Preparation method of polysulfone hollow fiber membrane with gradient pore structure
Through the polysulfone hollow fiber membrane with gradient pore structure, the problem of the pore size of existing membrane materials being unregulated and prone to blockage in virus filtration is solved, and efficient virus separation and membrane performance are achieved.
Patent Information
- Application Number
- CN202410915530.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-22
AI Technical Summary
During the virus filtration process, existing membrane materials have an uncontrollable pore size, and an "trade-off" effect, which leads to low separation efficiency and easy blockage, making it difficult to meet the needs of complex biological systems.
Polysulfone hollow fiber membranes with gradient pore structures are composed of outer dense membrane structures and inner porous membrane structures. By regulating the formulation composition of the outer and inner cast film liquids and the temperature difference of core liquids, the pore size is achieved from the inner layer. Gradually smaller the outer layer to avoid membrane blockage and improve separation efficiency.
The step by step separation of virus particles is achieved, the permeability and separation performance of the membrane is improved, the membrane blockage is avoided, and the separation efficiency and stability are significantly improved.
Smart Images

Figure CN118988014A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of membrane materials, and in particular to a polysulfone hollow fiber membrane with a gradient pore structure and a preparation method thereof. Background Art
[0002] Virus contamination is a common threat to biological products produced by human or animal cell lines. At the same time, virus contamination can occur at any stage of the entire process of biological product production, ultimately leading to global safety incidents. Therefore, the control of biological product virus safety is of great significance to ensure the safety and effectiveness of drugs. Due to the high price and disposable nature of virus removal filters, it has become an important link in increasing the cost of biological products.
[0003] Virus filters can efficiently remove enveloped and non-enveloped viruses through size screening. They are not affected by the differences in the physicochemical properties of different viruses and the interactions regulated by operating conditions. They have been proven to provide robust performance in the blood products processing industry. However, membrane treatment technology still faces many challenges in practical applications, such as the uncontrollable pore size of membrane materials and the "trade-off" effect between permeate flux and retention performance. These shortcomings are more obvious when applied to virus removal systems. This is because solutions such as cell culture fluids belong to complex biological systems with complex components, close molecular weights between components, and a large number of interactions. The solution has high viscosity, which leads to a large number of components being enriched on the membrane surface to form membrane contamination. The membrane pores are easily blocked during the separation process, thus placing higher requirements on the membrane separation efficiency.
[0004] After searching, the Chinese patent with announcement number CN113842792 discloses an asymmetric PES filter membrane for virus removal and its preparation method. The flat membrane body includes a pre-filtration layer and a separation layer for intercepting viruses. The other side of the pre-filtration layer and the other side of the separation layer are transitioned with continuous fibers and formed in one piece. The PES filter membrane has a strong interception effect on small viruses with a particle size of 20nm or more, but the filtration load is low, which is difficult to meet the use requirements of large-scale liquid filtration.
[0005] Therefore, there is an urgent need for a gradient pore structure polysulfone hollow fiber membrane and a preparation method thereof. Summary of the invention
[0006] The purpose of the present invention is to solve the defects in the prior art and to propose a polysulfone hollow fiber membrane with a gradient pore structure and a preparation method thereof.
[0007] According to one aspect of the present invention, a polysulfone hollow fiber membrane with a gradient pore structure is provided.
[0008] A polysulfone hollow fiber membrane with a gradient pore structure consists of an outer dense membrane structure and an inner porous membrane structure, wherein there is no obvious interface between the outer dense membrane structure and the inner porous membrane structure, wherein the structures of the dense layer and the porous layer are both sponge pore structures.
[0009] The pore size of the outer dense membrane structure is 0.005-0.02 μm, the thickness of the outer dense membrane structure is 30-50 μm, and the surface porosity is 10%-30%.
[0010] The pore size of the inner porous membrane structure is 0.04-0.08 μm, the thickness of the inner porous membrane structure is 40-70 μm, and the inner surface porosity is 40%-60%.
[0011] The polysulfone material is at least one of polyethersulfone, polysulfone, sulfonated polysulfone and sulfonated polyethersulfone, and has a weight average molecular weight of 60,000-90,000.
[0012] The hollow fiber membrane is prepared by taking polysulfone polymer as raw material, and then adding a first organic solvent, a second organic solvent, a pore-forming agent and a small molecule additive.
[0013] Wherein, the first organic solvent is at least one of diethyl phthalate, triacetin, methyl benzoate, ethyl benzoate, triethyl phosphate and trimethyl phosphate.
