self-rotating and self-cleaning photo-thermal device and method
CN117902661A
MXene-TiO2-Ag double-layer hydrogel as well as preparation and application thereof
CN118388718A
Electronic apparatus and method for data labeling based domain-dependent template
KR102763213B1
Cited By
Dynamic scouring type salt-resistant solar interface evaporation system
CN120887497A