Composite hollow fiber membrane and preparation method thereof
By performing melt-engagement modification and combined stretching and annealing treatment on the twin-screw extruder, the problems of long production cycle, low yield and reduced porosity of hollow fiber ultrafiltration membranes are solved, and high strength, hydrophilicity and high The preparation of flux composite hollow fiber membranes improves production efficiency and membrane product quality.
Patent Information
- Application Number
- CN202411299707.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing thermal phase separation method has a long production cycle and low yield. The membrane wire contains many pore defects and low tensile strength. The porosity is reduced due to high temperature annealing, and the water flux is reduced. Give full play to the advantages of ß-crystalline PVDF film.
A solid feeding system and a liquid feeding system are added to the twin-screw extruder, melt-engage modification is carried out, combined with stretching and annealing shaping treatment, component proportions and process conditions are adjusted, and high-strength, large-throughput composite hollow fiber membranes are prepared.
Achieve mass production of ß-crystalline polyvinylidene fluoride hollow fiber membranes with high strength, low viscosity and good hydrophilicity, improve the porosity and water flux of the membrane wire, extend the service life of the product, and improve the production. Efficiency and avoid volatility and decomposition of organic solvents.
Abstract
Description
Technical Field
[0001] The invention relates to the field of hollow fiber ultra-microfiltration membrane manufacturing, in particular to a composite hollow fiber membrane under a thermochromatographic method and a preparation method thereof. Background Art
[0002] Polyvinylidene fluoride has excellent thermal stability and corrosion resistance. Its good chemical resistance is extremely well utilized by the water treatment membrane industry. Therefore, it has attracted more and more attention and promotion in the field of membrane separation in recent years. In microfiltration and ultrafiltration, polyethersulfone and polyvinylidene fluoride have always been used as membrane materials with excellent performance. Their preparation process is mostly the non-solvent precipitation gel phase inversion (NIPS) method, which includes the preparation of flat membranes and hollow fiber membranes. However, the disadvantage of this method is that the solvent in the spinning solution is exchanged with the non-solvent in the coagulation bath during phase separation and molding, and finger-like pores are easily formed. In addition, the polymer content in the spinning solution is generally less than 25%, which makes the membrane fibers prepared by this method have low strength and poor corrosion resistance.
[0003] The other is the thermally induced phase separation method. As an emerging membrane-making technology, it mainly causes phase separation by cooling to form a three-dimensional porous network structure. This method uses the characteristics of high-temperature compatibility and low-temperature phase separation of resin and diluent to prepare a homogeneous porous membrane. The membrane prepared by this method has the characteristics of high strength, good chemical resistance, and uniform pore size, which greatly improves the service life of the membrane. The thermally induced phase separation method has gradually become the leading preparation technology for the new generation of PVDF porous membranes. However, due to the limitations of the performance of polyvinylidene fluoride materials themselves, the strength improvement is limited. Therefore, similar polyethersulfone composite modified thermo-induced phase PVDF (polyvinylidene fluoride) porous membrane technology with inherent strength advantages has become a research direction.
[0004] In the existing discussion on the preparation of hollow fiber ultrafiltration membranes by thermally induced phase separation, a process for preparing polyvinylidene fluoride hollow fiber membranes using an improved TIPS method has been reported. During the production process, this process converts the PVDF polymer from the conventional α-crystal form to the ß-crystal form as much as possible, so that the polyvinylidene fluoride hollow fiber membrane has higher mechanical strength while still having stronger hydrophilic properties than other crystal forms. This can be said to be an excellent improvement on the performance of TIPS membrane fibers. However, this method uses a high-temperature stirring kettle for heating and stirring, and then adopts a method similar to the NIPS method for static degassing, which makes the production cycle too long and the output low. In addition, the molten spinning solution with high viscosity has a poor static degassing effect, so the membrane contains more pore defects during spinning. In addition, due to the limitation that the degassing effect worsens with the increase in viscosity, the increase in polymer content is limited, the proportion of organic liquid is high, and the tensile strength of the product is low. At the same time, in order to obtain a higher ß-crystal content under a lower tensile strength, a multi-stage high-temperature annealing process has to be adopted, which causes the mold holes generated during the annealing process to deform and collapse, resulting in a decrease in the porosity of the membrane and a decrease in water flux.