[0014] The second organic solvent includes at least one of dimethylformamide, dimethylacetamide, N-methylpyrrolidone and N,N-diethylformamide.
[0015] The pore former is at least one of polyvinyl pyrrolidone (PVP-K30, PVP-K60 or PVP-K90), polyvinyl alcohol and LiCl.
[0016] The small molecule additive is at least one of ethylene glycol, propylene glycol, n-butanol, diethylene glycol, triethylene glycol, polyethylene glycol 200 and polyethylene glycol 400.
[0017] In order to obtain a hollow fiber membrane with a gradient pore structure, the present invention selects different solvents to prepare the surface casting liquid and the inner layer casting liquid respectively, so that when the casting liquid is solidified into a membrane, due to the different exchange rates between the solvent in the casting liquid and the non-solvent water in the coagulation bath or the core liquid, different pore sizes are finally produced in the inner and outer layers of the membrane. Among them, the solubility parameter of the first solvent in the surface casting liquid with water is greater than 6MPa 0.5, and the temperature difference between the casting liquid and the coagulation bath is greater than 40°C, so delayed phase separation occurs in the solidification process, the double diffusion rate of the first solvent and water is slow, and a dense cortex is easily formed on the surface of the membrane; while the solubility parameters of the second solvent in the inner casting liquid are close to those of water, and the temperatures of the casting liquid and the core liquid are close, instantaneous phase separation occurs in the solidification process, and a large-pore sponge pore structure is easily formed in the inner layer of the membrane, and the cross-sectional pore size of the hollow fiber membrane finally prepared shows a gradient change.
[0018] According to another aspect of the present invention, a method for preparing a polysulfone hollow fiber membrane with a gradient pore structure is also provided.
[0019] A method for preparing a polysulfone hollow fiber membrane with a gradient pore structure comprises the following steps:
[0020] (1) Preparation of surface casting solution: putting a polymer, a first organic solvent, a pore former and a small molecule additive into a stirring kettle, stirring at 120-150° C. for 24 hours to form a homogeneous solution, then cooling to 80-90° C. and continuing stirring for 6 hours, standing to degas, and obtaining a surface casting solution, wherein the mass fractions of the polymer, the first organic solvent, the pore former and the small molecule additive are 20-26%, 60-70%, 5-10% and 2-7%, respectively;
[0021] (2) Preparation of inner layer casting solution: Put the polymer, the second organic solvent, the pore former and the small molecule additive into a stirring kettle, stir at 80-90° C. for 24 h to form a homogeneous solution, then cool to 40-60° C. and continue stirring for 6 h, let stand to degas, and obtain the surface casting solution, wherein the mass fractions of the polymer, the second organic solvent, the pore former and the small molecule additive are 15-19%, 62-72%, 5-10% and 2-7%, respectively;
[0022] (3) core liquid preparation: the core liquid comprises a second organic solvent and water, the mass fractions of the second organic solvent and water are 45-60% and 40%-55% respectively, and the core liquid temperature is controlled at 40-70° C.;
[0023] (4) Spinning: The surface casting liquid, the inner casting liquid and the core liquid are respectively passed through respective metering pumps and extruded through a three-channel spinneret to form a fiber tubular liquid surface. The casting liquid pressure is 0.1-0.3 MPa. Before entering the coagulation bath, the liquid film passes through an air region with a height of 5-30 cm and then enters the coagulation bath to undergo phase inversion and solidification to form a film, thereby obtaining a primary hollow fiber membrane. The coagulation bath is water and the coagulation bath temperature is 30-50° C.
[0024] (5) Rinsing: Soak the nascent hollow fiber membrane obtained in step (4) in hot water at 60-70° C. for 24 h to completely remove the pore-forming agent and solvent remaining in the membrane, thereby obtaining a hollow fiber membrane with a gradient pore structure.
[0025] Compared with the prior art, the advantages of the present invention are:
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The present invention provides a method for preparing a polysulfone hollow fiber membrane with a gradient pore structure, which adjusts the formula composition of the outer layer casting liquid and the inner layer casting liquid, and utilizes the temperature difference between the core liquid and the coagulation bath to make the phase separation rate of the outer layer casting liquid slower than that of the inner layer casting liquid, thereby achieving the pore size of the hollow fiber membrane gradually decreasing from the inner layer to the outer layer, and the thickness of the outer layer and the inner layer can be arbitrarily adjusted;
[0028] (2) When the membrane material prepared by the present invention is used for virus removal filtration, internal pressure filtration is adopted, and the raw material liquid enters from the large pore side. The gradient pores are conducive to the step-by-step separation of components with similar molecular weights, thereby improving the separation efficiency. Therefore, the virus particles in the solution can be separated step by step through the gradient pore size inside the membrane, while avoiding membrane clogging, thereby simultaneously achieving the improvement of membrane permeability and separation performance;
[0029] (3) The outer layer and the inner layer of the double-layer hollow fiber membrane prepared by the present invention are both made of the same material, and there is no obvious interface between the two, so that the gradient pore structure hollow fiber membrane provided by the present invention has good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.
[0031] Figure 1 This is a cross-sectional SEM schematic diagram of the hollow fiber membrane prepared in Example 2 of the present invention;
[0032] Figure 2 This is a SEM schematic diagram of the inner and outer surfaces of the hollow fiber membrane prepared in Example 2 of the present invention;
[0033] Figure 3 This is a cross-sectional SEM schematic diagram of the hollow fiber membrane prepared in Comparative Example 1 of the present invention;
[0034] Figure 4 This is a schematic SEM diagram of the inner and outer surfaces of the hollow fiber membrane prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0036] The invention provides a polysulfone hollow fiber membrane with a gradient pore structure. The hollow fiber membrane consists of an outer dense membrane structure and an inner porous membrane structure. There is no obvious interface between the outer dense membrane structure and the inner porous membrane structure. The structures of the dense layer and the porous layer are both sponge pore structures.
[0037] The pore size of the outer dense membrane structure is 0.005-0.02 μm, the thickness of the outer dense membrane structure is 30-50 μm, and the surface porosity is 10%-30%.
[0038] The pore size of the inner porous membrane structure is 0.04-0.08 μm, the thickness of the inner porous membrane structure is 40-70 μm, and the inner surface porosity is 40%-60%.
[0039] The polysulfone material is at least one of polyethersulfone, polysulfone, sulfonated polysulfone and sulfonated polyethersulfone, and has a weight average molecular weight of 60,000-90,000.
[0040] The hollow fiber membrane is prepared by taking polysulfone polymer as raw material, and then adding a first organic solvent, a second organic solvent, a pore-forming agent and a small molecule additive.
[0041] Wherein, the first organic solvent is at least one of diethyl phthalate, triacetin, methyl benzoate, ethyl benzoate, triethyl phosphate and trimethyl phosphate.
[0042] The second organic solvent includes at least one of dimethylformamide, dimethylacetamide, N-methylpyrrolidone and N,N-diethylformamide.
[0043] The pore former is at least one of polyvinyl pyrrolidone (PVP-K30, PVP-K60 or PVP-K90), polyvinyl alcohol and LiCl.
[0044] The small molecule additive is at least one of ethylene glycol, propylene glycol, n-butanol, diethylene glycol, triethylene glycol, polyethylene glycol 200 and polyethylene glycol 400.
[0045] The present invention also provides a method for preparing a polysulfone hollow fiber membrane with a gradient pore structure, comprising the following steps:
[0046] (1) Preparation of surface casting solution: Put the polymer, the first organic solvent, the pore former and the small molecule additive into a stirring kettle, stir at 120-150° C. for 24 hours to form a homogeneous solution, then cool to 80-90° C. and continue stirring for 6 hours, stand for degassing, and obtain a surface casting solution, wherein the mass fractions of the polymer, the first organic solvent, the pore former and the small molecule additive are 20-27%, 60-70%, 5-10% and 2-7%, respectively;
[0047] (2) Preparation of inner layer casting solution: Put the polymer, the second organic solvent, the pore former and the small molecule additive into a stirring kettle, stir at 80-90° C. for 24 h to form a homogeneous solution, then cool to 40-60° C. and continue stirring for 6 h, let stand to degas, and obtain the surface casting solution, wherein the mass fractions of the polymer, the second organic solvent, the pore former and the small molecule additive are 15-19%, 62-72%, 5-10% and 2-7%, respectively;
[0048] (3) core liquid preparation: the core liquid comprises a second organic solvent and water, the mass fractions of the second organic solvent and water are 35-60% and 40%-65% respectively, and the core liquid temperature is controlled at 40-70° C.;
[0049] (4) Spinning: The surface casting liquid, the inner casting liquid and the core liquid are respectively passed through respective metering pumps and extruded through a three-channel spinneret to form a fiber tubular liquid surface. The casting liquid pressure is 0.1-0.3 MPa. Before entering the coagulation bath, the liquid film passes through an air region with a height of 5-30 cm and then enters the coagulation bath to undergo phase inversion and solidification to form a film, thereby obtaining a primary hollow fiber membrane. The coagulation bath is water and the coagulation bath temperature is 30-50° C.