[0005] The traditional thermoinduced phase membrane preparation method has low polymer concentration and relatively high high-temperature solvent content. The entanglement between polymers is limited when the polymer solution is extruded and molded, resulting in poor tensile properties of the membrane fiber before and after molding. As a result, the ß-crystal ratio of the prepared membrane fiber product is not high. Post-treatment processes such as annealing are required to further increase the ß-crystal ratio, but this will cause a decrease in porosity and deformation of the membrane pore size, and the advantages of the ß-crystal PVDF membrane cannot be fully utilized. It is difficult to further improve the membrane fiber strength, water flux and other properties.
[0006] Therefore, it is very meaningful to use a more suitable production process to mass-produce β-crystalline polyvinylidene fluoride hollow fiber filtration membrane fibers with high polymer content, good membrane fiber strength and good hydrophilicity. Summary of the invention
[0007] In order to overcome the above-mentioned defects, it would be advantageous for the present invention to provide a high-strength, high-flux composite hollow fiber membrane and a preparation method thereof.
[0008] The technical concept of the present invention is as follows: by adding a solid feeding system and a liquid feeding system to a twin-screw extruder, each component material can be continuously added in proportion, and the materials are heated, melted and meshed by the twin-screw extruder to be modified, so that the high-strength polyethersulfone resin and the polyvinylidene fluoride resin are fully compounded; by adding a melt metering pump to adjust the metering pressure, ß-crystalline polyvinylidene fluoride hollow fiber primary membrane filaments are obtained; the obtained hollow fiber primary membrane filaments are subjected to a post-treatment combining stretching and annealing to obtain a high-strength, large-flux composite hollow fiber membrane.
[0009] To this end, according to one aspect of the present invention, a composite hollow fiber membrane is provided, which is characterized in that it is prepared by a thermotropic phase method and comprises the following components in weight percentage: Polyethersulfone resin: 10-15%, Polyvinylidene fluoride: 45-55%, Inorganic granules: 25-35%, Organic liquid: 5-15%.
[0010] Furthermore, the polyethersulfone resin is a polyether polymer or a polyethersulfone polymer; the polyvinylidene fluoride is a high molecular weight polyvinylidene fluoride, and its melt flow rate is 1-4g / 10min (230℃ / 21.6kg, that is, the test conditions are: temperature at 230℃ and pressure at 21.6kg).
[0011] Furthermore, the high molecular weight polyvinylidene fluoride is a homopolymer of vinylidene fluoride.
[0012] Furthermore, the inorganic granular material is selected from one or a mixture of more than one of calcium carbonate, barium carbonate, magnesium carbonate, copper carbonate, zinc carbonate, silicon dioxide, calcium hydroxide, and magnesium hydroxide.
[0013] Still further, the organic liquid is one or a mixture of more than one selected from benzoates, oxalates, citrates, and phthalates.
[0014] According to another aspect of the present invention, there is provided a method for preparing a composite hollow fiber membrane, comprising the following steps: 1) Solid feeding: Add the solid materials such as polyethersulfone resin, polyvinylidene fluoride and inorganic granules into their respective solid feeding systems, and these solid feeding systems continuously add the solid materials in the feed port of the twin-screw extruder according to the proportion; 2) Liquid feeding: The organic liquid is continuously added to the feed port of the twin-screw extruder in proportion through the liquid feeding system to form a mixed liquid together with the solid material in the twin-screw extruder; 3) Heating, extruding and cooling molding: The mixed liquid is heated to 180-260°C for melting through a twin-screw extruder, pressurized to above 11Mpa through a melt metering pump, and then extruded from the spinning die on the twin-screw extruder. At the same time, the extrusion stretch ratio is controlled to above 9, and air is provided to the hollow part of the spinning die. The mixed liquid is cooled and molded to obtain high-strength, high-content ß-crystalline polyvinylidene fluoride hollow fiber primary membrane fibers; 4) Stretching: Move the hollow fiber nascent membrane filaments in the air for 5 to 10 cm, then stretch them in a water bath at a speed of 45 to 55 m / min, control the temperature at 51 to 70°C, and control the stretching ratio between 2 and 6 times to form a hollow fiber membrane; 5) Annealing: The hollow fiber membrane obtained in step 4) is subjected to annealing treatment at a temperature of 80 to 180° C. for 10 to 120 seconds, and then rolled up; 6) Extraction: The hollow fiber membrane obtained in step 5) is added with an extraction reagent that can react with the inorganic particles and organic liquid in the hollow fiber membrane to extract the inorganic particles and organic liquid in the hollow fiber membrane, and then washed thoroughly with warm water to finally form a composite hollow fiber membrane.