[0050] (5) Rinsing: Soak the nascent hollow fiber membrane obtained in step (4) in hot water at 60-70° C. for 24 h to completely remove the pore-forming agent and solvent remaining in the membrane, thereby obtaining a hollow fiber membrane with a gradient pore structure.
[0051] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0052] Embodiment 1:
[0053] A method for preparing a polysulfone hollow fiber membrane with a gradient pore structure comprises the following steps:
[0054] (1) Preparation of surface casting solution: polysulfone, sulfonated polysulfone, triethyl phosphate, PVP-K90 and polyethylene glycol 200 are placed in a stirring tank, stirred at 140° C. for 24 h to form a homogeneous solution, then cooled to 80° C. and stirred for 6 h, and allowed to stand for degassing to obtain a surface casting solution, wherein the mass fractions of the polysulfone, sulfonated polysulfone, first organic solvent, pore former and small molecule additive are 24%, 2%, 62%, 7% and 5%, respectively;
[0055] (2) Preparation of inner layer casting solution: polysulfone, sulfonated polysulfone, N,N-dimethylacetamide, PVP-K30 and triethylene glycol are placed in a stirring kettle, stirred at 90°C for 24 hours to form a homogeneous solution, then cooled to 50°C and stirred for 6 hours, and allowed to stand for degassing to obtain a surface casting solution, wherein the mass fractions of the polysulfone, sulfonated polysulfone, second organic solvent, pore former and small molecule additive are 15%, 2%, 67%, 9% and 7%, respectively;
[0056] (3) core liquid preparation: the core liquid comprises N,N-dimethylacetamide and water, the mass fractions of N,N-dimethylacetamide and water are 45% and 55% respectively, and the core liquid temperature is controlled at 60°C;
[0057] (4) Spinning: The surface casting liquid, the inner casting liquid and the core liquid are respectively passed through respective metering pumps and extruded through a three-channel spinneret to form a fiber tubular liquid surface. The casting liquid pressure is 0.1 MPa. Before entering the coagulation bath, the liquid film passes through an air region with a height of 15 cm and then enters the coagulation bath to undergo phase inversion and solidification to form a membrane, thereby obtaining a primary hollow fiber membrane. The coagulation bath is water and the coagulation bath temperature is 40°C.
[0058] (5) Rinsing: Soak the nascent hollow fiber membrane obtained in step (4) in hot water at 60° C. for 24 h to completely remove the pore-forming agent and solvent remaining in the membrane, thereby obtaining a hollow fiber membrane with a gradient pore structure.
[0059] Embodiment 2:
[0060] A method for preparing a polysulfone hollow fiber membrane with a gradient pore structure comprises the following steps:
[0061] (1) Preparation of surface casting solution: polysulfone, sulfonated polysulfone, triethyl phosphate, PVP-K90 and polyethylene glycol 200 are placed in a stirring tank, stirred at 140° C. for 24 hours to form a homogeneous solution, then cooled to 80° C. and stirred for 6 hours, and allowed to stand for degassing to obtain a surface casting solution, wherein the mass fractions of the polysulfone, sulfonated polysulfone, first organic solvent, pore former and small molecule additive are 25%, 2%, 59%, 9% and 5%, respectively;
[0062] (2) Preparation of inner layer casting solution: polysulfone, sulfonated polysulfone, N,N-dimethylacetamide, PVP-K30 and triethylene glycol are placed in a stirring kettle, stirred at 90°C for 24 hours to form a homogeneous solution, then cooled to 50°C and stirred for 6 hours, and allowed to stand for degassing to obtain a surface casting solution, wherein the mass fractions of the polysulfone, sulfonated polysulfone, second organic solvent, pore former and small molecule additive are 16%, 2%, 64%, 11% and 7%, respectively;
[0063] (3) core liquid preparation: the core liquid comprises N,N-dimethylacetamide and water, the mass fractions of N,N-dimethylacetamide and water are 45% and 55% respectively, and the core liquid temperature is controlled at 60°C;
[0064] (4) Spinning: The surface casting liquid, the inner casting liquid and the core liquid are respectively passed through respective metering pumps and extruded through a three-channel spinneret to form a fiber tubular liquid surface. The casting liquid pressure is 0.1 MPa. Before entering the coagulation bath, the liquid film passes through an air region with a height of 15 cm and then enters the coagulation bath to undergo phase inversion and solidification to form a membrane, thereby obtaining a primary hollow fiber membrane. The coagulation bath is water and the coagulation bath temperature is 40°C.
[0065] (5) Rinsing: Soak the nascent hollow fiber membrane obtained in step (4) in hot water at 60° C. for 24 h to completely remove the pore-forming agent and solvent remaining in the membrane, thereby obtaining a hollow fiber membrane with a gradient pore structure, such as Figure 1-2 shown.
[0066] Embodiment 3:
[0067] A method for preparing a polysulfone hollow fiber membrane with a gradient pore structure comprises the following steps:
[0068] (1) Preparation of surface casting solution: polysulfone, sulfonated polysulfone, ethyl benzoate, PVP-K90 and polyethylene glycol 200 are placed in a stirring tank, stirred at 140° C. for 24 h to form a homogeneous solution, then cooled to 80° C. and stirred for 6 h, and allowed to stand for degassing to obtain a surface casting solution, wherein the mass fractions of the polysulfone, sulfonated polysulfone, first organic solvent, pore former and small molecule additive are 24%, 2%, 62%, 7% and 5%, respectively;
[0069] (2) Preparation of inner layer casting solution: polysulfone, sulfonated polysulfone, N,N-dimethylacetamide, PVP-K30 and polyethylene glycol 400 are placed in a stirring tank, stirred at 90°C for 24 hours to form a homogeneous solution, then cooled to 50°C and stirred for 6 hours, and allowed to stand for degassing to obtain a surface casting solution, wherein the mass fractions of the polysulfone, sulfonated polysulfone, second organic solvent, pore former and small molecule additive are 15%, 2%, 67%, 9% and 7%, respectively;
[0070] (3) core liquid preparation: the core liquid comprises N,N-dimethylacetamide and water, the mass fractions of N,N-dimethylacetamide and water are 45% and 55% respectively, and the core liquid temperature is controlled at 60°C;
[0071] (4) Spinning: The surface casting liquid, the inner casting liquid and the core liquid are respectively passed through respective metering pumps and extruded through a three-channel spinneret to form a fiber tubular liquid surface. The casting liquid pressure is 0.1 MPa. Before entering the coagulation bath, the liquid film passes through an air region with a height of 15 cm and then enters the coagulation bath to undergo phase inversion and solidification to form a membrane, thereby obtaining a primary hollow fiber membrane. The coagulation bath is water and the coagulation bath temperature is 40°C.
[0072] (5) Rinsing: Soak the nascent hollow fiber membrane obtained in step (4) in hot water at 60° C. for 24 h to completely remove the pore-forming agent and solvent remaining in the membrane, thereby obtaining a hollow fiber membrane with a gradient pore structure.
[0073] Embodiment 4:
[0074] A method for preparing a polysulfone hollow fiber membrane with a gradient pore structure comprises the following steps:
[0075] (1) Preparation of surface casting solution: polysulfone, sulfonated polysulfone, ethyl benzoate, PVP-K90 and polyethylene glycol 200 are placed in a stirring tank, stirred at 140° C. for 24 h to form a homogeneous solution, then cooled to 80° C. and stirred for 6 h, and allowed to stand for degassing to obtain a surface casting solution, wherein the mass fractions of the polysulfone, sulfonated polysulfone, first organic solvent, pore former and small molecule additive are 24%, 2%, 62%, 7% and 5%, respectively;
[0076] (2) Preparation of inner layer casting solution: polysulfone, sulfonated polysulfone, N,N-dimethylacetamide, PVP-K30 and polyethylene glycol 400 are placed in a stirring tank, stirred at 90°C for 24 hours to form a homogeneous solution, then cooled to 50°C and stirred for 6 hours, and allowed to stand for degassing to obtain a surface casting solution, wherein the mass fractions of the polysulfone, sulfonated polysulfone, second organic solvent, pore former and small molecule additive are 15%, 2%, 67%, 9% and 7%, respectively;
[0077] (3) core liquid preparation: the core liquid comprises N,N-dimethylacetamide and water, the mass fractions of N,N-dimethylacetamide and water are 40% and 60% respectively, and the core liquid temperature is controlled at 60°C;
[0078] (4) Spinning: The surface casting liquid, the inner casting liquid and the core liquid are respectively passed through respective metering pumps and extruded through a three-channel spinneret to form a fiber tubular liquid surface. The casting liquid pressure is 0.1 MPa. Before entering the coagulation bath, the liquid film passes through an air region with a height of 15 cm and then enters the coagulation bath to undergo phase inversion and solidification to form a membrane, thereby obtaining a primary hollow fiber membrane. The coagulation bath is water and the coagulation bath temperature is 40°C.