[0015] Furthermore, in the step 3), the heating and melting temperature of the mixed liquid is controlled at 180-220°C.
[0016] Furthermore, in the step 4), the water bath stretching temperature is controlled at 51-60° C., and the stretching ratio is controlled at 2-4 times.
[0017] Furthermore, in the step 5), the annealing temperature is controlled at 100-150° C., and the annealing treatment time is controlled at 50-70 seconds.
[0018] Still further, in step 6), the extraction reagent capable of reacting with the inorganic granular material is various acids or bases such as sulfuric acid, hydrochloric acid, acetic acid, sodium hydroxide or potassium hydroxide; the extraction reagent capable of reacting with the organic solvent is halogenated hydrocarbons, alcohols, and ethers such as dichloroethane, trichloroethane, methanol or ethanol.
[0019] Compared with the prior art, the present invention has the following advantages: 1) The polyethersulfone resin content is more suitable at 10-15%. When it is lower than the lower limit, the expected strength of the membrane cannot be achieved. The higher the polyethersulfone content, the greater the membrane strength. At the same time, the PVDF content decreases and the corrosion resistance of the membrane decreases. When it is higher than the upper limit, although the strength is greatly improved, the pore size distribution of the membrane becomes smaller, which is not conducive to the optimization of the membrane flux and pore size. In general, the polyethersulfone resin content is best when it is 10-15%. At the same time, the ß-crystal PVDF content is expressed as a percentage of the total crystal content. The higher the ß-crystal content, the better the hydrophilicity of the membrane and the greater the flux. Therefore, it is particularly suitable for membrane products with high requirements for membrane strength and membrane flux. When the content of inorganic particles is between 25% and 35%, it can ensure the effective distribution and uniformity of the membrane pore size, ensure the porosity of the membrane filaments, and thus effectively improve the flux and strength of the membrane filaments. If it is below the lower limit, the porosity is low and the flux is reduced. If it is above the upper limit, the number of macropores in the membrane filaments increases and the strength of the membrane filaments decreases. The organic liquid content is 5-15%, which can ensure the overall dispersibility and viscosity of the feed liquid. If it is higher than the upper limit, it is not conducive to the subsequent improvement of melt density and high-ratio stretching, and it is not conducive to the maximum transformation of the polyvinylidene fluoride material itself from the conventional α-crystal form to the ß-crystal form. If it is lower than the lower limit, the powder mixing effect is reduced, the viscosity of the feed liquid is increased, and it is not conducive to the improvement of the membrane pore size distribution and flux. 2) Through the composite processing of two commonly used ultra-microfiltration membrane materials, polyethersulfone resin and polyvinylidene fluoride resin, the high strength of polyethersulfone material and the corrosion resistance of polyvinylidene fluoride material are effectively combined, and the irreversible defects of the two single membrane products are effectively avoided, which greatly optimizes the quality of membrane products and increases the service life of membrane products, which is conducive to the promotion and popularization of large-scale production technology; 3) The twin-screw melt extrusion process with vacuum exhaust replaces the traditional long-term stirring process of the reactor and eliminates the long-term static degassing process of the reactor, which can not only greatly improve the production efficiency, but also effectively avoid the volatilization and decomposition of organic solvents in the formula, which is beneficial to environmental protection and the performance of the membrane fiber is fully guaranteed; 4) By adding a melt metering pump to the modified twin-screw spinning machine, the melt extrusion processing pressure can be increased several times compared to the conventional extruder, so that the melt density is high, the molecular entanglement is good, the