[0079] (5) Rinsing: Soak the nascent hollow fiber membrane obtained in step (4) in hot water at 60° C. for 24 h to completely remove the pore-forming agent and solvent remaining in the membrane, thereby obtaining a hollow fiber membrane with a gradient pore structure.
[0080] Embodiment 5:
[0081] A method for preparing a polysulfone hollow fiber membrane with a gradient pore structure comprises the following steps:
[0082] (1) Preparation of surface casting solution: polysulfone, ethyl benzoate, PVP-K90 and polyethylene glycol 200 are placed in a stirring tank, stirred at 140° C. for 24 h to form a homogeneous solution, then cooled to 80° C. and stirred for 6 h, and allowed to stand for degassing to obtain a surface casting solution, wherein the mass fractions of the polysulfone, the first organic solvent, the pore-forming agent and the small molecule additive are 24%, 64%, 7% and 5%, respectively;
[0083] (2) Preparation of inner layer casting solution: polysulfone, N,N-dimethylacetamide, PVP-K30 and polyethylene glycol 400 are placed in a stirring kettle, stirred at 90°C for 24 hours to form a homogeneous solution, then cooled to 50°C and stirred for 6 hours, and allowed to stand for degassing to obtain a surface casting solution, wherein the mass fractions of the polysulfone, the second organic solvent, the pore former and the small molecule additive are 15%, 69%, 9% and 7%, respectively;
[0084] (3) core liquid preparation: the core liquid comprises N,N-dimethylacetamide and water, the mass fractions of N,N-dimethylacetamide and water are 40% and 60% respectively, and the core liquid temperature is controlled at 60°C;
[0085] (4) Spinning: The surface casting liquid, the inner casting liquid and the core liquid are respectively passed through respective metering pumps and extruded through a three-channel spinneret to form a fiber tubular liquid surface. The casting liquid pressure is 0.1 MPa. Before entering the coagulation bath, the liquid film passes through an air region with a height of 15 cm and then enters the coagulation bath to undergo phase inversion and solidification to form a membrane, thereby obtaining a primary hollow fiber membrane. The coagulation bath is water and the coagulation bath temperature is 40°C.
[0086] (5) Rinsing: Soak the nascent hollow fiber membrane obtained in step (4) in hot water at 60° C. for 24 h to completely remove the pore-forming agent and solvent remaining in the membrane, thereby obtaining a hollow fiber membrane with a gradient pore structure.
[0087] Comparative Example 1:
[0088] (1) Preparation of casting solution: polysulfone, sulfonated polysulfone, triethyl phosphate, PVP-K90 and polyethylene glycol 200 are placed in a stirring tank, stirred at 140°C for 24 hours to form a homogeneous solution, then cooled to 80°C and stirred for 6 hours, and allowed to stand for degassing to obtain a casting solution. The mass fractions of the polysulfone, sulfonated polysulfone, organic solvent, pore former and small molecule additive are 24%, 2%, 62%, 7% and 5% respectively;
[0089] (2) Preparation of core liquid: The core liquid comprises triethyl phosphate and water, the mass fractions of triethyl phosphate and water are 45% and 55% respectively, and the core liquid temperature is controlled at 60° C.;
[0090] (3) Spinning: The casting liquid and the core liquid are respectively passed through their respective metering pumps and extruded through a double-channel spinneret to form a fiber tubular liquid surface. The casting liquid pressure is 0.1 MPa. Before entering the coagulation bath, the liquid film passes through an air region with a height of 15 cm and then enters the coagulation bath to undergo phase inversion and solidification to form a membrane, thereby obtaining a primary hollow fiber membrane. The coagulation bath is water and the coagulation bath temperature is 40°C.
[0091] (4) Rinsing: Soak the nascent hollow fiber membrane obtained in step (3) in hot water at 60° C. for 24 h to completely remove the pore-forming agent and solvent remaining in the membrane, thereby obtaining a hollow fiber membrane such as Figure 3-4 shown.
[0092] Comparative Example 2:
[0093] (1) Preparation of casting solution: polysulfone, sulfonated polysulfone, N,N-dimethylacetamide, PVP-K90 and polyethylene glycol 200 are placed in a stirring kettle, stirred at 90°C for 24 hours to form a homogeneous solution, then cooled to 60°C and stirred for 6 hours, and allowed to stand for degassing to obtain a casting solution. The mass fractions of the polysulfone, sulfonated polysulfone, organic solvent, pore former and small molecule additive are 20%, 2%, 66%, 7% and 5% respectively;
[0094] (2) core liquid preparation: the core liquid comprises N,N-dimethylacetamide and water, the mass fractions of N,N-dimethylacetamide and water are 45% and 55% respectively, and the core liquid temperature is controlled at 60°C;
[0095] (3) Spinning: The casting liquid and the core liquid are respectively passed through their respective metering pumps and extruded through a double-channel spinneret to form a fiber tubular liquid surface. The casting liquid pressure is 0.1 MPa. Before entering the coagulation bath, the liquid film passes through an air region with a height of 15 cm and then enters the coagulation bath to undergo phase inversion and solidification to form a membrane, thereby obtaining a primary hollow fiber membrane. The coagulation bath is water and the coagulation bath temperature is 40°C.
[0096] (4) Rinsing: Soak the nascent hollow fiber membrane obtained in step (3) in hot water at 60° C. for 24 h to completely remove the pore-forming agent and solvent remaining in the membrane, thereby obtaining a hollow fiber membrane.
[0097] Characterization and membrane performance testing:
[0098] (1) Pure water flux test: Equal amounts of membrane fibers were taken from Examples 1-5 and Comparative Examples 1-2 to prepare membrane modules of the same area. The membrane area of the module was 0.02 m 2 Before the test, anhydrous ethanol was injected into the assembly to ensure that the membrane fibers were completely wetted. The pure water flux of the assembly was tested using a homemade tangential flow filtration device with an operating pressure of 0.1 MPa. Pure water flux (LMH) = 60 × permeate volume (L) / membrane area (m 2 ) / collection time (min)
[0099] (2) Mechanical properties test: The strength of the membrane filament was tested using an electronic universal testing machine at a test speed of 25 mm / min and at room temperature.
[0100] Table 1 Pure water flux and mechanical properties of membrane materials prepared in Examples and Comparative Examples
[0101] Pure water flux (LMH) Tension(N) Example 1 640 1.40 Example 2 620 1.45 Example 3 630 1.50 Example 4 655 1.35 Example 5 610 1.55 Comparative Example 1 420 1.45 Comparative Example 2 470 1.20
[0102] As can be seen from Table 1, the pure water flux of the double-layer gradient pore hollow fiber membranes prepared in Examples 1-5 is higher than that of the single-layer membrane in the comparative example, indicating that the gradient pore structure can indeed significantly increase the permeability of the membrane.
[0103] (3) Retention performance test: The retention performance of the membrane fibers of the embodiment and the comparative example was tested using a solution of polystyrene microspheres of different sizes as the raw material solution. The filtration method was tangential flow filtration, the operating pressure was 0.10 MPa, and the concentrations of the raw material solution and the permeate were detected by an ultraviolet spectrophotometer at a detection wavelength of 210 nm. The microsphere retention rate (%) = (1-permeate absorbance / stock solution absorbance) × 100%. The results are shown in Table 2.
[0104] Table 2 Separation performance of membrane materials prepared in Examples and Comparative Examples
[0105]
[0106]
[0107] As shown in Table 2, the retention rates of the hollow fiber membranes with gradient pore structures prepared in the examples for polystyrene microspheres are all greater than 90%, while the retention performance of the membrane materials prepared in the comparative examples is poor, indicating that the design of the gradient pore structure has obvious advantages in separation performance.
[0108] (4) Virus removal performance test: Bacteriophage MS-2ATCC 15597-B1 (MS-2 bacteriophage, particle size about 25 nm) was added to sterile distilled water to prepare a virus removal solution with a concentration of about 1.0 × 10 7 The test stock solution contained MS-2 bacteriophage at a concentration of PFU / mL. The test stock solution was passed through an area of 0.02 m 2 The components were filtered at a temperature of 25°C and a filtration differential pressure of 100 kPa. Based on the method of Overlay agar assay, Standard Method 9211-D (APHA, 1998, Standard methods for the examination of water and wastewater, 18th ed.), 1 mL of the diluted stock solution and filtrate were inoculated in the test culture dish, and the plaques were counted to obtain the concentration of MS-2 phage before and after the filtration test. The virus removal rate was calculated as follows: Removal rate % = (1-phage concentration in the permeate / phage concentration in the stock solution) × 100%, and the logarithmic removal rate LRV2 means -1 gX = 2, X = 0.01, indicating that the phage concentration in the permeate is 1%. The results are shown in Table 3.
[0109] Table 3 Virus removal performance of membrane materials prepared in Examples and Comparative Examples
[0110]
[0111] It can be seen from Table 3 that the hollow fiber membrane prepared by the present invention can effectively remove viruses.