melt has better viscoelasticity after extrusion, and a larger die stretch ratio can be achieved, thereby preparing a fiber membrane with a large ß-crystal content. At the same time, the fiber membrane is further stretched at a high ratio to further convert the remaining crystal structure into the ß-crystal, thereby obtaining a hollow fiber primary filament with a high ß-crystal content; 5) Adding a certain amount of inorganic granules as fillers in the melt increases the melt viscosity, which is beneficial to pressurization during extrusion. At the same time, during the later annealing and shaping period, the occupancy characteristics of the inorganic fillers are used to maintain the stability of the ß-crystal form and prevent crystal transformation; At the same time, the low-temperature annealing process is used to ensure that the membrane product has a higher porosity and the membrane pore size remains unchanged. At the same time, the material itself is transformed from the conventional α-crystal form to the ß-crystal form to the greatest extent, with a higher polarity, thereby ensuring that it is more hydrophilic than other crystal forms, so that the filtration membrane fiber has excellent strength and water flux retention.
[0020] These and other aspects of the invention will be more clearly elucidated with reference to the embodiments described hereinafter. DETAILED DESCRIPTION
[0021] The present invention is described in detail below with reference to specific embodiments. Embodiment 1
[0022] The polyethersulfone resin, polyvinylidene fluoride, calcium carbonate and dioctyl phthalate are mixed, wherein the polyethersulfone resin content is 10%, the polyvinylidene fluoride content is 55%, the calcium carbonate content is 25%, and the dioctyl phthalate content is 10%. The above substances are respectively added into the corresponding solid feeding system and liquid feeding system and continuously added into the feeding port of the twin-screw extruder. The slurry is heated and melted (200°C) by the twin-screw extruder, meshed and modified, and pressurized to 12MPa by a melt pump. Then, the slurry is extruded through the spinning die of the twin-screw extruder, i.e., the circular ring mouth, and the extrusion stretch ratio is controlled to be 9. The extruded hollow fiber primary membrane filament moves 10cm in the air and is directly immersed in a water bath of 55°C for stretching. The stretching rate is 55m / min and the stretching ratio is 2. Then, a heat setting treatment, i.e., annealing, is performed for about 55 seconds, and the temperature is controlled at 100°C to obtain a hollow fiber membrane; The obtained hollow fiber membrane was rolled up, bundled into a bundle, immersed in a trichloroethane solution for 2 hours to extract dioctyl phthalate, and then immersed in a 15% hydrochloric acid solution for 4 hours to react and remove calcium carbonate; Then, the membrane was soaked and rinsed in warm water for 4 hours to obtain a porous composite hollow fiber membrane; The composite hollow fiber membrane has an inner diameter of 0.65 mm, an outer diameter of 1.25 mm, a wall thickness of 0.3 mm, a porosity of 86%, a ß-crystal content of 75%, a tensile strength of 15 N, and a pure water pass rate of 1280 L / (m2.h). Embodiment 2
[0023] Mix polyethersulfone resin, polyvinylidene fluoride, propyl benzoate and barium carbonate, wherein the content of polyethersulfone resin is 15%, the content of polyvinylidene fluoride is 45%, the content of calcium carbonate is 35% and the content of butyl benzoate is 5%. The above substances are respectively added into the corresponding solid feeding system and liquid feeding system and continuously added into the feeding port of the twin-screw extruder. The materials are heated and melted (200°C) by the twin-screw extruder, meshed and modified, pressurized to 15MPa by a melt pump, and extruded through the spinning die of the twin-screw extruder, i.e., the circular ring mouth, and the extrusion stretch ratio is controlled to be 10. The extruded product, i.e., the primary hollow fiber membrane, moves 7cm in the air and is directly immersed in a 70°C water bath for stretching. The stretching rate is 45m / min and the stretching ratio is 4. Then, a heat setting treatment is performed for about 60 seconds, and the temperature is controlled at 130°C to obtain a hollow fiber membrane; The obtained hollow fiber membrane was rolled up, bundled into a bundle, immersed in a methanol solution for 2 hours to extract propyl benzoate, and then immersed in a 20% sulfuric acid solution for 3 hours to react with barium carbonate; Then, the membrane was soaked and rinsed in warm water for 4 hours to obtain a porous composite hollow fiber membrane; The composite hollow fiber membrane has an inner diameter of 0.65 mm, an outer diameter of 1.25 mm, a wall thickness of 0.3 mm, a porosity of 80%, a ß-crystal content of 85%, a tensile strength of 17 N, and a pure water pass rate of 1680 L / (m2.h). Embodiment 3
[0024] Mix polyethersulfone resin, polyvinylidene fluoride, tributyl citrate and silicon dioxide, wherein the content of polyethersulfone resin is 12%, the content of polyvinylidene fluoride is 47%, the content of calcium carbonate is 26%, and the content of butyl benzoate is 15%. The above substances are respectively added into the corresponding solid feeding system and liquid feeding system and continuously added into the feeding port of the twin-screw extruder. The materials are heated and melted (200°C) by the twin-screw extruder, meshing and modified. After being pressurized to 16MPa by a melt pump, they are extruded through the spinning die of the twin-screw extruder, i.e., the circular ring mouth. The extrusion stretch ratio is controlled to be 11. The extruded product moves 5cm in the air and is directly immersed in a water bath of 51°C for stretching. The stretching rate is 50m / min and the stretching ratio is controlled to be 6. Then, a heat setting treatment is performed for about 65 seconds, and the temperature is controlled at 150°C to obtain a hollow fiber membrane; The obtained hollow fiber membrane was rolled up, bundled into a bundle, immersed in a dichloroethane solution for 2 hours to extract tributyl citrate, and then immersed in a 25% sodium hydroxide solution for 2 hours to react and remove silica; Then, the membrane was soaked and rinsed in warm water for 4 hours to obtain a porous composite hollow fiber membrane; The composite hollow fiber membrane has an inner diameter of 0.65 mm, an outer diameter of 1.25 mm, a wall thickness of 0.3 mm, a porosity of 90%, a ß-crystal content of 79%, a tensile strength of 20 N, and a pure water pass rate of 1150 L / (m2.h).
[0025] The present invention effectively compounds polyethersulfone resin and polyvinylidene fluoride and uses the TIPS method to prepare a large-scale production process of ß-crystalline polyvinylidene fluoride composite hollow fiber filtration membrane. The method fully utilizes the strength and high performance of polyethersulfone itself and obtains as many ß-crystalline polyvinylidene fluoride composite primary membranes as possible during membrane fiber molding, and then performs low-temperature stretching to further increase the ß-crystalline content and the porosity, so that the product improves production efficiency while ensuring high strength, hydrophilicity and high flux, and the membrane fiber quality is more stable.
[0026] The technical content and technical features of the present invention have been disclosed above, but it is understood that under the creative ideas of the present invention, those skilled in the art can make various changes and improvements to the above structure, including the combination of technical features disclosed or claimed separately here, and other combinations that obviously include these features. These variations and / or combinations all fall within the technical field involved in the present invention and fall within the protection scope of the claims of the present invention.
Claims
1. A composite hollow fiber membrane, characterized in that The thermoplastic phase method is used to prepare the composite material, and the components are as follows in weight percentage: Polyethersulfone resin: 10-15%, Polyvinylidene fluoride: 45-55%, Inorganic granules: 25-35%, Organic liquid: 5-15%.
2. The composite hollow fiber membrane according to claim 1, characterized in that: The polyethersulfone resin is a polyether polymer or a polyethersulfone polymer; the polyvinylidene fluoride is a high molecular weight polyvinylidene fluoride, and its melt flow rate is 1-4g / 10min (230℃ / 21.6kg).