[0112] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a polysulfone hollow fiber membrane with a gradient pore structure, It is characterized in that The following steps are involved: (1) Preparation of surface casting solution: putting a polymer, a first organic solvent, a pore former and a small molecule additive into a stirring kettle, stirring at 120-150° C. for 24 hours to form a homogeneous solution, then cooling to 80-90° C. and continuing stirring for 6 hours, standing to degas, and obtaining a surface casting solution, wherein the mass fractions of the polymer, the first organic solvent, the pore former and the small molecule additive are 20-26%, 60-70%, 5-10% and 2-7%, respectively; (2) Preparation of inner layer casting solution: Put the polymer, the second organic solvent, the pore former and the small molecule additive into a stirring kettle, stir at 80-90° C. for 24 h to form a homogeneous solution, then cool to 40-60° C. and continue stirring for 6 h, let stand to degas, and obtain the surface casting solution, wherein the mass fractions of the polymer, the second organic solvent, the pore former and the small molecule additive are 15-19%, 62-72%, 5-10% and 2-7%, respectively; (3) core liquid preparation: the core liquid comprises a second organic solvent and water, the mass fractions of the second organic solvent and water are 45-60% and 40%-55% respectively, and the core liquid temperature is controlled at 40-70° C.; (4) Spinning: The surface casting liquid, the inner casting liquid and the core liquid are respectively passed through respective metering pumps and extruded through a three-channel spinneret to form a fiber tubular liquid surface. The casting liquid pressure is 0.1-0.3 MPa. Before entering the coagulation bath, the liquid film passes through an air region with a height of 5-30 cm and then enters the coagulation bath to undergo phase inversion and solidification to form a film, thereby obtaining a primary hollow fiber membrane. The coagulation bath is water and the coagulation bath temperature is 30-50° C. (5) Rinsing: Soak the nascent hollow fiber membrane obtained in step (4) in hot water at 60-70° C. for 24 h to completely remove the pore-forming agent and solvent remaining in the membrane, thereby obtaining a hollow fiber membrane with a gradient pore structure.
2. The method for preparing the gradient pore structure polysulfone hollow fiber membrane according to claim 1, It is characterized in that The polymer in step (1) is at least one of polyethersulfone, polysulfone, sulfonated polysulfone and sulfonated polyethersulfone, and has a weight average molecular weight of 60,000-90,000.
3. The method for preparing the gradient pore structure polysulfone hollow fiber membrane according to claim 1, It is characterized in that In step (1), the first organic solvent is at least one of diethyl phthalate, triacetin, methyl benzoate, ethyl benzoate, triethyl phosphate and trimethyl phosphate; In step (2), the second organic solvent is at least one of dimethylformamide, dimethylacetamide, N-methylpyrrolidone and N,N-diethylformamide.
4. The method for preparing the gradient pore structure polysulfone hollow fiber membrane according to claim 1, It is characterized in that The pore-forming agent in step (1) and step (2) is at least one of polyvinyl pyrrolidone, polyvinyl alcohol and LiCl; The small molecule additive is at least one of ethylene glycol, propylene glycol, n-butanol, diethylene glycol, triethylene glycol, polyethylene glycol 200 and polyethylene glycol 400.
5. The method for preparing a polysulfone hollow fiber membrane with a gradient pore structure according to any one of claims 1 to 4, It is characterized in that The hollow fiber membrane includes an outer dense membrane structure and an inner porous membrane structure. The inner diameter of the hollow fiber membrane is 0.40-0.80 mm and the outer diameter is 0.60-1.10 mm.
6. The method for preparing the gradient pore structure polysulfone hollow fiber membrane according to claim 5, It is characterized in that The pore size of the outer dense membrane structure of the hollow fiber membrane is 0.005-0.02 μm, the thickness of the outer dense membrane structure is 30-50 μm, and the surface porosity is 10%-30%; The pore size of the inner porous membrane structure of the hollow fiber membrane is 0.04-0.08 μm, the thickness of the inner porous membrane structure is 40-70 μm, and the inner surface porosity is 40%-60%.
Citation Information
Patent Citations
Polyether sulfone hollow fiber microporous membrane and preparation method
CN109012194A
Acid-resistant hollow fiber nanofiltration membrane and preparation method thereof
CN110732246A
Double-layer composite hollow fiber membrane for vaccine virus concentration and purification and preparation method of double-layer composite hollow fiber membrane
CN117563437A
Polymer-based film, preparation method therefor, and use thereof
WO2021083162A1
Cited By
Hollow fiber membrane based on surface charge adsorption of antiviral material and preparation method of hollow fiber membrane
CN121155377A
Filter element base tube coating method
CN122424982A