3. The composite hollow fiber membrane according to claim 2, characterized in that: The high molecular weight polyvinylidene fluoride is a homopolymer of vinylidene fluoride.
4. The composite hollow fiber membrane according to claim 1, characterized in that The inorganic granular material is selected from one or a mixture of more than one of calcium carbonate, barium carbonate, magnesium carbonate, copper carbonate, zinc carbonate, silicon dioxide, calcium hydroxide and magnesium hydroxide.
5. The composite hollow fiber membrane according to claim 1, characterized in that: The organic liquid is selected from benzoic acid esters, oxalic acid esters, citrate esters, phthalic acid esters or a mixture of more than one thereof.
6. A method for preparing a composite hollow fiber membrane according to any one of claims 1 to 5, characterized in that: The steps include: 1) Solid feeding: Add the solid materials such as polyethersulfone resin, polyvinylidene fluoride and inorganic granules into their respective solid feeding systems, and these solid feeding systems continuously add the solid materials in the feed port of the twin-screw extruder according to the proportion; 2) Liquid feeding: The organic liquid is continuously added to the feed port of the twin-screw extruder in proportion through the liquid feeding system to form a mixed liquid together with the solid material in the twin-screw extruder; 3) Heating, extruding and cooling molding: The mixed liquid is heated to 180-260°C for melting through a twin-screw extruder, pressurized to above 11Mpa through a melt metering pump, and then extruded from the spinning die on the twin-screw extruder. At the same time, the extrusion stretch ratio is controlled to above 9, and air is provided to the hollow part of the spinning die. The mixed liquid is cooled and molded to obtain high-strength, high-content ß-crystalline polyvinylidene fluoride hollow fiber primary membrane fibers; 4) Stretching: Move the hollow fiber nascent membrane filaments in the air for 5 to 10 cm, then stretch them in a water bath at a speed of 45 to 55 m / min, control the temperature at 51 to 70°C, and control the stretching ratio between 2 and 6 times to form a hollow fiber membrane; 5) Annealing: The hollow fiber membrane obtained in step 4) is subjected to annealing treatment at a temperature of 80 to 180° C. for 10 to 120 seconds, and then rolled up; 6) Extraction: The hollow fiber membrane obtained in step 5) is added with an extraction reagent that can react with the inorganic particles and organic liquid in the hollow fiber membrane to extract the inorganic particles and organic liquid in the hollow fiber membrane, and then washed thoroughly with warm water to finally form a composite hollow fiber membrane.
7. The method for preparing a composite hollow fiber membrane according to claim 6, characterized in that: In the step 3), the heating and melting temperature of the mixed liquid is controlled at 180-220°C.
8. The method for preparing a composite hollow fiber membrane according to claim 6, characterized in that: In the step 4), the water bath stretching temperature is controlled at 51-60° C., and the stretching ratio is controlled at 2-4 times.
9. The method for preparing a composite hollow fiber membrane according to claim 6, characterized in that: In the step 5), the annealing temperature is controlled at 100-150° C., and the annealing treatment time is controlled at 50-70 seconds.
10. The method for preparing a composite hollow fiber membrane according to claim 6, characterized in that: In step 6), the extraction reagent capable of reacting with the inorganic granular material is sulfuric acid, hydrochloric acid, acetic acid, sodium hydroxide or potassium hydroxide; the extraction reagent capable of reacting with the organic solvent is dichloroethane, trichloroethane, methanol or ethanol.
Citation Information
Patent Citations
Preparation method for beta crystal phase polyvinylidene fluoride hollow fiber porous membrane
CN101342468A
Polyvinylidene fluoride hollow fiber film and preparation method thereof
CN101590374A
Polyvinylidene fluoride-polyether sulfone blended hollow fiber membrane and thermally induced phase separation preparation method
CN102219969A
Polyether sulfone hollow fiber filter membrane and its preparation method
CN102397759A
Polyvinylidene fluoride hollow fiber membrane and preparation method thereof
CN111644074A